Carbon fiber reinforced epoxy resin clasp nail as well as preparation method and application thereof
The use of carbon fiber reinforced epoxy resin nails solves the problems of voids and delamination at the joints of carbon/carbon composite insulation felt tubes for high-temperature furnaces, provides higher bonding strength and corrosion resistance, and avoids the contamination of metal nails. problem, achieving lightweight, high strength and high temperature stability.
Patent Information
- Application Number
- CN202410717120.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-04
- Publication Date
- 2024-10-18
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing carbon/carbon composite insulation felt tubes used in high-temperature furnaces are prone to voids and delamination at the splicing points. Traditional metal spatulas produce metal ion by-products after being used at high temperatures, which affects the performance of the felt tube, and is heavy and durable. insufficient.
Nails made of carbon fiber reinforced epoxy resin material are coated with epoxy resin on the surface of carbon fiber wires and cured to form lightweight, high-strength and durable nails for splicing between layers of insulation felt tubes. connection.
It significantly improves the bonding strength and yield of the insulation felt tube, avoids metal ion contamination, simplifies the process, and improves the corrosion resistance and high temperature stability of the product.
Smart Images

Figure CN118791835A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of thermal insulation felt tube connection, and in particular to a carbon fiber reinforced epoxy resin nail and a preparation method and application thereof. Background Art
[0002] Carbon / carbon composite materials are carbon-based composite materials with carbon fibers as the reinforcement phase. They are currently one of the few materials that can maintain high mechanical properties above 2000°C. They have excellent properties such as low specific gravity, high specific strength, high specific modulus, low thermal expansion coefficient, heat shock resistance, and ablation resistance. Therefore, carbon-carbon composite insulation cylinders are widely used in high-temperature industrial equipment such as high-temperature sintering furnaces.
[0003] At present, carbon / carbon composite insulation felt tubes for high-temperature furnaces are mainly of winding structure, that is, carbon felt or graphite felt is used as raw material, resin is used as adhesive, and after winding and forming, it is cured, carbonized and graphitized. This leads to the inevitable use of splicing wraps in the production process of the felt tube, and voids are prone to appear at the splicing.
[0004] The existing technology mostly adopts the method of applying phenolic resin on the joints for bonding, but the application of phenolic resin easily leads to delamination of the joints of the product, which leads to many problems, such as poor thermal insulation performance, difficulty in preparing special-shaped parts, poor interlayer bonding, and easy delamination during use. In addition, it is also proposed to improve the bonding force between insulation felt tubes by setting connecting parts, but traditional connecting parts, such as nails, are mostly made of metal materials, such as steel and iron, which have certain strength, but are heavy, easy to rust and lack durability. And the felt tube usually needs to be carbonized at high temperature, so the metal nails need to be removed in time after use at this temperature, otherwise metal ion byproducts may be generated to pollute the felt tube.
[0005] In view of this, the present invention is proposed. Summary of the invention
[0006] One of the purposes of the present invention is to provide a carbon fiber reinforced epoxy resin nail. The carbon fiber reinforced epoxy resin nail is a nail used to make the connection between the layers of the insulation felt tube more tightly, and is a lightweight, high-strength and durable nail. The nail is made of carbon fiber reinforced epoxy resin material, provides higher strength, and is not removed after use and is directly left inside the insulation felt tube.
[0007] The second object of the present invention is to provide a method for preparing the carbon fiber reinforced epoxy resin nail. The preparation method comprises the following steps: coating the epoxy resin on the surface of the carbon fiber filament, placing it in a mold, and performing a curing treatment to obtain the carbon fiber reinforced epoxy resin nail.
[0008] The third object of the present invention is to provide an application of the carbon fiber reinforced epoxy resin nail as a fixed splicing piece between thermal insulation felt tubes.
[0009] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:
[0010] In a first aspect, the present invention provides a carbon fiber reinforced epoxy resin nail, wherein the carbon fiber reinforced epoxy resin nail comprises a core body and a coating layer;
[0011] Wherein, the core is carbon fiber filaments, and the coating layer is an epoxy resin layer.
[0012] In the present invention, the carbon fiber reinforced epoxy resin nail has a carbon fiber filament as the core body, and an epoxy resin layer is formed on the surface thereof. The carbon fiber reinforced epoxy resin nail has excellent mechanical properties and corrosion resistance. It is applied to the connection between the layers of the insulation felt tube, which can make the insulation felt tube layers more tightly combined and significantly improve the bonding strength of the insulation felt tube. And because the core of the nail is carbon fiber filaments that are resistant to high temperatures, and the residual carbon rate of epoxy resin is very low after high temperatures, it can be made to be wrapped inside the felt tube after use to avoid removal, thereby further improving the performance of the product and increasing the process efficiency of preparing the insulation felt tube.
[0013] Preferably, the diameter of the carbon fiber filaments is 0.1-0.5 mm.
[0014] Preferably, the thickness of the epoxy resin layer is 0.5 to 1 mm;
[0015] Preferably, the epoxy resin layer is formed by coating epoxy resin on the surface of the core and curing it;
[0016] Preferably, the epoxy resin is selected from any one of E-20, E 44, E 51 or E 55, preferably E 51.
[0017] Preferably, the carbon fiber reinforced epoxy resin nail is an integrally formed structure, and the carbon fiber reinforced epoxy resin nail comprises: a nail body, a first nail leg and a second nail leg.
[0018] One end of the first nail leg is connected to one side of the nail body, and the end of the first nail leg away from the nail body has a first barb bent inwardly.
[0019] One end of the second nail leg is connected to the other side of the nail body, and one end of the second nail leg away from the nail body has a second barb bent inwardly.
[0020] Preferably, the horizontal length of the nail body is 20-40 mm.
[0021] Preferably, the nail body is a rod-shaped structure bent inwardly.
[0022] Preferably, the inward curvature of the middle of the nail body is 0-15°.
[0023] Preferably, the arc of the inner angle at the connection between the nail body and the first nail leg is 75-90°; the arc of the inner angle at the connection between the nail body and the second nail leg is 75-90°.
[0024] Preferably, the curvature of the outer angle at the connection between the nail body and the first nail leg is 90-105°; the curvature of the outer angle at the connection between the nail body and the second nail leg is 90-105°.
[0025] Preferably, both the first nail leg and the second nail leg are rod-shaped structures with the lower ends bent inwards.
[0026] Preferably, the bending arc of the first nail leg is 0-15°; the bending arc of the second nail leg is 0-15°.
[0027] Preferably, the vertical height of the first nail leg is less than 10 mm; the vertical height of the second nail leg is less than 10 mm.
[0028] Preferably, the inclined surface length of the first barb is 1-2 mm; the inclined surface length of the second barb is 1-2 mm.
[0029] Preferably, the inner angle between the first barb and the first nail leg is 25-35°; the outer angle between the first barb and the first nail leg is 10-20°;
[0030] Preferably, the inner angle between the second barb and the second nail leg is 25-35°; the outer angle between the second barb and the second nail leg is 10-20°.
[0031] In a second aspect, the present invention provides a method for preparing the carbon fiber reinforced epoxy resin nail as described in the first aspect, the preparation method comprising the following steps:
[0032] The epoxy resin is coated on the surface of the carbon fiber filaments, placed in a mold, and cured to obtain the carbon fiber reinforced epoxy resin nails.
[0033] Preferably, the curing treatment temperature is 120-140° C.; the curing treatment time is 0.5-2 h.
[0034] In a third aspect, the present invention provides an application of the carbon fiber reinforced epoxy resin nail as described in the first aspect as a fixed joint between thermal insulation felt tubes.
[0035] Compared with the prior art, the present invention has the following beneficial effects:
[0036] (1) The carbon fiber reinforced epoxy resin nail described in the present invention is a nail used to make the connection between the layers of the thermal insulation felt tube tighter. The nail is made of carbon fiber reinforced epoxy resin material, which provides higher strength and improves the bonding force between the thermal insulation felt tubes.
[0037] (2) The carbon fiber reinforced epoxy resin nails of the present invention have a very low residual carbon rate after high temperature. After use, they are wrapped inside the felt tube and can be carbonized together with the thermal insulation felt tube without being taken out. After the felt tube is fixed, they do not need to be taken out in time. The operation is simple and convenient, which improves the product yield.
[0038] (3) The felt tube connected by the carbon fiber reinforced epoxy resin nails of the present invention has the advantages of good thermal insulation performance, strong interlayer bonding force, and is not prone to delamination during use. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0040] Figure 1 It is a schematic diagram of the structure of the carbon fiber reinforced epoxy resin nail according to the present invention.
[0041] Among them, 101 is the nail body, 102 is the first nail leg, 103 is the second nail leg, 104 is the first barb, and 105 is the second barb.
[0042] Figure 2 It is a schematic structural diagram of the connection point of the felt tube connected by the carbon fiber reinforced epoxy resin nails of the present invention.
[0043] Among them, 26 is the first soft felt tube, 27 is the place where the nail does not pass through the first soft felt, 28 is the splicing gap, 29 is the place where the nail does not pass through the second soft felt, 30 is the second soft felt tube, 31 is the place where the nail is attached to the second soft felt, and 32 is the place where the nail is attached to the first soft felt. DETAILED DESCRIPTION
[0044] Unless otherwise defined herein, scientific and technical terms used in conjunction with the present invention shall have the meanings commonly understood by those of ordinary skill in the art. The meaning and scope of the terms should be clear, however, in the case of any potential ambiguity, the definitions provided herein take precedence over any dictionary or external definitions. In this application, unless otherwise stated, the use of "or" means "and / or". In addition, the use of the term "including" and other forms is non-limiting.
[0045] It should be noted that specific details are described in the following description to facilitate a full understanding of the present invention. However, the present invention can be implemented in a variety of other ways different from those described herein, and those skilled in the art can make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.
[0046] In the description of the present invention, it should be noted that the terms "center", "upper", "lower", "left", "right", "vertical", "horizontal", "inside", "outside", etc. indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, or the positions or positional relationships in which the product of the invention is usually placed when in use. They are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific position, be constructed and operated in a specific position, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", "third", etc. are only used to distinguish the description, and cannot be understood as indicating or implying relative importance.
[0047] In addition, the terms "horizontal", "vertical", "overhanging" and the like do not mean that the components are required to be absolutely horizontal or overhanging, but can be slightly tilted. For example, "horizontal" only means that its direction is more horizontal than "vertical", and does not mean that the structure must be completely horizontal, but can be slightly tilted.
[0048] In the description of the present invention, it is also necessary to explain that, unless otherwise clearly specified and limited, the terms "set", "install", "connect", and "connect" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0049] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0050] A first aspect of the present invention provides a carbon fiber reinforced epoxy resin nail, the carbon fiber reinforced epoxy resin nail comprising a core body and a coating layer;
[0051] Wherein, the core is carbon fiber filaments, and the coating layer is an epoxy resin layer.
[0052] In the present invention, the carbon fiber reinforced epoxy resin nails are made of carbon fiber carbon filaments to reinforce epoxy resin materials, that is, the epoxy resin mixture is coated on the carbon fiber carbon filaments to form an epoxy resin coating layer. The carbon fiber reinforced epoxy resin nail is a lightweight, high-strength and durable nail. The nail adopts a carbon fiber reinforced epoxy resin composite material, which can effectively improve the product yield and work efficiency.
[0053] As a preferred embodiment of the present invention, the diameter of the carbon fiber filaments is 0.1-0.5 mm, for example, 0.1 mm, 0.2 mm, 0.3 mm, 0.4 mm, 0.5 mm, etc., preferably 0.4-0.6 mm.
[0054] As a preferred embodiment of the present invention, the thickness of the epoxy resin layer is 0.5-1 mm, for example, 0.5 mm, 0.6 mm, 0.7 mm, 0.8 mm, 0.9 mm, 1 mm, etc.
[0055] Preferably, the epoxy resin layer is formed by coating epoxy resin on the surface of the core and curing the epoxy resin.
[0056] Preferably, the epoxy resin is selected from any one of E-20, E 44, E 51 or E 55, preferably E 51.
[0057] As a preferred embodiment of the present invention, Figure 1 As shown, the carbon fiber reinforced epoxy resin nail is an integrally formed structure, and the carbon fiber reinforced epoxy resin nail includes: a nail body 101 , a first nail leg 102 and a second nail leg 103 .
[0058] like Figure 1 As shown, one end of the first nail leg 102 is connected to one side of the nail body 101, and the end of the first nail leg 102 away from the nail body has a first barb 104 bent inwardly.
[0059] like Figure 1 As shown, one end of the second nail leg 103 is connected to the other side of the nail body 101, and the end of the second nail leg 103 away from the nail body has a second barb 105 bent inwardly.
[0060] As a preferred embodiment of the present invention, Figure 1 As shown, the horizontal length l of the nail body 101 101 It is 30 to 50mm, for example, it can be 30mm, 31mm, 32mm, 33mm, 34mm, 35mm, 36mm, 37mm, 38mm, 39mm, 40mm, 41mm, 42mm, 43mm, 44mm, 45mm, 46mm, 47mm, 48mm, 49mm, 50mm, etc.
[0061] As a preferred embodiment of the present invention, Figure 1 As shown, the nail body 101 is a rod-shaped structure bent inwardly.
[0062] As a preferred embodiment of the present invention, the inward bending arc of the middle of the nail body 101 is 0 to 15°, for example, it can be 0.5°, 1°, 2°, 3°, 4°, 5°, 6°, 7°, 8°, 9°, 10°, 11°, 12°, 13°, 14°, 15°, etc.
[0063] As a preferred embodiment of the present invention, Figure 1 As shown, the inner angle R at the connection between the nail body 101 and the first nail leg 102 is i12 The arc is 75 to 90°, for example, it can be 75°, 76°, 77°, 78°, 79°, 80°, 81°, 82°, 83°, 84°, 85°, 86°, 87°, 88°, 89°, 90°, etc.
[0064] As a preferred embodiment of the present invention, Figure 1 As shown, the inner angle radian R of the connection between the nail body 101 and the second nail leg 103 is i13 It is 75 to 90°, for example, it can be 75°, 76°, 77°, 78°, 79°, 80°, 81°, 82°, 83°, 84°, 85°, 86°, 87°, 88°, 89°, 90°, etc.
[0065] As a preferred embodiment of the present invention, Figure 1 As shown, the arc R of the outer angle at the connection between the nail body 101 and the first nail leg 102 e12 It is 90 to 105°, for example, it can be 90°, 91°, 92°, 93°, 94°, 95°, 96°, 97°, 98°, 99°, 100°, 101°, 102°, 103°, 104°, 105°, etc.
[0066] As a preferred embodiment of the present invention, Figure 1 As shown, the outer angle radian R of the connection between the nail body 101 and the second nail leg 103 is e13 It is 90 to 105°, for example, it can be 90°, 91°, 92°, 93°, 94°, 95°, 96°, 97°, 98°, 99°, 100°, 101°, 102°, 103°, 104°, 105°, etc.
[0067] As a preferred embodiment of the present invention, Figure 1 As shown, the first nail leg and the second nail leg are both rod-shaped structures with the lower ends bent inwards.
[0068] As a preferred embodiment of the present invention, the bending radius of the first nail leg 102 is 0 to 15°, for example, it can be 0.5°, 1°, 2°, 3°, 4°, 5°, 6°, 7°, 8°, 9°, 10°, 11°, 12°, 13°, 14°, 15°, etc.
[0069] As a preferred embodiment of the present invention, the bending radius of the second nail leg 103 is 0 to 15°, for example, it can be 0.5°, 1°, 2°, 3°, 4°, 5°, 6°, 7°, 8°, 9°, 10°, 11°, 12°, 13°, 14°, 15°, etc.
[0070] As a preferred embodiment of the present invention, Figure 1 As shown, the vertical height h of the first nail leg 102 102 It is less than 10 mm, for example, it can be 10 mm, 9.5 mm, 9 mm, 8.5 mm, 8 mm, 7.5 mm, 7 mm, 6.5 mm, 6 mm, 5 mm, etc.
[0071] As a preferred embodiment of the present invention, Figure 1 As shown, the vertical height h of the second nail leg 103 is 103 It is less than 10 mm, for example, it can be 10 mm, 9.5 mm, 9 mm, 8.5 mm, 8 mm, 7.5 mm, 7 mm, 6.5 mm, 6 mm, 5 mm, etc.
[0072] As a preferred embodiment of the present invention, Figure 1 As shown, the inclined length l of the first barb 104 It is 1 to 2 mm, for example, it can be 1 mm, 1.1 mm, 1.2 mm, 1.3 mm, 1.4 mm, 1.5 mm, 1.6 mm, 1.7 mm, 1.8 mm, 1.9 mm, 2 mm, etc.
[0073] As a preferred embodiment of the present invention, Figure 1 As shown, the inclined length l of the first barb 105 It is 1 to 2 mm, for example, it can be 1 mm, 1.1 mm, 1.2 mm, 1.3 mm, 1.4 mm, 1.5 mm, 1.6 mm, 1.7 mm, 1.8 mm, 1.9 mm, 2 mm, etc.
[0074] As a preferred embodiment of the present invention, Figure 1 As shown, the first barb 104 and the inner side of the first nail leg 102 are angled R i24It is 25 to 35°, for example, it can be 25°, 26°, 27°, 28°, 29°, 30°, 31°, 32°, 33°, 34°, 35°, etc.
[0075] As a preferred embodiment of the present invention, Figure 1 As shown, the first barb 104 and the outer side of the first nail leg 102 are angled R e24 It is 10 to 20°, for example, it can be 10°, 11°, 12°, 13°, 14°, 15°, 16°, 17°, 18°, 19°, 20°, etc.
[0076] As a preferred embodiment of the present invention, Figure 1 As shown, the inner angle R between the second barb 105 and the second nail leg 103 is i35 It is 25 to 35°, for example, it can be 25°, 26°, 27°, 28°, 29°, 30°, 31°, 32°, 33°, 34°, 35°, etc.
[0077] As a preferred embodiment of the present invention, Figure 1 As shown, the outer included angle R between the second barb 105 and the second nail leg 103 is e35 It is 10 to 20°, for example, it can be 10°, 11°, 12°, 13°, 14°, 15°, 16°, 17°, 18°, 19°, 20°, etc.
[0078] In a second aspect, the present invention provides a method for preparing the carbon fiber reinforced epoxy resin nail as described in the first aspect, the preparation method comprising the following steps:
[0079] The epoxy resin is coated on the surface of the carbon fiber filaments, placed in a mold, and cured to obtain the carbon fiber reinforced epoxy resin nails.
[0080] As a preferred embodiment of the present invention, the temperature of the curing treatment is 120-140°C, for example, it can be 120°C, 121°C, 122°C, 123°C, 124°C, 125°C, 126°C, 127°C, 128°C, 129°C, 130°C, 131°C, 132°C, 133°C, 134°C, 135°C, 136°C, 137°C, 138°C, 139°C, 140°C, etc.
[0081] As a preferred embodiment of the present invention, the curing treatment time is 0.5 to 2 hours, for example, it can be 0.5h, 0.6h, 0.7h, 0.8h, 0.9h, 1.1h, 1.2h, 1.3h, 1.4h, 1.5h, 1.6h, 1.7h, 1.8h, 1.9h, 2h, etc.
[0082] In a third aspect, the present invention provides an application of the carbon fiber reinforced epoxy resin nail as described in the first aspect as a fixed joint between thermal insulation felt tubes.
[0083] like Figure 2 As shown, the carbon fiber reinforced epoxy resin nails of the present invention can be used for connecting the joints between the layers of the insulation felt tube, which can make the layers of the insulation felt tube more tightly combined and significantly improve the bonding strength of the insulation felt tube.
[0084] The present invention is further described below by way of examples. Unless otherwise specified, the materials in the examples are prepared according to existing methods or directly purchased from the market.
[0085] Example 1
[0086] The present embodiment provides a carbon fiber reinforced epoxy resin nail, which includes a core and a coating layer; wherein the core is a carbon fiber filament with a diameter of 0.5 mm, and the coating layer is an epoxy resin layer with a thickness of 0.5 mm; and the epoxy resin layer is formed by coating epoxy resin E 51 on the surface of the carbon fiber filament and curing it.
[0087] The carbon fiber reinforced epoxy resin nail is an integrally formed structure, and the carbon fiber reinforced epoxy resin nail includes: a nail body, a first nail leg and a second nail leg; wherein, one end of the first nail leg is connected to one side of the nail body, and the end of the first nail leg away from the nail body has a first barb bent inwardly; wherein, one end of the second nail leg is connected to the other side of the nail body, and the end of the second nail leg away from the nail body has a second barb bent inwardly.
[0088] The horizontal length of the nail body is 40 mm, and the nail body is a rod-shaped structure that bends inwardly, and the inward bending arc in the middle of the nail body is 10°.
[0089] The curvature of the inner angle at the connection between the nail body and the first nail leg is 90°; the curvature of the inner angle at the connection between the nail body and the second nail leg is 90°. The curvature of the outer angle at the connection between the nail body and the first nail leg is 105°; the curvature of the outer angle at the connection between the nail body and the second nail leg is 105°. Both the first nail leg and the second nail leg are rod-shaped structures with the lower end bent inward; the curvature of the first nail leg is 15°; the curvature of the second nail leg is 15°; the vertical height of the first nail leg is 10 mm; the vertical height of the second nail leg is 10 mm.
[0090] Among them, the inclined length of the first barb is 1.5mm; the inclined length of the second barb is 1.5mm; the inner angle between the first barb and the first nail leg is 30°; the outer angle between the first barb and the first nail leg is 15°; the inner angle between the second barb and the second nail leg is 30°; the outer angle between the second barb and the second nail leg is 15°.
[0091] The carbon fiber reinforced epoxy resin nails in this embodiment are prepared by the following steps:
[0092] The epoxy resin E51 is coated on the surface of the carbon fiber filaments, placed in a mold, and the mold is placed in a heating press. The mold is heated at 130° C. for 1 hour to solidify the epoxy resin E51 to form the desired nail shape. After cooling, the mold is demolded to obtain the carbon fiber reinforced epoxy resin nail.
[0093] Example 2
[0094] The present embodiment provides a carbon fiber reinforced epoxy resin nail, which includes a core and a coating layer; wherein the core is a carbon fiber filament with a diameter of 0.2 mm, and the coating layer is an epoxy resin layer with a thickness of 1 mm; and the epoxy resin layer is formed by coating epoxy resin E 51 on the surface of the carbon fiber filament and curing it.
[0095] The carbon fiber reinforced epoxy resin nail is an integrally formed structure, and the carbon fiber reinforced epoxy resin nail includes: a nail body, a first nail leg and a second nail leg; wherein, one end of the first nail leg is connected to one side of the nail body, and the end of the first nail leg away from the nail body has a first barb bent inwardly; wherein, one end of the second nail leg is connected to the other side of the nail body, and the end of the second nail leg away from the nail body has a second barb bent inwardly.
[0096] The horizontal length of the nail body is 35 mm, and the nail body is a rod-shaped structure that bends inwardly, and the inward bending arc in the middle of the nail body is 15°.
[0097] The curvature of the inner angle at the connection between the nail body and the first nail leg is 80°; the curvature of the inner angle at the connection between the nail body and the second nail leg is 80°. The curvature of the outer angle at the connection between the nail body and the first nail leg is 100°; the curvature of the outer angle at the connection between the nail body and the second nail leg is 100°. Both the first nail leg and the second nail leg are rod-shaped structures with the lower ends bent inwards; the curvature of the first nail leg is 10°; the curvature of the second nail leg is 10°; the vertical height of the first nail leg is 8 mm; the vertical height of the second nail leg is 8 mm.
[0098] Among them, the inclined length of the first barb is 1mm; the inclined length of the second barb is 1mm; the inner angle between the first barb and the first nail leg is 35°; the outer angle between the first barb and the first nail leg is 20°; the inner angle between the second barb and the second nail leg is 35°; the outer angle between the second barb and the second nail leg is 20°.
[0099] The carbon fiber reinforced epoxy resin nails in this embodiment are prepared by the following steps:
[0100] The epoxy resin E51 is coated on the surface of the carbon fiber filaments, placed in a mold, the mold is placed in a heating press, and heated at 120° C. for 1.5 hours to solidify the epoxy resin E51 to form the desired nail shape, and then demolded after cooling to obtain the carbon fiber reinforced epoxy resin nail.
[0101] Example 3
[0102] The present embodiment provides a carbon fiber reinforced epoxy resin nail, which includes a core and a coating layer; wherein the core is a carbon fiber filament with a diameter of 0.1 mm, and the coating layer is an epoxy resin layer with a thickness of 0.7 mm; and the epoxy resin layer is formed by coating epoxy resin E 51 on the surface of the carbon fiber filament and curing it.
[0103] The carbon fiber reinforced epoxy resin nail is an integrally formed structure, and the carbon fiber reinforced epoxy resin nail includes: a nail body, a first nail leg and a second nail leg; wherein, one end of the first nail leg is connected to one side of the nail body, and the end of the first nail leg away from the nail body has a first barb bent inwardly; wherein, one end of the second nail leg is connected to the other side of the nail body, and the end of the second nail leg away from the nail body has a second barb bent inwardly.
[0104] The horizontal length of the nail body is 45 mm, and the nail body is a rod-shaped structure that bends inwardly, and the inward bending arc in the middle of the nail body is 5°.
[0105] The curvature of the inner angle at the connection between the nail body and the first nail leg is 75°; the curvature of the inner angle at the connection between the nail body and the second nail leg is 75°. The curvature of the outer angle at the connection between the nail body and the first nail leg is 90°; the curvature of the outer angle at the connection between the nail body and the second nail leg is 90°. Both the first nail leg and the second nail leg are rod-shaped structures with the lower end bent inward; the curvature of the first nail leg is 5°; the curvature of the second nail leg is 5°; the vertical height of the first nail leg is 10 mm; the vertical height of the second nail leg is 10 mm.
[0106] Among them, the inclined length of the first barb is 2mm; the inclined length of the second barb is 2mm; the inner angle between the first barb and the first nail leg is 25°; the outer angle between the first barb and the first nail leg is 10°; the inner angle between the second barb and the second nail leg is 25°; the outer angle between the second barb and the second nail leg is 10°.
[0107] The carbon fiber reinforced epoxy resin nails in this embodiment are prepared by the following steps:
[0108] The epoxy resin E51 is coated on the surface of the carbon fiber filaments, placed in a mold, and the mold is placed in a heating press. The epoxy resin E51 is heated at 135° C. for 40 minutes to solidify the epoxy resin E51 to form the desired nail shape. The nail is demolded after cooling to obtain the carbon fiber reinforced epoxy resin nail.
[0109] Example 4
[0110] This embodiment provides a carbon fiber reinforced epoxy resin nail, which is different from Embodiment 1 only in that epoxy resin E51 is replaced by epoxy resin E44, and other parameters are completely consistent with Embodiment 1.
[0111] Example 5
[0112] This embodiment provides a carbon fiber reinforced epoxy resin nail, which is different from Embodiment 1 only in that epoxy resin E51 is replaced by epoxy resin E55, and other parameters are completely consistent with Embodiment 1.
[0113] Comparative Example 1
[0114] This comparative example provides a carbon fiber nail, wherein the carbon fiber reinforced epoxy resin nail is formed only by carbon fiber filaments with a diameter of 1 mm.
[0115] The carbon fiber nail is an integrally formed structure, and includes: a nail body, a first nail leg and a second nail leg; wherein one end of the first nail leg is connected to one side of the nail body, and the end of the first nail leg away from the nail body has a first barb bent inwardly; wherein one end of the second nail leg is connected to the other side of the nail body, and the end of the second nail leg away from the nail body has a second barb bent inwardly.
[0116] The horizontal length of the nail body is 40 mm, and the nail body is a rod-shaped structure that bends inwardly, and the inward bending arc in the middle of the nail body is 10°.
[0117] The curvature of the inner angle at the connection between the nail body and the first nail leg is 90°; the curvature of the inner angle at the connection between the nail body and the second nail leg is 90°. The curvature of the outer angle at the connection between the nail body and the first nail leg is 105°; the curvature of the outer angle at the connection between the nail body and the second nail leg is 105°. Both the first nail leg and the second nail leg are rod-shaped structures with the lower end bent inward; the curvature of the first nail leg is 15°; the curvature of the second nail leg is 15°; the vertical height of the first nail leg is 10 mm; the vertical height of the second nail leg is 10 mm.
[0118] Among them, the inclined length of the first barb is 1.5mm; the inclined length of the second barb is 1.5mm; the inner angle between the first barb and the first nail leg is 30°; the outer angle between the first barb and the first nail leg is 15°; the inner angle between the second barb and the second nail leg is 30°; the outer angle between the second barb and the second nail leg is 15°.
[0119] The carbon fiber nails in this embodiment are prepared by the following steps:
[0120] The carbon fiber filaments are placed in a mold, the mold is placed in a heating press, and heated at 130° C. for 1 hour to form a desired nail shape, and the mold is demoulded after cooling to obtain the carbon fiber nail.
[0121] Comparative Example 2
[0122] This comparative example provides an epoxy resin nail, which is formed by thermally curing epoxy resin E51, and the diameter of the nail is 1 mm.
[0123] The epoxy resin nail is an integrally formed structure, and includes: a nail body, a first nail leg and a second nail leg; wherein one end of the first nail leg is connected to one side of the nail body, and the end of the first nail leg away from the nail body has a first barb bent inwardly; wherein one end of the second nail leg is connected to the other side of the nail body, and the end of the second nail leg away from the nail body has a second barb bent inwardly.
[0124] The horizontal length of the nail body is 40 mm, and the nail body is a rod-shaped structure that bends inwardly, and the inward bending arc in the middle of the nail body is 10°.
[0125] The curvature of the inner angle at the connection between the nail body and the first nail leg is 90°; the curvature of the inner angle at the connection between the nail body and the second nail leg is 90°. The curvature of the outer angle at the connection between the nail body and the first nail leg is 105°; the curvature of the outer angle at the connection between the nail body and the second nail leg is 105°. Both the first nail leg and the second nail leg are rod-shaped structures with the lower end bent inward; the curvature of the first nail leg is 15°; the curvature of the second nail leg is 15°; the vertical height of the first nail leg is 10 mm; the vertical height of the second nail leg is 10 mm.
[0126] Among them, the inclined length of the first barb is 1.5mm; the inclined length of the second barb is 1.5mm; the inner angle between the first barb and the first nail leg is 30°; the outer angle between the first barb and the first nail leg is 15°; the inner angle between the second barb and the second nail leg is 30°; the outer angle between the second barb and the second nail leg is 15°.
[0127] The epoxy resin nails in this embodiment are prepared by the following steps:
[0128] The epoxy resin E51 is placed in a mold, and the mold is placed in a heating press. The epoxy resin E51 is heated at 130° C. for 1 hour to solidify the epoxy resin E51 to form a desired nail shape. The epoxy resin nail is demoulded after cooling to obtain the epoxy resin nail.
[0129] Comparative Example 3
[0130] This comparative example provides a carbon fiber reinforced phenolic resin nail, which is different from Example 1 only in that the epoxy resin layer is replaced by a phenolic resin layer of equal thickness, and the phenolic resin is the phenolic resin PF9501 produced by Shengquan. Other parameters are exactly the same as those in Example 1.
[0131] Comparative Example 4
[0132] This comparative example provides a carbon fiber reinforced phenolic resin nail, which is different from Example 1 only in that the first nail leg has no first barb at the end away from the nail body, and the second nail leg has no second barb at the end away from the nail body, and other parameters are exactly the same as Example 1.
[0133] Test Example 1
[0134] Test samples: carbon fiber reinforced epoxy resin nails provided in Examples 1 to 5, and nails provided in Comparative Examples 1 to 4;
[0135] Test method:
[0136] (1) Quality: Use a weighing instrument to test the quality of each carbon fiber reinforced epoxy resin nail;
[0137] (2) Mechanical strength: The tensile strength, impact strength and bending strength of each nail were tested according to GB / T2567-2008;
[0138] (3) Interlayer bonding strength: The above-mentioned nails are used at the interlayer joints of two carbon-carbon composite insulation felt tubes of the same material and specification to connect the two, and are simultaneously carbonized at 2000°C. The interlayer bonding strength of the two insulation felt tubes is then tested.
[0139] The specific test results are shown in Table 1:
[0140] Table 1
[0141]
[0142] As shown in Table 1, the carbon fiber reinforced epoxy resin nail has a carbon fiber filament as the core body, and an epoxy resin layer is formed on the surface thereof. The carbon fiber reinforced epoxy resin nail has excellent mechanical properties and corrosion resistance. When applied to the connection between the layers of the insulation felt tube, the insulation felt tube can be more tightly bonded and the bonding strength of the insulation felt tube can be significantly improved. And because the core of the nail is carbon fiber filaments that are resistant to high temperatures, and the residual carbon rate of epoxy resin after high temperatures is very low, it can be made to be wrapped inside the felt tube after use to avoid removal, thereby further improving the performance of the product and increasing the process efficiency of preparing the insulation felt tube.
[0143] It can be seen from the test results of Comparative Examples 1 and 2 that although the nails prepared using only carbon fiber filaments or only epoxy resin are light in weight, their mechanical properties are very poor, which results in poor bonding strength between the insulation felt tube layers and easy disconnection after the two are used to connect the two layers of insulation felt tubes.
[0144] From the test results of Comparative Example 3, it can be seen that although the hardness of phenolic resin is not a problem, the nails are still very hard after carbonization at high temperature, which significantly reduces the thermal insulation of the product, so the use effect is poor.
[0145] It can be seen from the test results of comparative example 4 that if the nails are not provided with barbs, their tensile strength will be significantly reduced, which is not conducive to the connection between the layers of the thermal insulation felt tube.
[0146] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A carbon fiber reinforced epoxy resin nail, characterized in that: The carbon fiber reinforced epoxy resin nail comprises a core body and a coating layer; Wherein, the core is carbon fiber filaments, and the coating layer is an epoxy resin layer.
2. The carbon fiber reinforced epoxy resin nail according to claim 1, characterized in that: The diameter of the carbon fiber filaments is 0.1-0.5 mm.
3. The carbon fiber reinforced epoxy resin nail according to claim 1, characterized in that: The thickness of the epoxy resin layer is 0.5 to 1 mm; Preferably, the epoxy resin layer is formed by coating epoxy resin on the surface of the core and curing it; Preferably, the epoxy resin is selected from any one of E-20, E 44, E 51 or E 55, preferably E 51.
4. The carbon fiber reinforced epoxy resin nail according to claim 1, characterized in that: The carbon fiber reinforced epoxy resin nail is an integrally formed structure, and the carbon fiber reinforced epoxy resin nail comprises: a nail body, a first nail leg and a second nail leg; Wherein, one end of the first nail leg is connected to one side of the nail body, and the end of the first nail leg away from the nail body has a first barb bent inwardly; One end of the second nail leg is connected to the other side of the nail body, and one end of the second nail leg away from the nail body has a second barb bent inwardly.
5. The carbon fiber reinforced epoxy resin nail according to claim 4, characterized in that: The horizontal length of the nail body is 30 to 50 mm; Preferably, the nail body is a rod-shaped structure bent inwardly; Preferably, the inward curvature of the middle of the nail body is 0-15°.
6. The carbon fiber reinforced epoxy resin nail according to claim 4, characterized in that: The arc of the inner angle at the connection between the nail body and the first nail leg is 75 to 90 degrees; the arc of the inner angle at the connection between the nail body and the second nail leg is 75 to 90 degrees; Preferably, the curvature of the outer angle at the connection between the nail body and the first nail leg is 90-105°; the curvature of the outer angle at the connection between the nail body and the second nail leg is 90-105°; Preferably, the first nail leg and the second nail leg are both rod-shaped structures with the lower ends bent inwards; Preferably, the curvature of the first nail leg is 0-15°; the curvature of the second nail leg is 0-15°; Preferably, the vertical height of the first nail leg is less than 10 mm; the vertical height of the second nail leg is less than 10 mm.
7. The carbon fiber reinforced epoxy resin nail according to claim 4, characterized in that: The inclined surface length of the first barb is 1 to 2 mm; the inclined surface length of the second barb is 1 to 2 mm; Preferably, the inner angle between the first barb and the first nail leg is 25-35°; the outer angle between the first barb and the first nail leg is 10-20°; Preferably, the inner angle between the second barb and the second nail leg is 25-35°; the outer angle between the second barb and the second nail leg is 10-20°.
8. A method for preparing carbon fiber reinforced epoxy resin nails according to any one of claims 1 to 7, characterized in that: The preparation method comprises the following steps: The epoxy resin is coated on the surface of the carbon fiber filaments, placed in a mold, and cured to obtain the carbon fiber reinforced epoxy resin nails.
9. The method for preparing carbon fiber reinforced epoxy resin nails according to claim 8, characterized in that: The temperature of the curing treatment is 120-140° C.; the time of the curing treatment is 0.5-2 hours.
10. Use of the carbon fiber reinforced epoxy resin nail according to any one of claims 1 to 7 as a fixed splicing piece between thermal insulation felt tubes.
Citation Information
Patent Citations
Multi-material joints and methods
CN104210157A
U-shaped bone nail having muscle / bone induction activity and realizing flexible connection after degradation
CN111227916A
Preforms for moulding process and resins therefor
CN1261303A
Dog node of oblique raw bamboo beam and horizontal supporting wood beam
CN202416581U