Compound, preparation method thereof and preparation method of polyolefin elastomer

By using salicylaldimine neutral nickel catalyst with large steric hindrance group and secondary coordination effect, the problems of complex preparation process and low performance of polyethylene elastomer in the existing technology are solved, and high molecular weight and high degree of branching are achieved. The preparation of polyethylene elastomer simplifies the process and improves material performance.

CN118791533APending Publication Date: 2024-10-18CHANGCHUN INSTITUTE OF APPLIED CHEMISTRY CHINESE ACADEMY OF SCIENCES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410837634.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

Existing catalysts used to prepare polyethylene elastomers require a large amount of cocatalysts, resulting in complex processes and reduced performance, and it is difficult to obtain polyethylene elastomers with high molecular weight and high degree of branching.

Method used

Using a salicylaldimine neutral nickel catalyst with large steric hindrance groups and secondary coordination effects, by adjusting the substituent groups in its structure, the preparation of polyethylene elastomers with high molecular weight and high degree of branching can be achieved, reducing the need for auxiliaries. Catalyst dependence.

Benefits of technology

The preparation process of polyolefin elastomers is simplified, polyethylene elastomers with high molecular weight and high degree of branching are obtained, which improves material properties and reduces dependence on cocatalysts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118791533A_ABST
    Figure CN118791533A_ABST
Patent Text Reader

Abstract

The invention discloses a compound and a preparation method thereof, and a preparation method of a polyolefin elastomer, and belongs to the technical field of elastomer materials. Under the combined action of the secondary coordination effect of R4 and the steric effect of an aryl large steric hindrance group of R5, the compound with the structure as shown in the formula 1 is used as a salicylaldehyde imine neutral nickel catalyst to catalyze polyolefin polymerization to obtain a polyolefin elastomer with high molecular weight and high branching degree at the same time. The compound is used for preparing the polyolefin elastomer, and a new thought is provided for simplifying the preparation process of the polyolefin elastomer. # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of elastomer materials, and in particular to a compound and a preparation method thereof, and a preparation method of a polyolefin elastomer. Background Art

[0002] Polyolefins have played an indispensable role in daily life and industrial production due to their structural diversity and wide applicability. Polyolefin thermoplastic elastomer is a high-performance polyolefin that is rubber-elastic at room temperature and has the characteristics of low density, large bending, high low-temperature impact resistance, easy processing, and reusability. This product has been widely used in the automotive manufacturing industry at home and abroad.

[0003] In recent years, the research on the preparation of elastomeric materials using ethylene monomers has attracted much attention. The catalysts used to prepare polyethylene elastomers are mainly [N,N]-coordinated cationic nickel catalysts, which require the addition of a large amount of co-catalysts, such as MAO or alkyl aluminum, which not only increases the process cost but also makes the preparation process more complicated. In addition, the aluminum in the co-catalyst will remain in the polyethylene, reducing the performance of the polyethylene elastomer.

[0004] Salicylaldehyde imine neutral nickel catalyst has become an important catalyst for the preparation of polyethylene elastomers due to its unique oxygen affinity, active center stability and applicability to aqueous phase polymerization. Through in-depth research, it was found that by adjusting the different position groups in the salicylaldehyde imine neutral nickel catalyst, such as the phenol oxygen ortho group, the leaving ligand group and the aromatic amine group, the structure and properties of polyethylene elastomers can be finely controlled. For example, Mecking et al. successfully prepared a variety of materials from low molecular weight polymers to low-branched ultra-high molecular weight polyethylene through the clever application of terphenyl aromatic amine groups; Marks et al. introduced sulfonyl groups to obtain low molecular weight and highly branched polymers; 2,6-diisopropyl substituted aromatic amine catalysts generally produce polyethylene with medium molecular weight and medium branching degree. This is because the increase in branching degree and the decrease in molecular weight of the polyethylene prepared by salicylaldehyde imine neutral nickel catalyst often occur simultaneously. When the branching degree rises to the level of elastomer, the molecular weight can no longer meet the requirements.

[0005] Therefore, it is of great significance to study and develop a new type of salicylaldehyde imine neutral nickel catalyst to achieve the preparation of high molecular weight and high branching degree polyethylene elastomer. Summary of the invention

[0006] In view of this, the technical problem to be solved by the present invention is to provide a compound and a preparation method thereof and a preparation method of a polyolefin elastomer. The compound is used to catalyze olefin polymerization to prepare a polyolefin elastomer.

[0007] In order to achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0008] The present invention provides a compound having a structure shown in Formula 1:

[0009]

[0010] Wherein Ar1 and Ar2 are independently selected from C 6 ~C 14 Aryl;

[0011] The C 6 ~C 14 Aryl groups include, but are not limited to, phenyl, naphthyl, benzyl, anthracenyl, phenanthrenyl, fluorenyl, and the like.

[0012] R 1 , R 2 , R 3 independently selected from H, halogen, C 1 ~C 20 Alkyl, C 1 ~C 10 Alkoxy, fluorine-substituted C 1 ~C 6 Alkyl, C 6 ~C 14 One or more of aryl, nitro, amino, and hydroxyl;

[0013] The fluorine-substituted C 1 ~C 6 The number of fluorine atoms in the alkyl group is 1, 2 or 3.

[0014] Preferably, the fluorine-substituted C 1 ~C 6 The alkyl group is selected from trifluoromethyl, trifluoroethyl, trifluoropropyl, CH 2 F. CHF 2 , CH 3 CH 2 F, CH 2 FCH 2 F, CH 3 CHF 2 , CH 3 CH 2 CH 2 F, etc.

[0015] R 4 Selected from O, S, Se, SO 2 , SO, SeO 2 , SeO, CO, CS, NH, NO or SiO;

[0016] The above R 4 It has a secondary coordination effect.

[0017] The secondary coordination effect refers to the polar group R 4 The electron coordination effect with the central metal nickel occurs. The central metal nickel is an electron-deficient group, and the polar group R 4 It is an electron-rich group, and the two groups are close to each other in spatial structure, so there is a certain secondary coordination effect between the two. The existence of secondary coordination effect makes it easier for chain transfer to occur when nickel metal catalyzes ethylene polymerization, so the catalytic polymer has a higher degree of branching.

[0018] R 5 Selected from H, halogen, C 1 ~C 20 Alkyl, C 1 ~C 10 Alkoxy, fluorine-substituted C 1 ~C 6 Alkyl, C 6 ~C 14 One or more of aryl, nitro, amino, hydroxyl, and aryl bulky steric hindrance groups, and at least contains aryl bulky steric hindrance groups;

[0019] R 6 , R 7 independently selected from H, halogen, C 1 ~C 20 Alkyl, C 1 ~C 10 Alkoxy, fluorine-substituted C 1 ~C 6 One or more of alkyl, nitro, amino, and hydroxyl;

[0020] L is selected from C 6 ~C 14 Aryl or C 1 ~C 10 alkyl;

[0021] R L Selected from -PPh 3 、-PMe 3 , CH 3 CN-, pyridyl, 2-methylpyridyl, 3-methylpyridyl or 4-methylpyridyl;

[0022] m is selected from an integer between 1 and 3;

[0023] n is an integer selected from 1 to 5.

[0024] The CH of the present invention 3 The short lines “-” in CN- represent coordination bonds, specifically the coordination bonds formed by the lone pair of electrons in the nitrogen atom and the metal center Ni.

[0025] The compounds of the present invention also contain a large steric hindering group R 5 and the group R with secondary coordination effect 4 , a single active center (Ni) salicylaldehyde imine neutral nickel catalyst.

[0026] The compound can be used as a salicylaldehyde imine neutral nickel catalyst with a single active center for catalytic synthesis of polyolefin elastomers.

[0027] The compound of the present invention is used to catalyze the polymerization of olefin monomers, which contain a large steric hindrance group R 5 and the group R with secondary coordination effect 4 The synergistic effect enables the polymerization reaction to obtain a polyolefin elastomer with both high molecular weight and high branching degree, which provides a new catalyst for the preparation of polyolefin elastomers. In addition, during the catalytic reaction of the polyolefin elastomer, it is not necessary to add a large amount of co-catalyst, such as alkyl aluminum or MAO (methylaluminoxane), which makes the preparation process of the polyolefin elastomer more convenient.

[0028] The polyolefin elastomer is preferably a polyethylene elastomer or a polypropylene elastomer.

[0029] More preferably, Ar1 and Ar2 are independently selected from C 6 ~C 10 Aryl;

[0030] More preferably, the C 6 ~C 10 Aryl includes, but is not limited to, phenyl, naphthyl, benzyl, and the like.

[0031] More preferably, the R 1 , R 2 , R 3 independently selected from H, halogen, C 1 ~C 10 Alkyl, C 1 ~C 6 Alkoxy, fluorine-substituted C 1 ~C 4 Alkyl, C 6 ~C 14 One or more of aryl, nitro, amino, and hydroxyl;

[0032] The C 1 ~C 10 Alkyl groups include, but are not limited to, methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, n-pentyl, neopentyl, hexyl, heptyl, octyl, nonyl, decyl, and the like.

[0033] The C 1 ~C 6Alkoxy groups include, but are not limited to, methoxy, ethoxy, n-propoxy, isopropoxy, n-butoxy, isobutoxy, tert-butoxy, n-pentoxy, and the like.

[0034] The fluorine-substituted C 1 ~C 4 Alkyl groups include, but are not limited to, trifluoromethyl, trifluoroethyl, trifluoropropyl, CH 2 F. CHF 2 , CH 3 CH 2 F, CH 2 FCH 2 F, CH 3 CHF 2 , CH 3 CH 2 CH 2 F etc.

[0035] More preferably, R 4 Selected from O, Se, SO 2 , SO, NH or NO;

[0036] More preferably, R 5 Selected from H, halogen, C 1 ~C 10 Alkyl, C 1 ~C 6 Alkoxy, fluorine-substituted C 1 ~C 4 Alkyl, C 6 ~C 14 Aryl, nitro, amino, C 10 ~C 16 One or more of the aromatic bulky steric groups, and at least C 10 ~C 16 Aryl is a large steric hindering group;

[0037] More preferably, the R 6 , R 7 independently selected from H, halogen, C 1 ~C 10 Alkyl, C 1 ~C 6 Alkoxy, fluorine-substituted C 1 ~C 4 One or more of alkyl, nitro, amino, and hydroxyl;

[0038] More preferably, L is selected from C 6 ~C 10 Aryl or C 1 ~C 6 alkyl;

[0039] More preferably, R LSelected from -PPh 3 、-PMe 3 , CH 3 CN-, pyridyl, 2-methylpyridyl, 3-methylpyridyl or 4-methylpyridyl;

[0040] More preferably, said m is selected from 1 or 2;

[0041] More preferably, the n is selected from an integer between 1 and 3.

[0042] The C 1 ~C 10 Alkyl, C 1 ~C 6 Alkoxy, fluorine-substituted C 1 ~C 4 Alkyl, C 6 ~C 14 The scope of the aryl group is the same as above and will not be repeated here.

[0043] More preferably, the C 6 ~C 14 Aryl groups also contain substituents;

[0044] More preferably, the C 6 ~C 14 The substituents of the aryl group are selected from halogen, C 1 ~C 10 Alkyl, C 1 ~C 6 Alkoxy, fluorine-substituted C 1 ~C 6 One or more of alkyl, nitro, amino, and hydroxyl.

[0045] More preferably, the C 1 ~C 20 Alkyl, C 1 ~C 10 Alkoxy groups also contain substituents;

[0046] More preferably, the C 1 ~C 20 Alkyl, C 1 ~C 10 The substituent of the alkoxy group is selected from one or more of halogen, nitro, amino and hydroxyl.

[0047] It is further preferred that the Ar1 and Ar2 are independently selected from phenyl or naphthyl;

[0048] Further preferably, the R 1Selected from H, methyl, tert-butyl, iodine, trifluoromethyl, nitro, p-methylphenyl, p-trifluoromethylphenyl, p-nitrophenyl, m-methylphenyl, m-trifluoromethylphenyl, m-nitrophenyl, o-methylphenyl, o-trifluoromethylphenyl, o-nitrophenyl, anthracenyl, 6-methylanthracenyl, 6-methoxyanthracenyl, 6-tert-butylanthracenyl, 6-chloroanthracenyl, 6-trifluoromethylanthracenyl, 6-nitroanthracenyl, 6-methylanthracenyl;

[0049] Further preferably, the R 2 is selected from H, methyl, tert-butyl, methoxy, iodine, trifluoromethyl or nitro;

[0050] Further preferably, the R 3 is selected from H, methyl, methoxy, tert-butyl, fluorine, trifluoromethyl, nitro, methyl, methoxy, tert-butyl, fluorine, trifluoromethyl, nitro, methyl, methoxy, tert-butyl, fluorine, trifluoromethyl or nitro; further preferably, said R 3 is selected from H, 4-methyl, 4-methoxy, 4-tert-butyl, 4-fluoro, 4-trifluoromethyl, 4-nitro, 3-methyl, 3-methoxy, 3-tert-butyl, 3-fluoro, 3-trifluoromethyl, 3-nitro, 2-methyl, 2-methoxy, 2-tert-butyl, 2-fluoro, 2-trifluoromethyl or 2-nitro;

[0051] Further preferably, the R 4 Selected from O, SO 2 or SO;

[0052] Further preferably, the R 5 Selected from H, methyl, tert-butyl, methoxy, phenyl, One or more of diphenylmethyl, anthracenyl, and naphthyl, and at least One or more of benzhydryl, anthracenyl, and naphthyl;

[0053] Further preferably, the R 6 , R 7 independently selected from H, halogen, C 1 ~C 10 Alkyl, C 1 ~C 6 One or more of alkoxy; further preferably, L is selected from phenyl, naphthyl or methyl;

[0054] Further preferably, the R L Selected from PPh 3 、PMe 3 , CH 3 CN-, pyridyl, 2-methylpyridyl, 3-methylpyridyl or 4-methylpyridyl;

[0055] Further preferably, said m is selected from 1 or 2;

[0056] More preferably, n is selected from 1 or 2.

[0057] It is further preferred that the Ar1 and Ar2 are selected from phenyl groups;

[0058] More preferably, the R 1 Selected from tert-butyl, anthracenyl, 6-methylanthracenyl, p-methylphenyl, m-methylphenyl, o-methylphenyl or phenyl;

[0059] More preferably, the R 2 is selected from H, methyl, tert-butyl or methoxy;

[0060] More preferably, the R 3 is selected from H, methyl, methoxy or tert-butyl;

[0061] More preferably, the R 3 is selected from H, 4-methyl, 4-methoxy or 4-tert-butyl;

[0062] More preferably, the R 4 Selected from SO 2 , L is selected from Ph or methyl, R L Selected from PPh 3 、PMe 3 , CH 3 CN-, pyridyl, 2-methylpyridyl, 3-methylpyridyl or 4-methylpyridyl;

[0063] More preferably, the R 5 Selected from H, methyl, tert-butyl, methoxy, phenyl, One or more of

[0064] More preferably, the R 6 , R 7 Selected from H;

[0065] More preferably, said m is selected from 1;

[0066] More preferably, n is selected from 2.

[0067] In some specific embodiments of the present invention, when R 1 Selected from anthracene, R 3 Selected from H, R 4 Selected from SO 2 , R 5 Selected from R 6 , R 7 is selected from H, L is selected from Ph, RL Selected from -PPh 3 , when n is 2, R 2 Preferred is methyl, tert-butyl or methoxy.

[0068] In some specific embodiments of the present invention, when R 2 Selected from H, R 3 Selected from H, R 4 Selected from SO 2 , R 5 Selected from R 6 , R 7 is selected from H, L is selected from Ph, R L Selected from -PPh 3 , when n is 2, the R 1 Preferred is p-methylphenyl, m-methylphenyl, o-methylphenyl or 6-methylanthryl.

[0069] In some specific embodiments of the present invention, when R 1 Selected from tert-butyl, R 2 Selected from H, R 4 Selected from SO 2 , R 5 Selected from R 6 , R 7 is selected from H, L is selected from Ph, R L Selected from -PPh 3 , when n is 2, R 3 Preferred is methyl, tert-butyl or methoxy.

[0070] In some specific embodiments of the present invention, when R 1 Selected from tert-butyl, R 2 Selected from H, R 3 Selected from H, R 5 Selected from R 6 , R 7 is selected from H, L is selected from Ph, R L Selected from -PPh 3 , when n is 2, R 4 Preferably O, S, Se, SO 2 , SO, SeO 2 , SeO, CO, CS, NH, NO or SiO.

[0071] In some specific embodiments of the present invention, when R 1 Selected from tert-butyl, R 2 Selected from H, R 3 Selected from H, R 4 Selected from SO 2 , R 6, R 7 is selected from H, L is selected from Ph, R L Selected from -PPh 3 , the R 5 Preferably H, methyl, tert-butyl, methoxy, phenyl, Any two of

[0072] In some specific embodiments of the present invention, when R 1 Selected from tert-butyl, R 2 Selected from H, R 3 Selected from H, R 4 Selected from SO 2 , R 5 Selected from R 6 , R 7 When n is 2, L is preferably phenyl or methyl, and R L Preferred is -PPh 3 、-PMe 3 , CH 3 CN-, pyridyl, 2-methylpyridyl, 3-methylpyridyl or 4-methylpyridyl.

[0073] More preferably, the compound has a structure shown in Formula 1-1:

[0074]

[0075] The R 1 , R 2 , R 3 , R 4 , R 5 , L, R L The value range of is the same as above and will not be repeated here.

[0076] Preferably, the compound has any of the following structures:

[0077]

[0078] Preferably, the method for preparing the compound of the structure shown in Formula 1 comprises the following steps:

[0079] 1) heating dibenzosuberol and aniline of formula (1) under the action of a catalyst to react to prepare aniline of formula (3);

[0080] 2) reacting the aniline of formula (3) and the salicylaldehyde of formula (2) in an acidic environment to obtain a ligand of formula (4);

[0081] 3) reacting the ligand represented by formula (4) and a nickel source in an alkaline environment to prepare a compound represented by formula 1;

[0082]

[0083] Preferably, in the step 1), the catalyst is selected from a mixed solution of anhydrous zinc chloride and concentrated hydrochloric acid;

[0084] The heating temperature in step 1) is 120°C to 170°C, and more preferably 160°C.

[0085] After step 1), extraction, filtration and washing are further performed.

[0086] The extraction is preferably carried out using dichloromethane and saturated brine.

[0087] The washing is preferably performed with hexane.

[0088] Preferably, in step 2), the molar ratio of aniline represented by formula (3) to salicylaldehyde represented by formula (2) is 1:(1-1.5).

[0089] Preferably, the acidic environment in step 2) is provided by one or more of p-toluenesulfonic acid monohydrate, hydrochloric acid, and acetic acid.

[0090] Preferably, the reaction temperature in step 2) is 70°C to 100°C, more preferably 80°C to 90°C. In some specific embodiments of the present invention, it is preferably 85°C.

[0091] After the reaction is completed, filter and wash.

[0092] Preferably, the alkaline environment in step 3) is provided by one or more of NaH, pyridine, 2-methylpyridine, 3-methylpyridine, or 4-methylpyridine;

[0093] Preferably, the nickel source in step 3) is selected from NiMe 2 (tmeda) and containing leaving group R L A mixture of compounds, NiPhCl(PPh 3 ) 2 、NiMe 2 Py 2 One or more of; more preferably NiPhCl(PPh 3 ) 2 .

[0094] Preferably, the leaving group R L R in the compound L Selected from -PPh 3 、-PMe 3 , CH3 CN-, pyridyl, 2-methylpyridyl, 3-methylpyridyl or 4-methylpyridyl.

[0095] The nickel source is selected from NiPhCl (PPh 3 ) 2 or NiMe 2 Py 2 When it can provide the nickel atom in the compound of the present invention, it can also provide L and R L group, wherein the L group is phenyl or methyl, R L The group is -PPh 3 or pyridyl.

[0096] The nickel source is selected from NiMe 2 (tmeda) and containing leaving group R L When the mixture of compounds, NiMe 2 (tmeda) provides the nickel atom in the compound of the present invention and can also provide a methyl group as the L group.

[0097] Preferably, the molar ratio of the dibenzosuberol to the aniline represented by formula (1) is preferably 1:(1-1.5); more preferably 1:1.

[0098] Preferably, the molar ratio of the ligand represented by formula (4) to the nickel source is 1:(1-2); more preferably 1:1.1.

[0099] The present invention also provides a method for preparing a polyethylene elastomer, wherein the above compound or the compound prepared by the above method is used to catalyze the polymerization reaction of olefin monomers to obtain a polyolefin elastomer.

[0100] In the present invention, the ratio of the compound to the olefin monomer is preferably 1 μmol: (2-5) bar; more preferably 1 μmol: (2-3) bar; further preferably 1 μmol: 3 bar.

[0101] Preferably, the polyolefin elastomer is selected from polyethylene elastomer or polypropylene elastomer.

[0102] More preferably, the polymerization further adds Ni(COD) 2 or B(C 6 F 5 ) 3 After addition, the activity of olefin polymerization is significantly improved, and the molecular weight and branching degree of polyolefin are not significantly affected.

[0103] The temperature when the compound of the present invention catalyzes olefin polymerization is preferably 30°C to 50°C; more preferably 30°C or 50°C.

[0104] The pressure when the compound of the present invention catalyzes ethylene polymerization is preferably 8 to 30 bar, and the reaction time is preferably 30 min.

[0105] Compared with the prior art, the present invention provides a compound with a structure shown in Formula 1. wherein Ar1 and Ar2 are independently selected from C 6 ~C 14 Aryl; R 1 , R 2 , R 3 independently selected from H, halogen, C 1 ~C 20 Alkyl, C 1 ~C 10 Alkoxy, fluorine-substituted C 1 ~C 6 Alkyl, C 6 ~C 14 One or more of aryl, nitro, amino, and hydroxyl; R 4 Selected from O, S, Se, SO 2 , SO, SeO 2 , SeO, CO, CS, NH, NO or SiO; R 5 Selected from H, halogen, C 1 ~C 20 Alkyl, C 1 ~C 10 Alkoxy, fluorine-substituted C 1 ~C 6 Alkyl, C 6 ~C 14 One or more of aryl, nitro, amino, hydroxyl, and aryl bulky steric hindrance groups, and at least contains aryl bulky steric hindrance groups; R 6 , R 7 independently selected from H, halogen, C 1 ~C 20 Alkyl, C 1 ~C 10 Alkoxy, fluorine-substituted C 1 ~C 6 One or more of alkyl, nitro, amino, and hydroxyl; L is selected from C 6 ~C 14 Aryl or C 1 ~C 10 Alkyl; R L Selected from -PPh 3 、-PMe 3 , CH 3 CN-, pyridyl, 2-methylpyridyl, 3-methylpyridyl or 4-methylpyridyl; m is selected from an integer between 1 and 3; n is selected from an integer between 1 and 5. The compound is 4 Secondary coordination effects and R 5The synergistic effect of the steric effect of the large steric hindrance group of the aromatic group enables it to be used as a salicylaldimine neutral nickel catalyst to catalyze polyolefin polymerization to obtain a polyolefin elastomer with both high molecular weight and high branching degree. The present invention uses the compound for the preparation of the polyolefin elastomer, providing a new idea for simplifying the preparation process of the polyolefin elastomer. BRIEF DESCRIPTION OF THE DRAWINGS

[0106] Figure 1 This is the hydrogen nuclear magnetic resonance spectrum of the aniline prepared in step (1) of Example 1;

[0107] Figure 2 is the hydrogen nuclear magnetic resonance spectrum of the salicylaldehyde ligand prepared in step (2) of Example 1;

[0108] Figure 3 The hydrogen nuclear magnetic resonance spectrum of the salicylaldimine nickel catalyst prepared in Example 1;

[0109] Figure 4 This is the nuclear magnetic resonance phosphine spectrum of the salicylaldehyde imine nickel catalyst prepared in Example 1;

[0110] Figure 5 The single crystal diffraction pattern of the salicylaldehyde imine nickel catalyst prepared in Example 1;

[0111] Figure 6 is a stress-strain curve of the polyethylene elastomer of Item 8 of Table 5;

[0112] Figure 7 This is the stretch recovery curve of the polyethylene elastomer in entry 8 of Table 5 (SR=58%). DETAILED DESCRIPTION

[0113] In order to further illustrate the present invention, the compound and the preparation method thereof and the preparation method of the polyolefin elastomer provided by the present invention are described in detail below with reference to the embodiments.

[0114] In the following embodiments of the present invention, the compound has a structure shown in Formula 1-1:

[0115]

[0116] The preparation method of formula 1-1 comprises the following steps:

[0117]

[0118] The synthesis process is as follows:

[0119] 1) Dibenzosuberol and general formula aniline (a) are added into a round-bottom flask at a molar ratio of 1:1, and then the temperature is raised to 100°C to dissolve all the raw materials, and then 0.5 equivalent of a mixed solution of anhydrous zinc chloride and concentrated hydrochloric acid is added, and the mixture is stirred at above 160°C for more than 2 hours, cooled to room temperature, and dissolved with a large amount of dichloromethane, and the mixed solution of the crude product is poured into a 500mL separatory funnel, and saturated salt water is added for extraction and separation, and the organic phase is retained, and an appropriate amount of anhydrous sodium sulfate is added to the organic phase for drying for 30 minutes. After filtering off the desiccant, the crude product is vacuum concentrated and spin-dried, and the crude product is washed and filtered with hexane to obtain the target product with a yield of about 80%.

[0120] 2) The general salicylaldehyde skeleton (b) and the general aniline (c) are added to an organic solvent at a molar ratio of 1:N (N≥1), and 10 mg of p-toluenesulfonic acid monohydrate is added, and 20 ml of methanol is added to dissolve, and the mixture is reacted in an oil bath at 85°C for 24 hours. After the reaction time is over, the suspension of the crude product is cooled to room temperature, and the suspension is filtered using a sand core funnel. The filter cake is washed 3 times with an appropriate amount of methanol and 1 time with hexane, and a light yellow solid product is obtained after vacuum drying, with a yield of about 85%.

[0121] 3) In a nitrogen environment of a glove box, place the general formula ligand (d) and the nickel source in a 25 mL spin flask at a molar ratio of 1:N (N≥1), dissolve in toluene, and add 2 equivalents of a leaving group R L The solution color turns brown-red and reacts at room temperature for 6 hours. The brown-red solution is filtered and concentrated, hexane is added dropwise, and the solution is purified by precipitation in a refrigerator. The solid is filtered and washed with ice hexane and then dried to obtain the target product with a yield of more than 60%.

[0122] In the above reaction equation, R 1 , R 2 , R 3 independently selected from H, halogen, C 1 ~C 20 Alkyl, C 1 ~C 10 Alkoxy, fluorine-substituted C 1 ~C 6 Alkyl, C 6 ~C 14 One or more of aryl, nitro, amino, and hydroxyl;

[0123] R 4 Selected from O, S, Se, SO 2 , SO, SeO 2 , SeO, CO, CS, NH, NO or SiO;

[0124] R 5 Selected from H, halogen, C 1 ~C20 Alkyl, C 1 ~C 10 Alkoxy, fluorine-substituted C 1 ~C 6 Alkyl, C 6 ~C 14 One or more of aryl, nitro, amino, hydroxyl, and aryl bulky steric hindrance groups, and at least contains aryl bulky steric hindrance groups;

[0125] L is selected from C 6 ~C 14 Aryl or C 1 ~C 10 alkyl;

[0126] R L Selected from -PPh 3 、-PMe 3 , CH 3 CN-, pyridyl, 2-methylpyridyl, 3-methylpyridyl or 4-methylpyridyl.

[0127] Example 1

[0128] (1) Synthesis of aniline: Weigh 2-aminodiphenyl sulfone (5 g, 21.4 mmol) and dibenzosuberol (9.01 g, 42.8 mmol) in a 250 mL round-bottom flask and place the raw materials in an oil bath at 95 °C until the solid is completely melted. Then, a mixed solution of anhydrous zinc chloride (1.46 g, 10 mmol) and concentrated hydrochloric acid (2 mL) is added dropwise, and the oil bath is heated to 160 °C for 2 h.

[0129] After the reaction time is over, the crude product is cooled to room temperature, and a large amount of dichloromethane is added to dissolve the crude product. The mixed solution of the crude product is poured into a 500mL separatory funnel, saturated brine is added for extraction and separation, the organic phase is retained, and an appropriate amount of anhydrous sodium sulfate is added to the organic phase for drying for 30 minutes. After filtering out the desiccant, the crude product is vacuum concentrated and spin-dried, and the crude product is washed and filtered with hexane to obtain 12.3g of brown-red solid product, with a yield of about 93.1%.

[0130]

[0131] 1 H NMR (500 MHz, 298 K, CDCl 3,7.26ppm): δ=7.71-7.66(m,2H,aryl-H),7.55-7.50(m,1H,aryl-H),7.44-7.40(m,2H,aryl-H),7.21-7.16 (m,5H,aryl-H),7.13-7.04(m,10H,aryl-H),6.94-6.90(m,2H,aryl-H),6.55(s,1H,aryl-H),5.23(s,2H,NH 2 ),4.97(s,1H,CH),4.87(s,1H,CH),2.89-2.82(m,2H,CH 2 ),2.71-2.59(m,4H,CH 2 ),2.48-2.40(m,2H,CH 2 ).

[0132] (2) Synthesis of ligand: Weigh 3-tert-butyl salicylaldehyde (0.5 g, 2.81 mmol) and aniline (1.76 g, 3.11 mmol) in a 48 mL pressure bottle, add 15 mg of p-toluenesulfonic acid monohydrate, add 20 ml of methanol to dissolve, and react in an 85 ° C oil bath for 24 h. After the reaction time is over, the suspension of the crude product is cooled to room temperature, and the suspension is filtered with a sand core funnel. The filter cake is washed 3 times with an appropriate amount of methanol and once with hexane. After vacuum drying, 1.84 g of light yellow solid product is obtained, and the yield is about 84.1%.

[0133]

[0134] 1 H NMR (500 MHz, 298 K, CDCl 3 ,7.26ppm): δ=12.10(s,1H,OH),7.80-7.77(m,1H,aryl-H),7.58(s,1H,aryl-H),7.49-7.42(m,4H,aryl-H),7.31-7.26(m ,3H,aryl-H),7.24-7.10(m,9H,aryl-H),6.89-6.75(m,9H,aryl-H),5.19(s,2H,CH),4.95(s,2H,CH),2.97-2.90(m,2H,CH 2 ),2.86-2.45(m,6H,CH 2 ),1.51(s,9H,C(CH 3 ) 3 ).

[0135] 13C NMR (125MHz, 298K, CDCl 3 ,77.16ppm): δ=172.71(N=C-Ph),160.06(C-OH),145.13,141.08,140.68,139.69,139.23,137.30,136.33,135.92,133.02,132.20,131.76, 131.20,130.87,128.88,127.82,127.79,127.74,127.06,126.58,126 .16,125.97,118.68,118.49,57.97,57.92,56.17,35.00,29.50(C(CH 3 ) 3 ).

[0136] (3) Catalyst synthesis: In a glove box, N 2 In an atmosphere of , the ligand (200 mg, 0.26 mmol) obtained in step (2) and NaH solid (12.4 mg, 0.52 mmol) were placed in a 25 mL spinner flask. 10 mL of THF solvent was added and the reaction was continued for 6 h. After the reaction was completed, the excess NaH solid was filtered out and the solvent was drained to obtain a light yellow sodium salt. The sodium salt was dissolved in toluene and NiPhCl (PPh 3 ) 2 (200 mg, 0.29 mmol). The color of the solution changed from yellow to brownish red, and the reaction was carried out at room temperature for 6 hours. After the reaction was completed, the brownish red solution was filtered and concentrated, hexane was dripped into the concentrated solution, and the solution was placed in a refrigerator for precipitation and purification. The precipitated solid was filtered, washed with ice hexane and dried to obtain about 200 mg of brown solid, with a yield of 65.5%.

[0137]

[0138] 1 H NMR (500MHz, 298K, C 6 D 6,7.16ppm):δ=8.19-8.03(m,8H,aryl-H),7.92(s,1H,aryl-H),7.84-7.80(m,2H,aryl-H),7.28-7.25(m,1H,aryl-H),7.03-7.00(m,9H,aryl-H),6.99-6.90(m,8H,aryl-H),6.87-6.79(m,3H,aryl-H),6.74-6.69(m,3H,aryl-H),6.68-6.45(m,8H,aryl-H),6.38-6.3(m,1H,aryl-H),6.29-6.23(m,1H,aryl-H),6.02-5.97(m,1H,aryl-H),5.81-5.76(m,1H,aryl-H),5.73(s,1H,CH),4.97(s,1H,CH),2.86-2.75(m,1H,CH 2 ),3.71-3.62(m,2H,CH 2 ),2.56-2.45(m,2H,CH 2 ),2.34-2.22(m,2H,CH 2 ),2.04-1.87(m,1H,CH 2 ),1.01(s,9H,C(CH 3 ) 3 ).

[0139] 13 C NMR(100MHz,298K,C 6 D 6 ,128.06ppm):δ=169.03(N=C-Ph),166.63(Ni-O-C),143.76,143.04,142.06,141.58,140.44,140.20,139.78,139.00,138.84,138.61,136.78,136.07,135.46,135.38,134.54,132.38,132.27,131.73,131.59,131.49,131.11,130.47,129.82,129.34,126.90,126.61,126.55,125.98,125.70,124.94,120.24,112.45,58.35,34.75,33.12,33.01,32.46,31.97,30.19,29.87,23.06,21.43,14.35.

[0140] 31P NMR (202MHz, 298K, C 6 D 6 ,7.16ppm):δ=21.79.

[0141] The present invention tests the effect of the substituent change on ethylene polymerization by changing the substituent in the above compound (neutral nickel catalyst of salicylaldimine), and the test results are shown in Tables 1 to 7. The preparation process of the compound (neutral nickel catalyst of salicylaldimine) is the same as that of Example 1, except that the raw materials in each reaction are different.

[0142] The substitution changes in the following Tables 1 to 7 are all included in Formula 1-1.

[0143]

[0144] Table 1 Different salicylaldehyde imine neutral nickel catalysts (changing the substituent R 2 ) on ethylene polymerization

[0145]

[0146] Reaction conditions: salicylaldehyde imine neutral nickel catalyst (5 μmol), toluene (100 mL), ethylene pressure (15 bar), polymerization time (30 min), polymerization temperature (30 ° C), for items 1 to 7, 10 μmol of Ni (COD) was added 2 . Activity: 10 6 gmol -1 h -1 The unit is M w 、M w / M n : weight average molecular weight and polymer dispersity index, respectively, measured by GPC in 1,2,4-trichlorobenzene at 150°C relative to polystyrene standards. Degree of branching = number of branches per 1000 carbon atoms, measured by H NMR spectroscopy.

[0147] Note: Nickel catalyst (R 3 =H, R 4 =SO 2 , R 6 =H, R 7 =H, R 1 = anthracenyl, L = Ph, R L =PPh 3 ).

[0148] The polymerization reaction process: First, a 350 mL reactor connected to a high-pressure gas pipeline was vacuum dried at 90°C for at least 1 h. Then the reactor was adjusted to 30°C, 96 mL of toluene was added to the reactor under an inert atmosphere, and then 5 μmol of salicylaldehyde imine neutral nickel catalyst and 10 μmol of Ni(COD) were added. 2 (If necessary) Dissolve in 2 mL toluene and inject into the polymerization system through a syringe. Under rapid stirring (750 rpm), ethylene is introduced and maintained at 15 bar. After 30 minutes, the pressure reactor is evacuated, 200 mL ethanol is added to quench the polymerization reaction, the polymer is filtered, and dried in a vacuum oven to constant weight.

[0149] Conclusion of polymerization data: Using the above-mentioned salicylaldehyde imine neutral nickel catalyst to catalyze ethylene polymerization can obtain polyethylene elastomers with both molecular weight and branching degree. 1 , R 3 , R 4 , R 5 , R 6 No change, change the substituent R 2 When the polymerization conditions are the same (time, temperature, pressure are the same), R 2 If it is an electron-withdrawing group (I, CF 3 、NO 2 ) compared to its electron-donating group (CH 3 , t Bu, OCH 3 ) lower branching degree; the catalysts in items 1 to 7 have a lower branching degree when Ni(COD) is added 2 After addition, the catalytic activity of the polymerization reaction will be significantly improved, while the effect on the molecular weight and branching degree of the polymer is not obvious.

[0150] Table 2 Different salicylaldehyde imine neutral nickel catalysts (changing the substituent R 1 ) on ethylene polymerization

[0151]

[0152]

[0153] Reaction conditions: nickel catalyst (5 μmol), toluene (100 mL), ethylene pressure (15 bar), polymerization time (30 min), polymerization temperature (30 ° C), for entries 1-5 and entries 11-28, Ni(COD) was added 2 10μmol. Activity: 10 6 g mol -1 h -1 The unit is M w 、Mw / M n : weight average molecular weight, polymer dispersity index, respectively, measured by GPC in 1,2,4-trichlorobenzene at 150°C, relative to polystyrene standards. Degree of branching = number of branches per 1000 carbon atoms, measured by proton nuclear magnetic resonance spectroscopy.

[0154] Note: Nickel catalyst (R 2 =H, R 3 =H, R 4 =SO 2 , R 6 =H, R 7 =H, L = Ph, R L =PPh 3 ).

[0155] The polymerization reaction process: First, a 350 mL reactor connected to a high-pressure gas pipeline was vacuum dried at 90 ° C for at least 1 h. Then the reactor was adjusted to 30 ° C, 96 mL of toluene was added to the reactor under an inert atmosphere, and then 5 μmol of Ni catalyst and 10 μmol of Ni(COD) were added. 2 (If necessary) Dissolve in 2 mL toluene and inject into the polymerization system through a syringe. Under rapid stirring (750 rpm), ethylene is introduced and maintained at 15 bar. After 30 minutes, the pressure reactor is evacuated, 200 mL ethanol is added to quench the polymerization reaction, the polymer is filtered, and dried in a vacuum oven to constant weight.

[0156] Conclusion of polymerization data: Using the above-mentioned salicylaldehyde imine neutral nickel catalyst to catalyze ethylene polymerization can obtain polyethylene elastomers with both molecular weight and branching degree. 2 , R 3 , R 4 , R 5 No change, change the substituent R 1 When the polymerization conditions are the same (time, temperature, pressure), the small group (CH 3 , I, CF 3 、NO 2 ), the activity and molecular weight are greatly reduced, and the degree of branching increases; R 1 If it is an electron withdrawing group (m-trifluoromethylphenyl, m-nitrophenyl, p-trifluoromethylphenyl, p-nitrophenyl, o-trifluoromethylphenyl, o-nitrophenyl, 6-trifluoromethylanthracenyl, 6-nitroanthracenyl) compared to the electron donating group (p-methylphenyl, m-methylphenyl, o-methylphenyl, 6-methylanthracenyl) has a lower degree of branching. Add Ni(COD) 2 After addition, the polymerization activity of the same catalyst will be significantly improved, while the effect on the molecular weight and branching degree of the polymer is not obvious.

[0157] Table 3 Different salicylaldehyde imine neutral nickel catalysts (changing the substituent R 3 ) on ethylene polymerization

[0158]

[0159]

[0160] Reaction conditions: nickel catalyst (5 μmol), Ni(COD) 2 (10 μmol), toluene (100 mL), ethylene pressure (15 bar), polymerization time (30 min), polymerization temperature (30 ° C). Activity: 10 6 gmol -1 h -1 The unit is M w 、M w / M n : weight average molecular weight, polymer dispersity index, respectively, measured by GPC in 1,2,4-trichlorobenzene at 150°C, relative to polystyrene standards. Degree of branching = number of branches per 1000 carbon atoms, measured by proton nuclear magnetic resonance spectroscopy.

[0161] Note: Nickel catalyst (R 1 = t Bu, R 2 =H, R 4 =SO 2 , R 6 =H, R 7 =H, L = Ph, R L =PPh 3 ). The above-mentioned ortho and para positions refer to R 3 With R 4 The positional relationship on the Ar2 ring.

[0162] The polymerization reaction process: First, a 350 mL reactor connected to a high-pressure gas pipeline was vacuum dried at 90 ° C for at least 1 h. Then the reactor was adjusted to 30 ° C, 96 mL of toluene was added to the reactor under an inert atmosphere, and then 5 μmol of Ni catalyst and 10 μmol of Ni (COD) were added. 2 Dissolved in 2 mL toluene and injected into the polymerization system through a syringe. Under rapid stirring (750 rpm), ethylene was introduced and maintained at 15 bar. After 30 minutes, the pressure reactor was evacuated, 200 mL ethanol was added to quench the polymerization reaction, the polymer was filtered, and dried in a vacuum oven to constant weight.

[0163] Conclusion of polymerization data: Using the above-mentioned salicylaldehyde imine neutral nickel catalyst to catalyze ethylene polymerization can obtain polyethylene elastomers with both molecular weight and branching degree. 1 , R 2 , R 4 , R 5 No change, change the substituent R 3 When the polymerization conditions are the same (time, temperature, pressure are the same), R 3 If it is an electron-withdrawing group (F, CF 3 、NO 2 ) compared to its electron-donating group (CH 3 , t Bu, OCH 3 ) has a lower degree of branching.

[0164] Table 4 Different salicylaldehyde imine neutral nickel catalysts (changing substituent R 4 ) on ethylene polymerization

[0165]

[0166]

[0167] Reaction conditions: nickel catalyst (5 μmol), Ni(COD) 2 (10 μmol), toluene (100 mL), ethylene pressure (15 bar), polymerization time (30 min), polymerization temperature (30 ° C). Activity: 10 6 gmol -1 h -1 The unit is M w 、M w / M n : weight average molecular weight, polymer dispersity index, respectively, measured by GPC in 1,2,4-trichlorobenzene at 150°C, relative to polystyrene standards. Degree of branching = number of branches per 1000 carbon atoms, measured by proton nuclear magnetic resonance spectroscopy.

[0168] Note: Nickel catalyst (R 1 = t Bu, R 2 =H, R 3 =H, R 6 =H, R 7 =H, L = Ph, R L =PPh 3 ).

[0169] The polymerization reaction process: First, a 350 mL reactor connected to a high-pressure gas pipeline was vacuum dried at 90 ° C for at least 1 h. Then the reactor was adjusted to 30 ° C, 96 mL of toluene was added to the reactor under an inert atmosphere, and then 5 μmol of Ni catalyst and 10 μmol of Ni (COD) were added. 2 Dissolved in 2 mL toluene and injected into the polymerization system through a syringe. Under rapid stirring (750 rpm), ethylene was introduced and maintained at 15 bar. After 30 minutes, the pressure reactor was evacuated, 200 mL ethanol was added to quench the polymerization reaction, the polymer was filtered, and dried in a vacuum oven to constant weight.

[0170] Conclusion of polymerization data: Using the salicylaldehyde imine neutral nickel catalyst of the present invention to catalyze ethylene polymerization can obtain a polyethylene elastomer with both molecular weight and branching degree. 1 , R 2 , R 3 , R 5 No change, change the substituent R 4 When the polymerization conditions are the same (time, temperature, pressure are the same), R 4 If the secondary coordination group is O, S, Se, SO 2 , SO, SeO 2 When SeO, CO, CS, NH, NO or SiO is used, the molecular weight will be slightly lower and the degree of branching will be significantly increased, which will not affect the preparation of polyethylene elastomers. 4 =CH 2 ), Item 12(R 4 =SiH 2 ) as a comparative example, it can be seen that when R 4 Selected from CH 2 or SiH 2 When , the branching degree of polyethylene decreases significantly, and polyethylene elastomer cannot be prepared. The main reason is that these two groups have no polar groups and cannot produce secondary coordination effect with the central nickel metal. Therefore, the branching degree of the prepared polymer is low and polyethylene elastomer cannot be obtained.

[0171] Table 5 Different salicylaldehyde imine neutral nickel catalysts (changing substituent R 5 ) on ethylene polymerization

[0172]

[0173] Reaction conditions: nickel catalyst (5 μmol), Ni(COD) 2(10 μmol), toluene (100 mL), ethylene pressure (15 bar), polymerization time (30 min), polymerization temperature (30 ° C), all data are based on at least two parallel tests (unless otherwise stated). Activity: 10 6 g mol -1 h -1 The unit is M w 、M w / M n : weight average molecular weight and polymer dispersity index, respectively, measured by GPC in 1,2,4-trichlorobenzene at 150°C relative to polystyrene standards. Degree of branching = number of branches per 1000 carbon atoms, measured by H NMR spectroscopy.

[0174] Note: Nickel catalyst (R 1 = t Bu, R 2 =H, R 3 =H, R 4 =SO 2 , R 6 =H, R 7 =H, L = Ph, R L =PPh 3 ).

[0175] The polymerization reaction process: First, a 350 mL reactor connected to a high-pressure gas pipeline was vacuum dried at 90 ° C for at least 1 h. Then the reactor was adjusted to 30 ° C, 96 mL of toluene was added to the reactor under an inert atmosphere, and then 5 μmol of Ni catalyst and 10 μmol of Ni (COD) were added. 2 Dissolved in 2 mL toluene and injected into the polymerization system through a syringe. Under rapid stirring (750 rpm), ethylene was introduced and maintained at 15 bar. After 30 minutes, the pressure reactor was evacuated, 200 mL ethanol was added to quench the polymerization reaction, the polymer was filtered, and dried in a vacuum oven to constant weight.

[0176] Conclusion of polymerization data: Using the salicylaldehyde imine neutral nickel catalyst of the present invention to catalyze ethylene polymerization can obtain a polyethylene elastomer with both molecular weight and branching degree. 1 , R 2 , R 3 , R 4 No change, change the substituent R 5 When the polymerization conditions are the same (time, temperature, pressure are the same), R 5 If it is an electron-withdrawing group (F, CF 3 、NO 2 ) compared to its electron-donating group (CH 3 ,t Bu, OCH 3 ) or phenyl or H have a lower degree of branching.

[0177] Table 6 Effect of different reaction conditions on ethylene polymerization catalyzed by salicylaldehyde imine nickel catalyst of the present invention

[0178]

[0179] Reaction conditions: nickel catalyst (5 μmol), Ni(COD) 2 (10 μmol), toluene (100 mL), all data are based on at least two parallel tests (unless otherwise stated). 6 g mol -1 h -1 The unit is M w 、M w / M n : weight average molecular weight, polymer dispersity index, respectively, measured by GPC in 1,2,4-trichlorobenzene at 150°C, relative to polystyrene standards. Degree of branching = number of branches per 1000 carbon atoms, measured by proton nuclear magnetic resonance spectroscopy.

[0180] Note: Nickel catalyst (R 1 = t Bu, R 2 =H, R 3 =H, R 4 =SO 2 , R 6 =H, R 7 =H, L = Ph, R L =PPh 3 ).

[0181] The polymerization reaction process: First, a 350 mL glass pressure reactor connected to a high-pressure gas pipeline was vacuum dried at 90 ° C for at least 1 h. Then the reactor was adjusted to the target temperature, 96 mL of toluene was added to the reactor under an inert atmosphere, and then 5 μmol of Ni catalyst and 10 μmol of Ni(COD) were added. 2 Dissolve each in 2 mL of toluene and inject into the polymerization system through a syringe. Under rapid stirring (750 rpm), ethylene is introduced and maintained at a fixed pressure. After a certain period of time, the pressure reactor is emptied, 200 mL of ethanol is added to quench the polymerization reaction, the polymer is filtered, and dried in a vacuum oven to constant weight.

[0182] Conclusion of polymerization data: When the catalyst substituent R is controlled 1 , R 2 , R 3 , R 4 , R5 When the time is kept constant (30 min) and the temperature is kept constant (30°C), the activity and molecular weight of the polymer gradually increase with the increase of ethylene pressure. When the ethylene pressure is 30 bar, the molecular weight reaches the maximum, and the degree of branching gradually decreases with the increase of ethylene pressure; when the pressure is kept constant (30 bar) and the temperature is kept constant (30°C), the polymerization activity gradually decreases with the increase of reaction time, the molecular weight gradually increases with the increase of time, and the degree of branching does not change significantly; when the pressure is kept constant (30 bar) and the time is kept constant (30 min), the polymerization activity first increases and then decreases with the increase of temperature, the activity is highest at 50°C, the molecular weight decreases with the increase of temperature, and the degree of branching increases with the increase of temperature.

[0183] In Table 6, only the reaction conditions of items 1, 2, 6, 7, and 8 can produce polyethylene elastomers with both molecular weight and branching degree. Therefore, the temperature when the salicylaldehyde imine nickel catalyst of the present invention catalyzes ethylene polymerization is preferably 30°C to 50°C, the pressure is preferably 8 to 30 bar, and the reaction time is preferably 30 min. Table 7 Effects of different leaving groups and initiating groups on ethylene polymerization catalyzed by salicylaldehyde imine nickel catalyst of the present invention

[0184]

[0185]

[0186] Reaction conditions: catalyst (5 μmol), toluene (100 mL), ethylene (15 bar), polymerization time (30 min), polymerization temperature (30 ° C), for entries 1-9, Ni(COD) was added 2 10μmol. Activity: 10 6 g mol -1 h -1 The unit is M w 、M w / M n : weight average molecular weight and polymer dispersity index, respectively, measured by GPC in 1,2,4-trichlorobenzene at 150°C, relative to polystyrene standards. Degree of branching = number of branches per 1000 carbon atoms, measured by proton nuclear magnetic resonance spectroscopy.

[0187] Note: Nickel catalyst (R 1 = t Bu, R 2 =H, R 3 =H, R 4 =SO 2 , R 6 =H, R 7 =H).

[0188] The polymerization reaction process: First, a 350 mL reactor connected to a high-pressure gas pipeline was vacuum dried at 90 ° C for at least 1 h. Then the reactor was adjusted to the target temperature, 96 mL of toluene was added to the reactor under an inert atmosphere, and then 5 μmol of Ni catalyst and 10 μmol of Ni (COD) were added. 2 (If necessary) dissolved in 2 mL toluene and injected into the polymerization system through a syringe. Under rapid stirring (750 rpm), ethylene was introduced and maintained at a fixed pressure. After a certain period of time, the pressure reactor was evacuated, 200 mL of ethanol was added to quench the polymerization reaction, the polymer was filtered, and dried in a vacuum oven to constant weight.

[0189] Conclusion of polymerization data: Using the above-mentioned salicylaldehyde imine neutral nickel catalyst to catalyze ethylene polymerization can obtain polyethylene elastomers with both molecular weight and branching degree. 1 , R 2 , R 3 , R 4 , R 5 When the polymerization activity is constant, the leaving group R L The difference between the leaving group R and the leaving group R is obvious. The easier the leaving group is, the higher the polymerization activity is. However, the molecular weight and branching degree of the polymer will not change with the leaving group R. L The changes in the initiating group L produced obvious differences.

[0190] The above embodiments are only used to help understand the method and core idea of ​​the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.

Claims

1. The compound of the structure shown in Formula 1: in, Ar1 and Ar2 are independently selected from C 6 ~C 14 Aryl; R 1 , R 2 , R 3 independently selected from H, halogen, C 1 ~C 20 Alkyl, C 1 ~C 10 Alkoxy, fluorine-substituted C 1 ~C 6 Alkyl, C 6 ~C 14 One or more of aryl, nitro, amino, and hydroxyl; R 4 Selected from O, S, Se, SO 2 , SO, SeO 2 , SeO, CO, CS, NH, NO or SiO; R 5 Selected from H, halogen, C 1 ~C 20 Alkyl, C 1 ~C 10 Alkoxy, fluorine-substituted C 1 ~C 6 Alkyl, C 6 ~C 14 One or more of aryl, nitro, amino, hydroxyl, and aryl bulky steric hindrance groups, and at least contains aryl bulky steric hindrance groups; R 6 , R 7 independently selected from H, halogen, C 1 ~C 20 Alkyl, C 1 ~C 10 Alkoxy, fluorine-substituted C 1 ~C 6 One or more of alkyl, nitro, amino, and hydroxyl; L is selected from C 6 ~C 14 Aryl or C 1 ~C 10 alkyl; R L Selected from -PPh 3 、-PMe 3 , CH 3 CN-, pyridyl, 2-methylpyridyl, 3-methylpyridyl or 4-methylpyridyl; m is selected from an integer between 1 and 3; n is an integer selected from 1 to 5.

2. The compound according to claim 1, It is characterized in that Ar1 and Ar2 are independently selected from C 6 ~C 10 Aryl; The R 1 , R 2 , R 3 independently selected from H, halogen, C 1 ~C 10 Alkyl, C 1 ~C 6 Alkoxy, fluorine-substituted C 1 ~C 4 Alkyl, C 6 ~C 14 One or more of aryl, nitro, amino, and hydroxyl; The R 4 Selected from O, Se, SO 2 , SO, NH or NO; The R 5 Selected from H, halogen, C 1 ~C 10 Alkyl, C 1 ~C 6 Alkoxy, fluorine-substituted C 1 ~C 4 Alkyl, C 6 ~C 14 Aryl, nitro, amino, C 10 ~C 16 One or more of the aromatic bulky steric groups, and at least C 10 ~C 16 Aryl is a large steric hindering group; The R 6 , R 7 independently selected from H, halogen, C 1 ~C 10 Alkyl, C 1 ~C 6 Alkoxy, fluorine-substituted C 1 ~C 4 One or more of alkyl, nitro, amino, and hydroxyl; The L is selected from C 6 ~C 10 Aryl or C 1 ~C 6 alkyl; The R L Selected from -PPh 3 、-PMe 3 , CH 3 CN-, pyridyl, 2-methylpyridyl, 3-methylpyridyl or 4-methylpyridyl; The m is selected from 1 or 2; The n is selected from an integer between 1 and 3.

3. The compound according to claim 1 or 2, It is characterized in that The C 6 ~C 14 Aryl groups also contain substituents; The C 6 ~C 14 The substituents of the aryl group are selected from halogen, C 1 ~C 10 Alkyl, C 1 ~C 6 Alkoxy, fluorine-substituted C 1 ~C 6 One or more of alkyl, nitro, amino, and hydroxyl; The C 1 ~C 20 Alkyl, C 1 ~C 10 Alkoxy groups also contain substituents; The C 1 ~C 20 Alkyl, C 1 ~C 10 The substituent of the alkoxy group is selected from one or more of halogen, nitro, amino and hydroxyl.

4. The compound according to claim 1, It is characterized in that The Ar1 and Ar2 are independently selected from phenyl or naphthyl; The R 1 Selected from H, methyl, tert-butyl, iodine, trifluoromethyl, nitro, p-methylphenyl, p-trifluoromethylphenyl, p-nitrophenyl, m-methylphenyl, m-trifluoromethylphenyl, m-nitrophenyl, o-methylphenyl, o-trifluoromethylphenyl, o-nitrophenyl, anthracenyl, 6-methylanthracenyl, 6-methoxyanthracenyl, 6-tert-butylanthracenyl, 6-chloroanthracenyl, 6-trifluoromethylanthracenyl, 6-nitroanthracenyl, 6-methylanthracenyl; The R 2 is selected from H, methyl, tert-butyl, methoxy, iodine, trifluoromethyl or nitro; The R 3 is selected from H, methyl, methoxy, tert-butyl, fluorine, trifluoromethyl, nitro, methyl, methoxy, tert-butyl, fluorine, trifluoromethyl, nitro, methyl, methoxy, tert-butyl, fluorine, trifluoromethyl or nitro; The R 4 Selected from O, SO 2 or SO; The R 5 Selected from H, methyl, tert-butyl, methoxy, phenyl, One or more of diphenylmethyl, anthracenyl, and naphthyl, and at least One or more of benzhydryl, anthracenyl, and naphthyl; The R 6 , R 7 independently selected from H, halogen, C 1 ~C 10 Alkyl, C 1 ~C 6 One or more of alkoxy; said L is selected from phenyl, naphthyl or methyl; The R L Selected from -PPh 3 、-PMe 3 , CH 3 CN-, pyridyl, 2-methylpyridyl, 3-methylpyridyl or 4-methylpyridyl; The m is selected from 1 or 2; The n is selected from 1 or 2.

5. The compound according to claim 1, It is characterized in that Ar1 and Ar2 are selected from phenyl groups; The R 1 is selected from tert-butyl, anthracenyl, 6-methylanthracenyl, p-methylphenyl, m-methylphenyl, o-methylphenyl or phenyl; The R 2 is selected from H, methyl, tert-butyl or methoxy; The R 3 is selected from H, methyl, methoxy or tert-butyl; The R 4 Selected from SO 2 , L is selected from Ph or methyl, R L Selected from PPh 3 、PMe 3 , CH 3 CN-, pyridyl, 2-methylpyridyl, 3-methylpyridyl or 4-methylpyridyl; The R 5 Selected from H, methyl, tert-butyl, methoxy, phenyl, One or more of diphenylmethyl, anthracenyl, and naphthyl, and at least The R 6 , R 7 Selected from H; The m is selected from 1; The n is selected from 2.

6. The compound according to claim 1, It is characterized in that The compound has any of the following structures:

7. A method for preparing the compound according to claim 1, It is characterized in that The following steps are involved: 1) heating dibenzosuberol and aniline of formula (1) under the action of a catalyst to react to prepare aniline of formula (3); 2) reacting the aniline of formula (3) and the salicylaldehyde of formula (2) in an acidic environment to obtain a ligand of formula (4); 3) reacting the ligand represented by formula (4) and a nickel source in an alkaline environment to prepare a compound represented by formula 1; 8. The preparation method according to claim 7, It is characterized in that In the step 1), the catalyst is selected from a mixed solution of anhydrous zinc chloride and concentrated hydrochloric acid; The heating temperature in step 1) is 120°C to 170°C; The acidic environment in step 2) is provided by one or more of p-toluenesulfonic acid monohydrate, hydrochloric acid, and acetic acid; The alkaline environment in step 3) is provided by one or more of sodium hydride, pyridine, 2-methylpyridine, 3-methylpyridine, and 4-methylpyridine; The nickel source in step 3) is selected from NiMe 2 (tmeda) and containing leaving group R L A mixture of compounds, NiPhCl(PPh 3 ) 2 、NiMe 2 Py 2 One or more of; the leaving group R L R in the compound L Selected from -PPh 3 、-PMe 3 , CH 3 CN-, pyridyl, 2-methylpyridyl, 3-methylpyridyl or 4-methylpyridyl.

9. A method for preparing a polyolefin elastomer, It is characterized in that The polyolefin elastomer is obtained by catalyzing the polymerization reaction of olefin monomers using the compound described in any one of claims 1 to 6 or the compound prepared by the preparation method described in claim 7 or 8.

10. The preparation method according to claim 9, It is characterized in that The polymerization reaction also adds Ni(COD) 2 or B(C 6 F 5 ) 3 .