Composite phase change material with high heat storage density and preparation method thereof

By mixing and processing oxalic acid dihydrate, organic acid, magnesium sulfate heptahydrate, and alkyl alcohol amide phosphate in a specific ratio, a high heat storage density composite phase change material is prepared, which solves the problems of flammability, high cost and high cost of existing materials. To solve the problem of high corrosiveness, environmental temperature control suitable for electronic components is achieved.

CN118792015APending Publication Date: 2024-10-18ANHUI UNIVERSITY OF TECHNOLOGY
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410802051.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-20
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

Existing environmental temperature control materials such as high-purity paraffin are flammable and costly. The melting point of dihydrate oxalic acid phase change material does not meet the requirements and is highly corrosive to container materials. It cannot be effectively used for temperature control of electronic components.

Method used

By mixing oxalic acid dihydrate, organic acid, magnesium sulfate heptahydrate, and alkyl alcohol amide phosphate in a specific ratio, and subjecting it to sealing insulation and constant temperature magnetic stirring, a high heat storage density composite phase change material is prepared. Its melting point is adjusted and Reduce corrosivity.

Benefits of technology

The prepared composite phase change material has significantly improved heat storage density, reduced cost, no self-ignition and low corrosion, and is suitable for environmental temperature management of electronic equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118792015A_ABST
    Figure CN118792015A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of environment temperature control materials, and particularly relates to a high-heat-storage-density composite phase change material and a preparation method thereof.The preparation method comprises the following steps that 1, oxalic acid dihydrate, organic acid, magnesium sulfate heptahydrate and alkylolamide phosphate are evenly mixed according to the proportion under the stirring condition, and a mixture A is obtained; 2) sealing and preserving heat of the mixture A for a certain time, and magnetically stirring for a certain time at constant temperature to obtain a mixture B; and 3) naturally cooling the mixture B to room temperature and solidifying to obtain the high-heat-storage-density composite phase change material. The prepared composite phase change material is high in volume heat storage density, the melting temperature ranges from 65 DEG C to 75 DEG C, meanwhile, the composite phase change material has the advantages of being good in heat cycle performance, low in flammability and low in corrosivity, and can be applied to environment temperature management during instantaneous heat release of electronic equipment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of environmental temperature control materials, and in particular relates to a high heat storage density composite phase change material and a preparation method thereof. Background Art

[0002] Many precision electronic components (such as 5G equipment, radar, etc.) generate a lot of heat when working, which increases the ambient temperature. When the ambient temperature is higher than the working temperature required by the working system, the equipment efficiency and life will decrease, or even be damaged. To address this problem, the current main solution is to use phase change materials with suitable phase change temperatures to fit or wrap the electronic components, and absorb the generated heat through phase change so that the ambient temperature is controlled within the device operating temperature range to achieve ambient temperature management. Phase change energy storage materials have the characteristic of little temperature change when absorbing heat at the phase change temperature, so they can be used to absorb the heat released by the system and keep the ambient temperature relatively stable for a certain period of time, so as to achieve the purpose of regulating and controlling the ambient temperature of the phase change material. It is a good ambient temperature control material. Phase change materials used for temperature control of electronic components generally require a phase change temperature of 65-75°C, and the larger the latent heat of phase change, the better. At present, the material commonly used for ambient temperature thermal management is high-purity paraffin with a carbon chain length greater than 32, and its melting latent heat value is 200-240J / g, but it has the disadvantages of being flammable and high cost. In addition, most phase change materials currently on the market cannot meet the needs of ambient temperature control.

[0003] Oxalic acid dihydrate has the advantages of ultra-high phase change latent heat (364J / g) and being relatively cheap and readily available compared to high-purity paraffin; however, when used for ambient temperature control, it also has disadvantages such as high phase change temperature (99°C) and high corrosiveness, so it cannot be directly used for ambient temperature control of electronic components. At present, there are relatively few studies on dihydrate oxalic acid-based composite materials at home and abroad: South China University of Technology obtained a composite phase change material with a phase change temperature of 56.13°C and a phase change latent heat of 246.9 J / g by compounding dihydrate oxalic acid and ammonium aluminum sulfate dodecahydrate (Wang Kai, Preparation and Properties of Dihydrate Oxalic Acid-Ammonium Alum Eutectic / Zirconium Oxide Modified Expanded Graphite Composite Phase Change Materials, Master's Thesis of South China University of Technology, 2021); Qinghai Institute of Salt Lakes, Chinese Academy of Sciences obtained a composite phase change material with a phase change temperature of 88.7°C and a phase change latent heat of 328.2 J / g by compounding dihydrate oxalic acid and sodium chloride (Han Lipeng, Research on the Tolerance of Dihydrate Oxalic Acid Phase Change Energy Storage Materials, Master's Thesis of Qinghai Institute of Salt Lakes, Chinese Academy of Sciences, 2019). There are also literature reports that the combination of oxalic acid dihydrate and borax can produce a phase change material with a phase change temperature of 87.3°C and a phase change latent heat of 344 J / g (Renewable Energy, 2019, (136): 657-663).

[0004] Although the above studies lowered the phase change temperature by combining oxalic acid dihydrate and soluble inorganic salts to form a eutectic or eutectic mixture, the melting temperature did not fall within the commonly used ambient temperature range of electronic components. In addition, the addition of inorganic salts increased the ionic conductivity of the phase change material when it melted, further increasing the electrochemical corrosion of the metal. Summary of the invention

[0005] In view of the shortcomings of phase change materials in the current environmental temperature control field, such as high-purity paraffin is flammable and costly; the melting point of existing dihydrate oxalic acid phase change materials does not meet the requirements of environmental temperature control and is highly corrosive to container materials, the present invention provides a high heat storage density composite phase change material and a preparation method thereof. The prepared composite phase change material is more suitable for application in the field of electronic component temperature control.

[0006] In order to achieve the above technical objectives and the above technical effects, the present invention is implemented through the following technical solutions:

[0007] The present invention provides a method for preparing a high heat storage density composite phase change material, comprising the following steps:

[0008] 1) under stirring conditions, oxalic acid dihydrate, organic acid, magnesium sulfate heptahydrate, and alkyl alcohol amide phosphate are uniformly mixed according to a proportion to obtain a mixture A;

[0009] 2) sealing and keeping the mixture A warm for a certain period of time, and then stirring the mixture with a constant temperature magnetic force for a certain period of time to obtain a mixture B;

[0010] 3) The mixture B is naturally cooled to room temperature and solidified to obtain a high heat storage density composite phase change material.

[0011] Furthermore, in step 1), the mass ratio of oxalic acid dihydrate, organic acid, magnesium sulfate heptahydrate, and alkyl alcohol amide phosphate is 40:60:1:0.05-0.4.

[0012] Furthermore, in step 1), the mass ratio of oxalic acid dihydrate, organic acid, magnesium sulfate heptahydrate, and alkyl alcohol amide phosphate is 40:60:1:0.1.

[0013] Furthermore, in step 1), the organic acid is glutaric acid.

[0014] Furthermore, in step 2), the sealing and heat preservation temperature is controlled at 95-105° C., and the heat preservation time is controlled at 2.5-3.5 h.

[0015] Furthermore, in step 2), the sealing and heat preservation temperature is controlled at 100° C., and the heat preservation time is controlled at 3 hours.

[0016] Furthermore, in step 2), the temperature of the constant temperature magnetic stirring is 100° C., and the time is controlled at 20 to 30 minutes.

[0017] Furthermore, in step 2), the temperature of the constant temperature magnetic stirring is 100° C., and the time is controlled at 25 min.

[0018] The present invention also provides a high heat storage density composite phase change material obtained by the above-mentioned preparation method.

[0019] The beneficial effects of the present invention are:

[0020] 1. Compared with high-purity paraffin with a melting point in the range of 65-75°C, the composite phase change material obtained in the present invention has a significantly higher heat storage density than paraffin, cannot burn autonomously (paraffin is flammable), and significantly reduces production costs.

[0021] 2. Compared with other disclosed oxalic acid dihydrate composite phase change materials, the composite phase change material obtained in the present invention is not compounded with inorganic salts, but the melting point of oxalic acid dihydrate is adjusted by organic acid, and the hydrolysis behavior of oxalic acid dihydrate when it melts is inhibited by organic acid, and the organic acid works together with alkyl alcohol amide phosphate to further reduce the corrosiveness of the material to metals.

[0022] 3. The composite phase change material obtained by the present invention also has the characteristics of good thermal cycle performance, low flammability and low corrosion, and can be applied to the environmental temperature management of electronic equipment during instantaneous heat release.

[0023] Of course, any product implementing the present invention does not necessarily need to achieve all of the above advantages at the same time. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.

[0025] Figure 1 is a differential scanning calorimetry (DSC) diagram of Example 1;

[0026] Figure 2 is a differential scanning calorimetry (DSC) diagram of Example 2;

[0027] Figure 3 is the differential scanning calorimetry (DSC) diagram of Example 3;

[0028] Figure 4 is a differential scanning calorimetry (DSC) diagram of Example 4;

[0029] Figure 5 is the differential scanning calorimetry (DSC) diagram of Example 5;

[0030] Figure 6 The tafel curves of Example 1 and Comparative Example 1 are shown. DETAILED DESCRIPTION

[0031] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0032] Example 1

[0033] Oxalic acid dihydrate, glutaric acid, magnesium sulfate heptahydrate and alkyl alcohol amide phosphate were uniformly mixed in a mass ratio of 40:60:1:0.05, sealed at 105°C and kept warm for 2.5 hours, and subjected to constant temperature magnetic stirring at 100°C for 20 minutes. The material was naturally cooled to room temperature and solidified to obtain a high heat storage density composite phase change material.

[0034] Example 2

[0035] Oxalic acid dihydrate, glutaric acid, magnesium sulfate heptahydrate and alkyl alcohol amide phosphate were uniformly mixed in a mass ratio of 40:60:1:0.1, sealed at 100°C and kept warm for 3 hours, and subjected to constant temperature magnetic stirring at 100°C for 25 minutes. The mixture was naturally cooled to room temperature and solidified to obtain a high heat storage density composite phase change material.

[0036] Example 3

[0037] Oxalic acid dihydrate, glutaric acid, magnesium sulfate heptahydrate and alkyl alcohol amide phosphate were uniformly mixed in a mass ratio of 40:60:1:0.2, sealed at 100°C and kept warm for 3 hours, and subjected to constant temperature magnetic stirring at 100°C for 25 minutes. The mixture was naturally cooled to room temperature and solidified to obtain a high heat storage density composite phase change material.

[0038] Example 4

[0039] Oxalic acid dihydrate, glutaric acid, magnesium sulfate heptahydrate and alkyl alcohol amide phosphate were uniformly mixed in a mass ratio of 40:60:1:0.3, sealed at 100°C and kept warm for 3 hours, and subjected to constant temperature magnetic stirring at 100°C for 25 minutes. The mixture was naturally cooled to room temperature and solidified to obtain a high heat storage density composite phase change material.

[0040] Example 5

[0041] Oxalic acid dihydrate, glutaric acid, magnesium sulfate heptahydrate and alkyl alcohol amide phosphate were uniformly mixed in a mass ratio of 40:60:1:0.4, sealed at 95°C and kept warm for 3.5 hours, and subjected to constant temperature magnetic stirring at 100°C for 30 minutes. The material was naturally cooled to room temperature and solidified to obtain a high heat storage density composite phase change material.

[0042] Comparative Example 1

[0043] Oxalic acid dihydrate, glutaric acid and magnesium sulfate heptahydrate are uniformly mixed in a mass ratio of 40:60:1, sealed at 100°C and kept warm for 3 hours, subjected to constant temperature magnetic stirring at 100°C for 25 minutes, and naturally cooled to room temperature for solidification to obtain a high heat storage density composite phase change material.

[0044] The thermal property data of Examples 1-5 and the thermal property data after 50 cycles are shown in Table 1 and Table 2 respectively:

[0045] Table 1 Thermal properties data of Examples 1-5

[0046]

[0047]

[0048] Table 2 Thermal properties of Examples 1-5 after 50 thermal cycles

[0049]

[0050] It can be seen from the above two tables that after 50 cycles, the supercooling and latent heat of phase change of Examples 1 to 5 do not change much; considering the volume heat storage density, whether before or after the cycle, the latent heat of phase change with the addition of 0.1% alkyl alcohol amide phosphate is the largest, and the volume heat storage density is also better, so the sample of Example 2 is the best.

[0051] Corrosion test: The samples of Example 2 and Comparative Example 1 were prepared into a 0.5 mol / L aqueous solution, and the electrochemical tafel curve of the solution was tested using an electrochemical workstation. The results are shown in Table 3. The self-corrosion potential of Example 2 is higher than that of Comparative Example 1, the self-corrosion current is lower than that of Comparative Example 1, and the polarization resistance is higher than that of Comparative Example 1. The above results show that the corrosiveness of Example 2 is less than that of Comparative Example 1.

[0052] Table 3 Tafel curve test results of Example 2 and Comparative Example 1

[0053]

[0054] Self-combustion test: Take a certain amount of the sample of Example 2 and wrap it with paper. Light the outer paper with a lighter. After the outer paper burns, observe whether the sample inside can burn autonomously. The results show that the sample of Example 2 does not burn autonomously, indicating that the sample has good flame retardancy.

[0055] The instrument used to measure the phase change temperature and phase change latent heat of the prepared samples is a DSC-500B differential scanning calorimeter produced by Shanghai Yingnuo Precision Instrument Co., Ltd. 10 mg of sample was placed in an aluminum crucible with a lid, and nitrogen was used as the purge gas and protective gas at a flow rate of 20 mL / min; the test temperature range was: room temperature to 100 ° C; under nitrogen atmosphere, the room temperature was raised to 100 ° C, the heating rate was 3 ° C / min, and the cooling rate was -3 ° C / min from 100 ° C to room temperature.

[0056] The instrument used to measure the tafel curves of Example 2 and Comparative Example 1 is the CH1760E electrochemical workstation produced by Shanghai Chenhua Instruments Xi'an Company, the four-electrode method, the reference electrode is a calomel electrode, the test temperature is room temperature, and the scanning rate is 0.01 V / s.

[0057] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A method for preparing a high heat storage density composite phase change material, It is characterized in that The steps include: 1) under stirring conditions, oxalic acid dihydrate, organic acid, magnesium sulfate heptahydrate, and alkyl alcohol amide phosphate are uniformly mixed according to a proportion to obtain a mixture A; 2) sealing and keeping the mixture A warm for a certain period of time, and then stirring the mixture with a constant temperature magnetic force for a certain period of time to obtain a mixture B; 3) The mixture B is naturally cooled to room temperature and solidified to obtain a high heat storage density composite phase change material.

2. The preparation method according to claim 1, It is characterized in that In step 1), the mass ratio of oxalic acid dihydrate, organic acid, magnesium sulfate heptahydrate and alkyl alcohol amide phosphate is 40:60:1:0.05-0.

4.

3. The preparation method according to claim 2, It is characterized in that In step 1), the mass ratio of oxalic acid dihydrate, organic acid, magnesium sulfate heptahydrate and alkyl alcohol amide phosphate is 40:60:1:0.

1.

4. The preparation method according to claim 1, It is characterized in that In step 1), the organic acid is glutaric acid.

5. The preparation method according to claim 1, It is characterized in that In step 2), the sealing and heat preservation temperature is controlled at 95-105° C., and the heat preservation time is controlled at 2.5-3.5 h.

6. The preparation method according to claim 5, It is characterized in that In step 2), the sealing and heat preservation temperature is controlled at 100° C., and the heat preservation time is controlled at 3 h.

7. The preparation method according to claim 1, It is characterized in that In step 2), the temperature of the constant temperature magnetic stirring is 100° C., and the time is controlled at 20 to 30 minutes.

8. The preparation method according to claim 7, It is characterized in that In step 2), the temperature of the constant temperature magnetic stirring is 100° C. and the time is controlled at 25 min.

9. A high heat storage density composite phase change material obtained by the preparation method according to any one of claims 1 to 8.

Citation Information

Cited By

  • High-heat-storage-density phase-change composite material and preparation method therefor

    WO2025260728A1