Glass fiber surface treating agent, preparation method thereof and application of glass fiber surface treating agent in preparation of acid-resistant cloth

By using a combined surface treatment agent of silane coupling agent and lignin black liquor on the glass fiber filter cloth, the problem of insufficient acid resistance of the glass fiber filter material is solved, resource recycling and cost reduction are achieved, and the performance of the acid-resistant cloth is satisfied. Require.

CN118792882APending Publication Date: 2024-10-18CHONGQING YIXUAN NEW MATERIAL TECH CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410858537.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

The existing glass fiber filter material has poor acid resistance, which limits its application range. Moreover, the production cost of existing solutions is high or the process is complex, making it difficult to effectively utilize the waste black liquor from the papermaking industry to reduce environmental protection expenses.

Method used

A glass fiber surface treatment agent including silane coupling agent, PTFE concentrated dispersion, silicone oil, penetrant, emulsifier and lignin black liquor is used to improve the acid resistance of the glass fiber surface through pre-hydrolysis and impregnation processes, and through double Roll extrusion and drying to obtain acid-resistant cloth.

Benefits of technology

It improves the acid resistance of fiberglass filter cloth, realizes resource recycling, reduces production costs, and meets industry standard performance indicators.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118792882A_ABST
    Figure CN118792882A_ABST
Patent Text Reader

Abstract

A glass fiber surface treating agent relates to the technical field of surface treating agents, and comprises 0.1-1% of a silane coupling agent, 10-50% of a PTFE concentrated dispersion liquid, 0.1-0.5% of silicone oil, 0.01-0.1% of a penetrant, 0.01-0.1% of an emulsifier, 0.1-5% of lignin black liquor, and the balance of pure water. The invention also provides a method for preparing the acid-resistant cloth. The method comprises the following steps: S1, preparing the glass fiber surface treating agent according to any one of claims 1-7 in a dipping tank; s2, dewaxing the raw glass cloth; s3, dipping the dewaxed glass raw cloth in the step S2 into the glass fiber surface treating agent prepared in the step S1; and S4, carrying out double-roller extrusion on the glass raw cloth impregnated in the step S3, and then drying to obtain an acid-resistant cloth finished product.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of surface treatment agents, and in particular to a glass fiber surface treatment agent, a preparation method thereof, and application thereof in the preparation of acid-resistant cloth. Background Art

[0002] Bag filter is the mainstream dust removal equipment at present. Its internal filter bag is the key factor affecting dust removal efficiency and operation cost. At present, most filter bags on the market use glass fiber filter cloth as raw material. Glass fiber has the advantages of hydrolysis resistance, high temperature resistance, high strength and small elongation. It has now developed into the main material of high-performance filter material. However, the acid resistance of glass fiber filter material is poor, which limits its application range.

[0003] In order to solve the above problems and expand the application field of glass fiber, in the Chinese patent with publication number CN101857376A, the acid resistance of glass is enhanced by increasing the content of alkali metal oxides, but this method will reduce the tensile strength of glass fiber; and in the two Chinese utility model patents with authorization announcement numbers CN209999804U and CN203829792U, chemical fibers such as polyphenylene sulfide and aramid are respectively used in combination with glass fiber to improve the acid resistance of filter materials. Although there are certain results, the process is too complicated and the production efficiency is too low.

[0004] At present, it seems that covering the outside of the glass fiber with an acid-resistant coating by surface treatment is an effective way to solve the problem of poor acid resistance of the filter material. This method can improve the acid resistance of the filter material while giving the glass fiber a certain mechanical strength. In the Chinese invention patent with publication number CN106076264A, gypsum is added to the glass fiber filter material. Its main component calcium sulfate is a commonly used acid-resistant filler. For example, in the Chinese invention patent with authorization announcement number CN102908828B, calcium carbonate is introduced into the filter material to make up for the lack of acid resistance of PTFE. Although these methods can solve the acid resistance problem, the introduction of new fillers will also lead to increased production costs; and the fillers used in industry are basically some regular chemicals. If a waste with better acid resistance can be found to replace conventional fillers, it will not only bring huge economic benefits to the enterprise, but also realize the recycling of resources and make certain contributions to the development of the green economy.

[0005] Black liquor is the waste liquid of pulp after washing and cooking in the papermaking process. It contains a large amount of lignin and caustic soda. Lignin is the only natural polymer containing benzene rings in nature. It has a complex structure and stable properties. It can only be dissolved in strong alkali and very few organic solvents and has good acid resistance. Every year, the papermaking industry generates a large amount of black liquor. If it is discharged into the river, it is easy to cause environmental pollution. It can only be evaporated and concentrated first, and the obtained lignin will be burned separately. The whole process will consume a lot of manpower and material resources. Moreover, the solid content of black liquor is about 15%, of which about 70% is lignin, and the remaining 30% is sodium hydroxide and sodium salt. It is a natural acid-resistant material. If it can be applied to glass fiber filter cloth, it can not only improve the acid resistance of the filter cloth, but also reduce the environmental protection expenses of processing black liquor, realize resource recycling, and become an example in the sustainable development strategy. Summary of the invention

[0006] In view of the deficiencies in the prior art, the present invention provides a glass fiber surface treatment agent, a preparation method and an application in the preparation of acid-resistant cloth, which solves the problems of high preparation cost of acid-resistant cloth surface treatment agents and how to apply black liquor to the surface treatment agent in the prior art.

[0007] A glass fiber surface treatment agent comprises, by mass fraction, 0.1-1% of a silane coupling agent, 10-50% of a PTFE concentrated dispersion, 0.1-0.5% of silicone oil, 0.01-0.1% of a penetrant, 0.01-0.1% of an emulsifier, 0.1-5% of a lignin black liquor, and the remainder is pure water.

[0008] Preferably, the content of the lignin black liquor is 0.5-3%.

[0009] Preferably, the silane coupling agent is one of KH550, KH560 and KH570.

[0010] Preferably, the silicone oil is methyl silicone oil or amino silicone oil.

[0011] Preferably, the penetrant is one of APE, OEP-70 and OE-35.

[0012] Preferably, the emulsifier is one of AEO-3, OP-10 and PEG200.

[0013] The present invention also provides a method for preparing a glass fiber surface treatment agent, which is characterized by comprising the following steps:

[0014] S1. pre-hydrolyzing the silane coupling agent and filtering the lignin black liquor;

[0015] S2. Take the pre-hydrolyzed silane coupling agent, add part of pure water and PTFE concentrated dispersion, stir evenly, and then add silicone oil, penetrant, emulsifier, lignin black liquor and remaining pure water in sequence.

[0016] The present invention also provides a method for preparing an acid-resistant cloth, comprising the following steps:

[0017] S1. Dewaxing the original glass cloth;

[0018] S2. The dewaxed glass cloth in S1 is immersed in a glass fiber surface treatment agent;

[0019] S3. The glass raw cloth impregnated in S2 is double-rolled and then dried to obtain a finished acid-resistant cloth.

[0020] Preferably, in step S1, the glass cloth is run at a line speed of 1-2 m / s and dewaxed at 300-330° C. for 5-8 min.

[0021] Preferably, in step S3, the gap between the two rollers is 0.4-0.6 mm, the drying temperature is 200-250° C., and the drying time is 5-8 min.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] 1. The present invention provides an acid-resistant glass fiber surface treatment agent. The characteristic of the treatment agent is that lignin black liquor, a waste of the papermaking industry, is introduced as an added component. Since the lignin black liquor contains a large amount of sodium hydroxide and its pH value can reach 10-12, the lignin black liquor can catalyze the hydrolysis of the silicon-oxygen bonds on the surface of the glass fiber during the impregnation process to generate a large amount of hydroxyl groups, which form hydrogen bonds with the hydroxyl groups of the silane coupling agent. In the drying process, further dehydration and condensation are carried out, and finally the silane coupling agent and the glass fiber surface are efficiently bonded, the bonding force between the silane coupling agent and the glass fiber surface is enhanced, the acid-resistant coating is ensured not to fall off easily, and the acid-resistant performance of the acid-resistant cloth is improved, that is, the acid-resistant cloth has good radial strength retention rate and weft strength retention rate.

[0024] 2. The glass fiber surface treatment agent prepared by the present invention uses the waste lignin black liquor of the papermaking industry as filler, which improves the acid resistance of the acid-resistant cloth, realizes the recycling of resources, saves the environmental protection expenses of processing lignin black liquor, and greatly reduces the production cost.

[0025] Other advantages, objectives and features of the present invention will be embodied in part through the following description, and in part will be understood by those skilled in the art through study and practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is a schematic diagram of the reaction principle of adding lignin black liquor in the present invention. DETAILED DESCRIPTION

[0027] In order to make the technical means, creative features, objectives and functions of the present invention clearer and easier to understand, the present invention is further described below in conjunction with the accompanying drawings and specific embodiments:

[0028] Example 1

[0029] S1. First, mix acetic acid and pure water, then slowly pour the mixed acid into KH550 and stir evenly. During this period, filter the lignin black liquor with a 400-mesh filter cloth;

[0030] S2. Take 0.1% of the pre-hydrolyzed KH550 by mass fraction, add 20% of the total amount of pure water to dilute, then add 10% of the PTFE concentrated dispersion, stir evenly, then add 0.1% of methyl silicone oil, 0.01% of APE, 0.01% of AEO-3, 0.5% of lignin black liquor and the remaining pure water in sequence, mix evenly, and obtain a glass fiber surface treatment agent;

[0031] S3. The S-type glass cloth with a width of 1650 mm was run at a line speed of 1 m / s, dewaxed at 300°C for 5 min, and then immersed in the glass fiber surface treatment agent prepared in S2;

[0032] S4. Adjust the double-roll gap to 0.4 mm, squeeze the original glass cloth impregnated in S3 through double rolls, and dry it in an oven at 200°C for 5 minutes to obtain a finished acid-resistant cloth.

[0033] Example 2

[0034] S1. First, acetic acid and pure water were mixed, and then the mixed acid solution was slowly poured into KH560 and stirred evenly. During this period, the lignin black liquor was filtered with a 400-mesh filter cloth;

[0035] S2. Take 1% of the pre-hydrolyzed KH560 by mass fraction, add 20% of the total amount of pure water to dilute, then add 50% of the PTFE concentrated dispersion, stir evenly, then add 0.5% of amino silicone oil, 0.1% of OEP-70, 0.1% of OP-10, 5% of lignin black liquor and the remaining pure water, mix evenly, and obtain a glass fiber surface treatment agent;

[0036] S3. The S-type glass cloth with a width of 1650 mm was run at a line speed of 1.5 m / s, dewaxed at 315°C for 6 min, and then immersed in the glass fiber surface treatment agent prepared in S2;

[0037] S4. Adjust the double-roll gap to 0.6 mm, squeeze the original glass cloth impregnated in S3 through double rolls, and dry it in an oven at 250°C for 8 minutes to obtain a finished acid-resistant cloth.

[0038] Example 3

[0039] S1. First, acetic acid and pure water were mixed, and then the mixed acid solution was slowly poured into KH570 and stirred evenly. During this period, the lignin black liquor was filtered with a 400-mesh filter cloth;

[0040] S2. Take 0.6% of the pre-hydrolyzed KH570 by mass fraction, add 20% of the total amount of pure water to dilute the pure water, then add 25% of the PTFE concentrated dispersion, stir evenly, then add 0.3% of amino silicone oil, 0.06% of OE-35, 0.05% of PEG200, 3% of lignin black liquor and the remaining pure water in sequence, mix evenly, and obtain a glass fiber surface treatment agent;

[0041] S3. The S-type glass cloth with a width of 1650 mm was run at a line speed of 2 m / s, dewaxed at 330°C for 8 min, and then immersed in the glass fiber surface treatment agent prepared in S2;

[0042] S4. Adjust the double-roll gap to 0.5 mm, squeeze the original glass cloth impregnated in S3 through double rolls, and then dry it in an oven at 225°C for 7 minutes to obtain a finished acid-resistant cloth.

[0043] Example 4

[0044] S1. First, mix acetic acid and pure water, then slowly pour the mixed acid into KH550 and stir evenly. During this period, filter the lignin black liquor with a 400-mesh filter cloth;

[0045] S2. Take 0.3% of the pre-hydrolyzed KH550 by mass fraction, add 20% of the total amount of pure water to dilute, then add 30% of the PTFE concentrated dispersion, stir evenly, then add 0.2% of methyl silicone oil, 0.04% of APE, 0.07% of PEG200, 0.1% of lignin black liquor and the remaining pure water in sequence, mix evenly, and obtain a glass fiber surface treatment agent;

[0046] S3. The S-type glass cloth with a width of 1650 mm was run at a line speed of 1 m / s, dewaxed at 330°C for 5 min, and then immersed in the glass fiber surface treatment agent prepared in S2;

[0047] S4. Adjust the double-roll gap to 0.6 mm, squeeze the original glass cloth impregnated in S3 through double rolls, and dry it in an oven at 200°C for 5 minutes to obtain a finished acid-resistant cloth.

[0048] Comparative Example 1

[0049] Compared with Example 1, in step S2, no 0.5% lignin black liquor is added, and pure water of equal mass is added, and other conditions are the same.

[0050] Comparative Example 2

[0051] Compared with Example 2, the black liquor in step S1 is not filtered, and the other conditions are the same.

[0052] Comparative Example 3

[0053] Compared with Example 3, in step S2, KH570, PTFE concentrated dispersion, amino silicone oil, OE-35, PEG200, lignin black liquor and pure water are added at the same time, and the other conditions are the same.

[0054] Comparative Example 4

[0055] Compared with Example 3, before preparing the glass fiber surface treatment agent, the pH of the lignin black liquor was adjusted to 7 with acetic acid, and the other conditions were the same.

[0056] Comparative Example 5

[0057] Compared with Example 3, the distance between the two rollers in step S4 is 0.35 mm, and the other conditions are the same.

[0058] Comparative Example 6

[0059] Compared with Example 3, the distance between the two rollers in step S4 is 0.65 mm, and the other conditions are the same.

[0060] In the above embodiments and comparative examples, KH550 is γ-aminopropyltriethoxysilane; KH560 is γ-glycidyloxypropyltrimethoxysilane; KH570 is γ-methacryloxypropyltrimethoxysilane; APE is polyoxyethylene lauryl ether potassium salt; OEP-70 is isooctyl alcohol polyoxyethylene ether potassium salt; OE-35 is isooctyl alcohol polyoxyethylene ether; AEO-3 is fatty alcohol polyoxyethylene ether; OP-10 is alkylphenol polyoxyethylene ether; PEG200 is polyethylene glycol.

[0061] In the above embodiment, when the silane coupling agent is pre-hydrolyzed, the addition of acetic acid can control the hydrolysis rate. Moreover, direct hydrolysis of the silane coupling agent will produce turbidity, and the addition of acetic acid can effectively inhibit the occurrence of this situation.

[0062] The above embodiments and comparative examples were tested as follows:

[0063] Weight test: GB / T 9914.3 (ISO 3374);

[0064] Stiffness test: ASTM D4032-08 (2012);

[0065] Oil content test: GB / T 9914.2 (ISO 1887);

[0066] Tensile strength test: GB / T 7689.5 (ISO 4606);

[0067] Acid resistance test: GB / T 6719-2009;

[0068] Aging resistance test: Place the acid-resistant cloth in a 200℃ oven for 30 days to test the retention rate of warp and weft tensile strength.

[0069] The above test results are shown in Table 1:

[0070]

[0071]

[0072] Table 1 Acid-resistant cloth performance test results

[0073] This industry requires the product weight to be between 760-820g / m 2 , stiffness is less than 11, oil content is between 9%-13%, tensile strength retention rate after acid treatment is greater than 95%, and aging resistance is higher than 80%.

[0074] It can be seen from Table 1 that after using lignin black liquor in Examples 1-4, the performance of the acid-resistant cloth prepared therefrom perfectly meets the industry standards.

[0075] Compared with Example 1, Comparative Example 1 does not use lignin black liquor. The radial strength retention rate and the weft strength retention rate of the acid-resistant cloth prepared by Comparative Example 1 cannot meet the industry standard and are quite different, indicating that its acid resistance is poor.

[0076] In Comparative Example 2, although its performance meets the industry standards, the use of unfiltered lignin black liquor will cause impurities in the lignin black liquor to remain on the acid-resistant cloth, forming black spots and affecting the appearance of the acid-resistant cloth.

[0077] Compared with the acid-resistant cloth prepared by the feeding method of Comparative Example 3, the radial strength retention rate, weft strength retention rate and aging resistance of the acid-resistant cloth of Comparative Example 3 do not meet the industry standards, and are far different from the performance of the acid-resistant cloth of Example 3. This is because the feeding method of Example 3 can effectively and stably combine the silane coupling agent with the PTFE concentrated dispersion.

[0078] For Comparative Example 4, after the pH value of the lignin black liquor was adjusted to 7, the sodium hydroxide in the lignin black liquor was neutralized in large quantities, resulting in the inability to completely catalyze the hydrolysis of the silicon-oxygen bonds on the surface of the glass fiber, and unable to generate a large number of hydroxyl groups to form hydrogen bonds with the hydroxyl groups of the silane coupling agent, thereby affecting the adhesion of the silane coupling agent to the glass fiber surface, reducing the acid resistance, and making the radial strength retention rate, weft strength retention rate and aging resistance performance all fail to meet industry standards.

[0079] For comparative example 5, the distance between the two rollers is too small, resulting in excessive squeezing of the original glass cloth, so that the gram weight, radial strength retention rate, weft strength retention rate and aging resistance of the acid-resistant cloth do not meet the industry standards.

[0080] As for Comparative Example 6, the distance between the two rollers is too large, so that the glass cloth cannot be fully squeezed, and the weight, stiffness and oil content of the acid-resistant cloth do not meet the industry standards.

[0081] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.

Claims

1. A glass fiber surface treatment agent, characterized in that: Calculated by mass fraction, the invention comprises 0.1-1% of silane coupling agent, 10-50% of PTFE concentrated dispersion, 0.1-0.5% of silicone oil, 0.01-0.1% of penetrant, 0.01-0.1% of emulsifier and 0.1-5% of lignin black liquor, and the balance is pure water.

2. A glass fiber surface treatment agent according to claim 1, characterized in that: The content of the lignin black liquor is 0.5-3%.

3. A glass fiber surface treatment agent according to claim 1, characterized in that: The silane coupling agent is one of KH550, KH560 and KH570.

4. A glass fiber surface treatment agent according to claim 1, characterized in that: The silicone oil is methyl silicone oil or amino silicone oil.

5. A glass fiber surface treatment agent according to claim 1, characterized in that: The penetrant is one of APE, OEP-70 and OE-35.

6. A glass fiber surface treatment agent according to claim 1, characterized in that: The emulsifier is one of AEO-3, OP-10 and PEG200.

7. A method for preparing a glass fiber surface treatment agent according to any one of claims 1 to 6, characterized in that: The following steps are involved: S1. pre-hydrolyzing the silane coupling agent and filtering the lignin black liquor; S2. Take the pre-hydrolyzed silane coupling agent, add part of pure water and PTFE concentrated dispersion, stir evenly, and then add silicone oil, penetrant, emulsifier, lignin black liquor and remaining pure water in sequence.

8. A method for preparing acid-resistant cloth, characterized in that: The following steps are involved: S1. Dewaxing the original glass cloth; S2. The dewaxed glass cloth in S1 is immersed in the glass fiber surface treatment agent according to any one of claims 1 to 6; S3. The glass raw cloth impregnated in S2 is double-rolled and then dried to obtain a finished acid-resistant cloth.

9. A method for preparing acid-resistant cloth according to claim 8, characterized in that: In step S1, the glass cloth is run at a line speed of 1-2 m / s and dewaxed at 300-330° C. for 5-8 min.

10. A method for preparing acid-resistant cloth according to claim 8, characterized in that: In step S3, the gap between the two rollers is 0.4-0.6 mm, the drying temperature is 200-250° C., and the drying time is 5-8 min.

Citation Information

Patent Citations

  • Acidproof glass fiber and preparation method thereof

    CN101857376A

  • Glass-fluorine composite filtering material with skin core structure and preparation method and application of glass-fluorine composite filtering material

    CN102908828B

  • Formula of anti-corrosion filter material

    CN106076264A

  • Aramid compound filter material

    CN203829792U

  • Composite filter material

    CN209999804U