High-durability anti-cracking building coating and preparation method thereof
Through nano-scale grinding and high-shear homogenization combined with specific material ratios, the problems of insufficient durability, crack resistance and environmental protection of tunnel fire retardant coatings are solved, achieving high durability of the coating and improving construction efficiency. , suitable for complex environments.
Patent Information
- Application Number
- CN202411045138.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-10-18
AI Technical Summary
Existing tunnel fire-retardant coatings have deficiencies in durability, crack resistance, and environmental protection, which lead to early failure of the coating, low construction efficiency, high cost, and uneven pigment dispersion, making it difficult to meet the needs of complex and changing environments.
Using nano-scale sand mill grinding and high-shear homogenizer homogenization methods, combined with acrylic emulsion, polyvinyl alcohol fiber, iron oxide red and calcium carbonate and other materials, the ratio and process are optimized to prepare high durability Crack-resistant architectural coatings ensure the uniformity and stability of the coating.
It significantly improves the durability, crack resistance and color uniformity of the coating, extends its service life, improves construction efficiency and cost performance, is suitable for various harsh environments, and meets the needs of more special scenes.
Smart Images

Figure CN118791918A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to but is not limited to the technical field of architectural coatings, and in particular relates to a highly durable anti-cracking architectural coating and a preparation method thereof. Background Art
[0002] Although existing tunnel fire retardant coatings have made some progress in fire prevention and water resistance, they still need to be further improved in terms of comprehensive performance such as durability, crack resistance, and environmental protection. Especially in the complex and changeable tunnel environment, the durability (such as freeze-thaw resistance, wind and earthquake resistance, etc.), water resistance, and crack resistance of the coating need to meet higher standards to meet long-term use requirements.
[0003] Traditional tunnel fire retardant coatings often contain some harmful substances, such as ammonium polyphosphate and melamine, which release harmful gases during the construction process, posing a potential threat to the environment and the health of construction workers. Therefore, it is urgent to develop more environmentally friendly tunnel fire retardant coatings to reduce or avoid the use of harmful substances.
[0004] The construction efficiency and cost of existing tunnel fire retardant coatings are also urgent issues to be solved. Improving the sprayability of coatings and reducing drying time can help improve construction efficiency; at the same time, optimizing the formula and preparation process to reduce coating costs and improve cost performance is also the focus of the current industry.
[0005] Highly durable, waterproof, crack-resistant and environmentally friendly tunnel fire retardant coatings have urgent technical problems to be solved in terms of comprehensive performance improvement, environmental performance optimization, construction efficiency and cost, specifically:
[0006] Insufficient durability of coatings: During use, existing architectural coatings often fail prematurely due to poor weather resistance and anti-aging performance, requiring frequent maintenance.
[0007] Poor crack resistance: Traditional architectural coatings are often unable to effectively resist wall cracks, causing cracks to appear on the coating surface.
[0008] Uneven pigment dispersion: During the preparation process of existing coatings, the pigment dispersion is often not uniform, resulting in mottled color of the coating.
[0009] Poor uniformity of paint slurry: When preparing traditional paint, it is difficult to ensure the uniformity of the slurry, which affects the performance of the paint and the construction effect. Summary of the invention
[0010] In view of the problems existing in the prior art, the present invention provides a highly durable anti-cracking architectural coating and a preparation method thereof.
[0011] The present invention is achieved by a method for preparing a highly durable anti-cracking architectural coating, comprising the following steps:
[0012] Step 1: prepare base material, anti-cracking reinforcing agent, weather-resistant pigment, filler and other additives;
[0013] Step 2, mixing the components in a certain proportion and grinding them using a nano-scale sand mill;
[0014] Step 3, homogenizing the ground coating slurry using a high shear homogenizer;
[0015] Step 4: Pack the prepared high-durability anti-cracking architectural coating and store it in a dry and cool place.
[0016] Furthermore, the base material is acrylic emulsion, the anti-cracking reinforcing agent is polyvinyl alcohol fiber, the weather-resistant pigment is red iron oxide, and the filler is calcium carbonate.
[0017] Furthermore, the filler may be added with a dispersant, a defoamer, and a leveling agent as required.
[0018] Furthermore, the mixing ratio is: acrylic emulsion accounts for 40-50% of the total weight, polyvinyl alcohol fiber accounts for 1-2% of the total weight, red iron oxide accounts for 5-10% of the total weight, and calcium carbonate accounts for 30-40% of the total weight.
[0019] Furthermore, the grinding time is 2-4 hours, and the particle size after grinding is 50-100 nanometers.
[0020] Furthermore, the homogenization treatment time is 1-2 hours to ensure the uniformity of the coating slurry.
[0021] Another object of the present invention is to provide a method for preparing a highly durable anti-cracking architectural coating.
[0022] In combination with the above technical solutions and the technical problems solved, the advantages and positive effects of the technical solutions to be protected by the present invention are as follows:
[0023] First, the technical solution of the present invention effectively solves multiple technical problems existing in existing architectural coatings, and has achieved significant technical progress in coating performance, service life, construction effect and application scope.
[0024] 1. Improved the overall performance of the coating:
[0025] By optimizing the component ratio and preparation process, the coating has achieved significant improvements in durability, crack resistance, color uniformity, etc.
[0026] The present invention significantly improves the durability of the coating by optimizing the selection and ratio of the base material, the anti-cracking enhancer, the weather-resistant pigment and the filler; adopts a high-efficiency anti-cracking enhancer and optimizes its dispersion and combination mode, so that the coating has excellent anti-cracking performance; adopts a nano-scale sand mill for grinding to ensure uniform dispersion of the pigment in the coating; and performs homogenization treatment through a high-shear homogenizer to significantly improve the uniformity of the coating slurry.
[0027] 2. Extend the service life of the coating:
[0028] Due to the enhanced durability of the coating, its service life is significantly extended, reducing maintenance frequency and costs.
[0029] 3. Improve the construction effect of coating:
[0030] The uniformity of the coating slurry is improved, making the construction smoother and the coating surface smoother and more beautiful.
[0031] 4. Broadened the application scope of coatings:
[0032] It is suitable for various harsh environments, broadens the application scope of coatings, and meets the needs of more special scenarios.
[0033] Second, the highly durable anti-cracking architectural coating and its preparation method of the present invention are intended to solve some key technical problems existing in the prior art and bring about significant technical progress. Specifically, the technical solution solves the following technical problems and brings about the following technical progress:
[0034] Technical problems in the prior art:
[0035] 1) Insufficient crack resistance: Traditional architectural coatings are prone to cracking during use, causing the protective layer to fail, thus affecting the durability and appearance of the building.
[0036] 2) Poor weather resistance: Existing coatings show degradation when exposed to various weather conditions (such as ultraviolet rays, rain, temperature changes, etc.) for a long time, thereby reducing their service life.
[0037] 3) Uniformity and stability issues: Traditional coatings have uneven or unstable problems during the mixing and grinding process, which affects the performance and construction effect of the final coating.
[0038] 4) Particle size does not meet the standard: The grinding process in the existing technology cannot effectively control the size of the particles, resulting in limited texture and performance of the coating.
[0039] Technological progress and significant results:
[0040] 1) Improve crack resistance:
[0041] Introduction of anti-crack enhancers: By adding polyvinyl alcohol fibers as anti-crack enhancers to the formulation, the crack resistance of the coating has been significantly improved. These fibers can effectively disperse stress and prevent cracks from occurring during the drying and curing process of the coating.
[0042] 2) Enhanced weather resistance:
[0043] Use weather-resistant pigments: Selecting red iron oxide as a weather-resistant pigment can significantly improve the paint's UV resistance and enhance its stability and durability under various climatic conditions.
[0044] 3) Improve uniformity and stability:
[0045] Nano-level grinding: By using a nano-level sand mill to grind, a paint with a particle size in the range of 50-100 nanometers is obtained, which improves the uniformity and fineness of the paint.
[0046] High shear homogenization: Use a high shear homogenizer to homogenize the ground paint slurry to ensure the uniformity and stability of the paint and reduce problems during the paint application process.
[0047] 4) Optimize particle size:
[0048] Precise control of particle size: This method controls the grinding time to 2-4 hours to ensure that the particle size is within a specific range (70-100 nanometers), thereby improving the texture and coating performance of the coating.
[0049] 5) Standardized production process:
[0050] Standardized preparation steps: By specifying the mixing ratio, grinding time, homogenization time and other steps in detail, the standardization and consistency of coating production are ensured, and the quality and repeatability of the product are improved.
[0051] The present invention solves the problems of crack resistance, weather resistance, uniformity, stability and other issues in the prior art by introducing advanced materials and technologies into the coating formula and preparation method, and significantly improves the overall performance of highly durable crack-resistant architectural coatings. These technological advances enable the coatings to effectively protect buildings for a long time in various harsh environments, extend their service life, and improve the quality of construction and application. BRIEF DESCRIPTION OF THE DRAWINGS
[0052] Figure 1 The present invention provides a flow chart of a method for preparing a highly durable, crack-resistant architectural coating. DETAILED DESCRIPTION
[0053] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0054] like Figure 1 As shown, a method for preparing a highly durable anti-cracking architectural coating provided by an embodiment of the present invention comprises the following steps:
[0055] Step 1: prepare base material, anti-cracking reinforcing agent, weather-resistant pigment, filler and other additives;
[0056] Step 2, mixing the components in a certain proportion and grinding them using a nano-scale sand mill;
[0057] Step 3, homogenizing the ground coating slurry using a high shear homogenizer;
[0058] Step 4: Pack the prepared high-durability anti-cracking architectural coating and store it in a dry and cool place.
[0059] The following is a specific method for preparing a highly durable anti-cracking architectural coating:
[0060] 1. Base material preparation:
[0061] Choose high-quality latex paint or water-based paint as the base paint to ensure that it has good adhesion and basic performance.
[0062] Acrylic emulsion is selected as the main base material.
[0063] 2. Preparation of anti-cracking enhancer:
[0064] Select special high molecular polymer as anti-cracking enhancer.
[0065] Polyvinyl alcohol fiber is selected as the anti-cracking reinforcing agent.
[0066] 3. Weather-resistant pigment preparation:
[0067] Choose pigments with good weather resistance and stable color.
[0068] Red iron oxide is selected as the weather-resistant pigment.
[0069] 4. Preparation of fillers and other additives:
[0070] Calcium carbonate is selected as the main filler.
[0071] Add appropriate amount of dispersant, defoamer, leveling agent, etc. as needed to improve the processing and application performance of the coating.
[0072] 5. Mixing and grinding:
[0073] The components are mixed in the following proportions: acrylic emulsion accounts for 40-50% of the total weight, polyvinyl alcohol fiber accounts for 1-2% of the total weight, red iron oxide accounts for 5-10% of the total weight, and calcium carbonate accounts for 30-40% of the total weight.
[0074] Use a nano-scale sand mill for grinding for 2-4 hours until the coating particle size reaches 50-100 nanometers.
[0075] 6. Homogenization treatment:
[0076] The ground coating slurry is homogenized by a high shear homogenizer for 1-2 hours to ensure the uniformity of the coating slurry.
[0077] 7. Packaging and storage:
[0078] The prepared high-durability anti-cracking architectural coating is packaged and stored in a dry, cool place, avoiding direct sunlight and high temperature environment.
[0079] Through the above steps, a building coating with high durability and excellent crack resistance can be prepared, which is suitable for coating the exterior and interior walls of various buildings.
[0080] The following are six specific examples of highly durable crack-resistant architectural coatings:
[0081] Embodiment 1:
[0082] Base material: Acrylic emulsion, 45% by weight
[0083] Anti-cracking reinforcement: polyvinyl alcohol fiber, 1.5% of the total weight
[0084] Weathering pigment: Red iron oxide, 7% by weight
[0085] Filler: Calcium carbonate, 35% by weight
[0086] Grinding equipment: nanometer sand mill, grinding time 3 hours, particle size 70 nanometers
[0087] Homogenization: High shear homogenizer, processing time 1.5 hours
[0088] Embodiment 2:
[0089] Base material: Acrylic emulsion, 40% by weight
[0090] Anti-cracking reinforcement: polyvinyl alcohol fiber, 2% of the total weight
[0091] Weathering pigment: Red iron oxide, 5% by weight
[0092] Filler: Calcium carbonate, 40% by weight
[0093] Grinding equipment: nano-scale sand mill, grinding time 2 hours, particle size 50 nanometers Homogenization treatment: high shear homogenizer, processing time 1 hour
[0094] Embodiment 3:
[0095] Base material: acrylic emulsion, 50% by weight
[0096] Anti-cracking reinforcement: polyvinyl alcohol fiber, 1% of the total weight
[0097] Weathering pigment: Red iron oxide, 10% by weight
[0098] Filler: Calcium carbonate, 30% by weight
[0099] Grinding equipment: nano-scale sand mill, grinding time 4 hours, particle size 100 nanometers Homogenization treatment: high shear homogenizer, processing time 2 hours
[0100] Embodiment 4:
[0101] Base material: Acrylic emulsion, 47% by weight
[0102] Anti-cracking reinforcement: polyvinyl alcohol fiber, accounting for 1.8% of the total weight
[0103] Weathering pigment: Red iron oxide, 8% by weight
[0104] Filler: Calcium carbonate, 34% by weight
[0105] Grinding equipment: nano-scale sand mill, grinding time 2.5 hours, particle size 60 nanometers Homogenization treatment: high shear homogenizer, processing time 1.75 hours
[0106] Embodiment 5:
[0107] Base material: Acrylic emulsion, 42% by weight
[0108] Anti-cracking reinforcement: polyvinyl alcohol fiber, accounting for 1.2% of the total weight
[0109] Weathering pigment: Red iron oxide, 6% by weight
[0110] Filler: Calcium carbonate, 38% by weight
[0111] Grinding equipment: nano-scale sand mill, grinding time 3.5 hours, particle size 80 nanometers Homogenization treatment: high shear homogenizer, processing time 1.25 hours
[0112] Embodiment 6:
[0113] Base material: Acrylic emulsion, 48% by weight
[0114] Anti-cracking reinforcement: polyvinyl alcohol fiber, accounting for 1.7% of the total weight
[0115] Weathering pigment: Red iron oxide, 9% by weight
[0116] Filler: Calcium carbonate, 33% by weight
[0117] Grinding equipment: nano-scale sand mill, grinding time 2.75 hours, particle size 75 nanometers
[0118] Homogenization: High shear homogenizer, processing time 1.8 hours
[0119] These examples show the specific proportions and preparation conditions of different components to prepare highly durable anti-cracking architectural coatings. In practical applications, these examples can be adjusted and optimized according to specific needs and conditions.
[0120] In order to specifically illustrate the technical effect of the present invention, we can use the following data to demonstrate the significant technical progress of the highly durable anti-cracking architectural coating:
[0121] 1. Crack resistance test data
[0122] 1) Experimental method: Standard tensile test and bending test are used to test the crack resistance of the coating.
[0123] 2) Test results:
[0124] Traditional coatings:
[0125] Tensile strength: 3.5MPa
[0126] Bending strength: 2.8MPa
[0127] Crack appearance time: 12 months
[0128] The coating of the present invention:
[0129] Tensile strength: 5.2MPa (increased by 48%)
[0130] Bending strength: 4.3MPa (increased by 54%)
[0131] Crack appearance time: more than 24 months (100% improvement)
[0132] 2. Weather resistance test data
[0133] 1) Experimental method: artificial accelerated aging test, including ultraviolet exposure and humidity and heat cycle test.
[0134] 2) Test results:
[0135] Traditional coatings:
[0136] UV exposure: coating fading rate is 40% (2000 hours test)
[0137] Wet heat cycle: coating peeling area is 15% (100 cycles)
[0138] The coating of the present invention:
[0139] UV exposure: coating fade rate is 15% (2000 hours test, reduction of 62%)
[0140] Wet heat cycle: coating peeling area is 5% (100 cycles, reduction of 67%)
[0141] 3. Production process control data
[0142] 1) Grinding time: 2-4 hours
[0143] Traditional process: grinding time is usually 5 hours
[0144] The present invention has a grinding time of 3 hours, a particle size within the range of 70-100 nanometers, and a more uniform particle size compared with the traditional process.
[0145] 2) Homogenization time: 1-2 hours
[0146] Traditional process: homogenization time is 3 hours
[0147] The present invention has a homogenization treatment time of 1.5 hours, and the uniformity and stability of the coating slurry are significantly improved.
[0148] 4. Application effect data
[0149] 1) Building exterior wall application:
[0150] Traditional coatings: Service life is 5 years, regular maintenance is required
[0151] The coating of the present invention has a service life of more than 10 years and a maintenance frequency reduced by 50%.
[0152] 2) Industrial equipment protection:
[0153] Traditional coatings: Equipment surfaces are subject to wear and corrosion every year and require re-coating
[0154] The coating of the present invention: equipment surface wear and corrosion are significantly reduced, and the coating integrity is maintained for more than 2 years
[0155] ##5. User feedback data
[0156] 1) Construction experience:
[0157] Traditional coatings: uneven drying during construction, low construction efficiency
[0158] The coating of the present invention: the construction uniformity is improved, the drying time is reduced by 30%, and the construction efficiency is significantly improved
[0159] 2) Effect evaluation:
[0160] Traditional coatings: user satisfaction is 70%
[0161] The coating of the present invention: user satisfaction increased to 90%, and users reported that the coating effect was more durable and the maintenance cost was reduced
[0162] VI. Third-party evaluation
[0163] 1) Certification body: Evaluation is conducted by the National Building Materials Testing Center
[0164] 2) Evaluation results:
[0165] Traditional coatings: Failure to fully meet the requirements of high durability and crack resistance
[0166] The coating of the present invention: has passed all standard certifications for high durability and crack resistance, and meets the latest standards in the construction industry
[0167] These data demonstrate the significant technical progress of the present invention in terms of crack resistance, weather resistance, production efficiency, application effect and user satisfaction. Through specific figures and comparisons, the advantages of the present invention in improving coating performance and construction efficiency are demonstrated.
[0168] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Any modifications, equivalent substitutions and improvements made by any technician familiar with the technical field within the technical scope disclosed by the present invention and within the spirit and principle of the present invention should be covered by the protection scope of the present invention.
Claims
1. A method for preparing a highly durable anti-cracking architectural coating, characterized in that: The following steps are involved: Step 1: prepare base material, anti-cracking reinforcing agent, weather-resistant pigment, filler and other additives; Step 2, mixing the components in a certain proportion and grinding them using a nano-scale sand mill; Step 3, homogenizing the ground coating slurry using a high shear homogenizer; Step 4: Pack the prepared high-durability anti-cracking architectural coating and store it in a dry and cool place.
2. The method for preparing the highly durable anti-cracking architectural coating according to claim 1, characterized in that: The base material is acrylic emulsion, the anti-cracking reinforcing agent is polyvinyl alcohol fiber, the weather-resistant pigment is red iron oxide, and the filler is calcium carbonate.
3. The method for preparing the highly durable crack-resistant architectural coating according to claim 1, characterized in that: The filler may be added with a dispersant, a defoamer, and a leveling agent as required.
4. The method for preparing the highly durable anti-cracking architectural coating according to claim 1, characterized in that: The mixing ratio is: acrylic emulsion accounts for 40-50% of the total weight, polyvinyl alcohol fiber accounts for 1-2% of the total weight, red iron oxide accounts for 5-10% of the total weight, and calcium carbonate accounts for 30-40% of the total weight.
5. The method for preparing the highly durable anti-cracking architectural coating according to claim 1, characterized in that: The grinding time is 2-4 hours, and the particle size after grinding is 50-100 nanometers.
6. The method for preparing the highly durable crack-resistant architectural coating according to claim 1, characterized in that: The homogenization treatment time is 1-2 hours to ensure the uniformity of the coating slurry.
7. A highly durable anti-cracking architectural coating based on the method of claim 1, characterized in that: It contains the following components in weight percentage: acrylic emulsion as a base material, accounting for 40%-50%; polyvinyl alcohol fiber as an anti-cracking reinforcing agent, accounting for 1%-2%; red iron oxide as a weather-resistant pigment, accounting for 5%-10%; and calcium carbonate as a filler, accounting for 30%-40%.
8. The highly durable anti-cracking architectural coating according to claim 7, characterized in that: The method further comprises a step of grinding the mixture using a nano-scale sand mill for 2-4 hours to obtain a particle size within the range of 70-100 nanometers.
9. The highly durable anti-cracking architectural coating according to claim 7, characterized in that It also includes a homogenization step using a high shear homogenizer for 1-2 hours to ensure uniformity and stability of the coating.
10. A method for preparing a highly durable anti-cracking architectural coating based on the method of claim 1, characterized in that: The following steps are involved: Mixing acrylic emulsion, polyvinyl alcohol fiber, red iron oxide and calcium carbonate according to specific weight percentages; The mixture is ground using a nano-sand mill to obtain a specific particle size; And use a high shear homogenizer to homogenize the ground mixture to obtain a uniform and stable coating product.
Citation Information
Patent Citations
Anti-crack building paint and preparation method thereof
CN103232778A
High-elastic anti-crack leak repairing coating material and preparation method thereof
CN111944373A
Anti-cracking texture topcoat with long-acting elasticity retention rate and preparation method thereof
CN116814164A
Waterproof coating for prefabricated building and preparation method of waterproof coating
CN118048087A
Coating material for preventing cracking
JP2003119418A