Underground bottom plate waterproof construction method
Through the combination of pre-sprayed anti-adhesive waterproofing coating and double-layer composite non-asphalt-based polymer waterproofing membrane, the problem that single-layer polymer pre-paved waterproofing membrane cannot meet the first-level waterproofing is solved, and strong bonding force and full-scale waterproofing are achieved. The interface is sealed and waterproof to avoid water channeling and leakage, improving the reliability of the underground floor waterproofing system.
Patent Information
- Application Number
- CN202411067922.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-10-18
AI Technical Summary
Among the existing underground floor waterproofing construction methods, a single course of polymer pre-paved waterproofing membrane cannot meet the basic requirements of first-level waterproofing. Common practices have compatibility issues with different types of materials, which can easily lead to hidden dangers of water channeling, and are easy to break after bonding. Cracks, hollows, or falls may occur, resulting in reduced waterproofing or water leakage.
Using a combination method of pre-sprayed anti-adhesive waterproof coating and double-layer composite non-asphalt-based polymer waterproofing membrane, the pre-sprayed anti-adhesive waterproof coating is sprayed on the specially treated surface of the upper main material layer, combined with the pressure of post-poured concrete. It forms a strong bonding force, avoids overlapping seams, and builds a full-interface sealed waterproof structure.
It effectively improves the peeling strength with post-cast concrete, prevents water from channeling, and forms a "skin-type" overall waterproofing, completely eliminating hidden dangers of leakage caused by overlapping joints, and improving the reliability of the underground floor waterproofing system.
Smart Images

Figure BDA0004979889460000131
Abstract
Description
Technical Field
[0001] The invention relates to an underground floor waterproofing construction method and belongs to the field of building waterproofing. Technical Background
[0002] The underground project pre-laid reverse-adhesive waterproofing technology, as a promotion technology of the Ministry of Housing and Urban-Rural Development's "10 New Technologies in the Construction Industry (2017 Edition)", was once a highly respected underground project bottom slab waterproofing method in the industry. However, with the release and implementation of the "General Specifications for Waterproofing of Buildings and Municipal Engineering", it has clearly required no less than two waterproof layers for the main structure waterproofing layer of the first-level underground project. A single layer of polymer pre-laid waterproofing membrane can no longer meet the basic requirements of the first-level waterproofing defense, and it needs to be used in combination with other waterproof materials, mostly with a single or multiple waterproof layers set under the polymer pre-laid waterproofing membrane. At present, the common practice in the industry is to design self-adhesive membranes or coatings under the pre-laid waterproof membranes, and adopt ① bonding the asphalt adhesive layer to the lower layer of the pre-laid polymer waterproof membrane, or ② directly laying the I and II courses in the air, or ③ applying the coating on the cushion layer before laying the pre-laid waterproof membrane. The above schemes have compatibility with different types of materials. There is a hidden danger of water leakage when laying the I and II courses in the air. When the I course is bonded to the cushion layer, the cushion layer is prone to cracking, hollowing, falling, etc., which leads to reduced waterproof effect and even water leakage. The above schemes cannot form effective bonding and are prone to forming a water storage layer, which seriously affects the waterproof quality. Based on the above problems, it is necessary to propose effective improvement measures from the aspects of product structure design, the composition of waterproof materials, and existing problems. It is urgent to develop a waterproof construction method suitable for underground floors.
[0003] CN2023208575463 discloses a waterproof structure for a basement, wherein the base plate includes a cushion layer, a second waterproof layer, a second pre-laid reverse-adhesive polymer waterproofing membrane structure layer and a base plate structure layer laid from bottom to top. The second waterproof layer is any one or two of asphalt membrane, waterproof membrane and waterproof coating; the second pre-laid reverse-adhesive polymer waterproofing membrane structure layer is any one of self-adhesive pre-laid reverse-adhesive polymer waterproofing membrane or backing pre-laid reverse-adhesive polymer waterproofing membrane. The above scheme still has the compatibility of different types of materials between course I and course II; there is a hidden danger of water leakage when course I and course II are laid empty; course I is bonded to the cushion layer, and the cushion layer is prone to cracking, hollowing, falling, etc., resulting in reduced waterproofing effect or even water leakage. Therefore, it is of great practical significance to develop a special underground floor waterproofing construction method for the specific application scenarios of underground engineering floors. Summary of the invention
[0004] The purpose of the present invention is to solve the common problems recorded in the technical background part, and to provide a method for underground floor waterproofing construction. The present invention is achieved through the following technical means: First, make full use of the "pre-spraying reverse-adhesion" technology, and upgrade the current common practice to a pre-spraying reverse-adhesion waterproof coating composite double-layer composite non-asphalt-based polymer waterproofing membrane method, that is, first lay the double-layer composite non-asphalt-based polymer waterproofing membrane on the cushion layer, and then spray the pre-spraying reverse-adhesion waterproof coating on the surface of the specially treated upper main material layer, and then pour the concrete to fully adhere to the pre-spraying reverse-adhesion waterproof coating, avoiding the above-mentioned problems in the technical background; second, the multiple hydroxyl and ester groups on the polymer structure can be fully close to the concrete slurry under pressure to form a strong bond force, It can effectively improve the peeling strength with the post-poured concrete, and the introduced silaneoxy group is reactive to inorganic matter. The silane coupling agent is between the inorganic and organic interfaces, and can form a bonding layer of organic matrix-silane coupling agent-inorganic matrix, which helps to improve the peeling strength with the post-poured concrete, form full adhesion, and prevent water leakage; thirdly, the coating-roll composite waterproof system structure has no overlap with the pre-sprayed anti-adhesive waterproof layer that is fully adhered to the post-poured concrete, forming a "skin-type" overall waterproof, completely eliminating the leakage risk caused by overlaps, forming a full-interface closed waterproof structure, and improving the reliability of the underground floor waterproofing system.
[0005] In order to achieve the above object, the technical solution adopted by the present invention is:
[0006] A method for underground floor waterproofing construction, characterized in that the overall waterproofing system structure is as follows from bottom to top: 1) directly laying a double-layer composite non-asphalt-based polymer waterproofing coiled material on the cushion layer, the coiled material is bonded by the adhesive layer with the corona-treated surface facing upward; 2) spraying construction pre-sprays an anti-adhesive waterproof coating, which undergoes water volatilization and photocatalytic curing. The curing takes 12 to 24 hours, and the specific curing time can be appropriately extended according to the weather. The coating is firmly bonded to the HDPE sheet treated with corona to form a continuous, uniform and non-lapping waterproof coating; 3) directly pouring concrete after the structural reinforcement is applied on the waterproof coating. Under the action of pressure, the concrete slurry can form full adhesion with the post-cast concrete through creep, coupling, chelation and the like, thereby achieving an excellent pre-paving anti-adhesive effect of waterproofing and preventing water from flowing through. The pre-sprayed anti-stick waterproof coating is composed of the following raw materials in parts by weight: 45-65 parts of polymer emulsion, 20-25 parts of modified filler, 5-10 parts of water, 5-10 parts of flame retardant, 1-5 parts of flame retardant synergist, 0.3-0.6 parts of dispersant, 0.6-0.8 parts of defoamer, 0.2-0.5 parts of photoinitiator, 0.5-1.0 parts of silane coupling agent, and 0.2-0.6 parts of thickener; the double-layer composite The preparation method of non-asphalt-based polymer waterproofing membrane comprises the following steps: S1, forming a 0.9-1.0 mm modified and toughened HDPE composite polymer layer on the lower main material layer; S2, evenly coating the surface of the composite polymer layer with a hot-melt pressure-sensitive adhesive after melting, with a coating thickness of 0.2-0.4 mm, leaving an overlap width of 90-120 mm on one side of the membrane width, and covering with an isolation edge film; S3, covering the adhesive film with a 0.4-0.5 mm thick HDPE sheet layer treated with corona; S4, rolling and packaging the double-layer composite non-asphalt-based polymer waterproofing membrane.
[0007] Preferably, the double-layer composite non-asphalt-based polymer waterproofing membrane comprises a lower main material layer, a glue layer, and an upper main material layer. The lower main material layer is a 0.9-1.0 mm HDPE composite polymer layer that has been modified and toughened; the glue layer is a hot-melt pressure-sensitive glue layer; and the upper main material layer is a 0.4-0.5 mm HDPE sheet layer with a specially treated upper surface.
[0008] Preferably, the special treatment on the upper surface of the upper main material layer is corona treatment.
[0009] Preferably, the polymer emulsion is at least one of acrylic emulsion, polyurethane emulsion and polyurethane acrylate composite emulsion, and the polymer emulsion has a solid content of 40 to 50%, a glass transition temperature of -40 to -45°C, and a branching degree of 0.70 to 0.85.
[0010] Preferably, the hot-melt pressure-sensitive adhesive is evenly coated on the surface of the composite polymer layer after being melted, and the coating thickness is 0.2 to 0.4 mm.
[0011] Preferably, the double-layer composite non-asphalt-based polymer waterproofing membrane has a reserved overlap width of 90 to 120 mm and is covered with an isolation edge membrane.
[0012] Compared with the prior art, the present invention has the following advantages:
[0013] In view of the above-mentioned problems existing in underground floor waterproofing, the present invention provides a practical underground floor waterproofing system structure: first, the "pre-spraying reverse-adhesion" technology is fully utilized to upgrade the current common practice to a pre-spraying reverse-adhesion waterproof coating composite double-layer composite non-asphalt-based polymer waterproofing membrane practice, that is, firstly, the double-layer composite non-asphalt-based polymer waterproofing membrane is laid on the cushion layer, and then the pre-spraying reverse-adhesion waterproof coating is sprayed on the surface of the upper main material layer that has been specially treated, and then the poured concrete is fully adhered to the pre-spraying reverse-adhesion waterproof coating, thereby avoiding the above-mentioned problems in the technical background; second, the polyhydroxyl and ester groups on the polymer structure can be fully bonded with the concrete slurry under pressure. Close to each other, forming a strong bond cooperation force, effectively improving the peeling strength with the post-cast concrete, and the introduced silane oxy group is reactive to inorganic matter. The silane coupling agent is between the inorganic and organic interfaces, and can form a bonding layer of organic matrix-silane coupling agent-inorganic matrix, which helps to improve the peeling strength with the post-cast concrete, form full adhesion, and prevent water leakage; thirdly, the coating-roll composite waterproof system structure has no overlap with the pre-sprayed anti-adhesive waterproof layer that is fully adhered to the post-cast concrete, forming a "skin-type" overall waterproof, which completely eliminates the leakage risks caused by overlaps, forms a full-interface closed waterproof structure, and improves the reliability of the underground floor waterproofing system.
[0014] In summary, the underground floor waterproofing construction method of the present invention makes full use of the characteristics of the pre-sprayed anti-adhesive waterproof coating, and preferably forms an underground floor coating-roll composite waterproofing system. The pre-sprayed anti-adhesive waterproof coating can be well bonded to the double-layer polymer waterproof roll and is flame retardant, thereby preventing welding slag from damaging the waterproof coating. It also has high peeling strength with the post-poured concrete and can form full adhesion with the structural waterproof concrete, thereby achieving excellent pre-sprayed anti-adhesive effects of waterproofing and water leakage prevention, and meeting the requirements of strong regulations in the waterproofing field. DETAILED DESCRIPTION
[0015] The following examples are used to illustrate the present invention so that those skilled in the art can reproduce the experimental results by referring to the description, but are not intended to limit the scope of the present invention.
[0016] Embodiment 1:
[0017] A method for waterproofing an underground floor, comprising a pre-sprayed anti-adhesive waterproof coating and a double-layer composite non-asphalt-based polymer waterproofing coiled material, wherein the components of the coating are formulated by weight as follows: 5 parts of water, 0.3 parts of dispersant GAXSN G5106, 0.6 parts of defoamer GAXSN G900, 22.5 parts of acrylic emulsion, 20 parts of surface-treated 800-mesh wollastonite powder, 5 parts of flame retardant diphenyl cresyl phosphate, 1 part of flame retardant synergist ultrafine zinc borate, 22.5 parts of acrylic emulsion, 0.2 parts of photosensitive initiator Irgacure-1700, 0.5 parts of silane coupling agent KH560, and 0.2 parts of polyurethane thickener GAXSN G400.
[0018] The acrylic emulsion has a solid content of 50%, a glass transition temperature of -40°C, and a branching degree of 0.85.
[0019] Preparation method of pre-spray anti-stick waterproof coating: weigh water, 1 / 2 acrylic emulsion, dispersant, and defoamer in parts by weight, add them into the barrel, and start stirring; after uniform dispersion, increase the stirring rate, add modified filler, flame retardant, and flame retardant synergist, and stir until uniform; slowly add the remaining acrylic emulsion, photosensitive initiator, and silane coupling agent, stir evenly, then add polyurethane thickener, continue stirring evenly, and filter the material to obtain;
[0020] Preparation method of double-layer composite non-asphalt-based polymer waterproofing membrane: firstly, the lower main material layer is formed: a 0.9mm modified and toughened HDPE composite polymer layer; then, the hot-melt pressure-sensitive adhesive is melted and evenly coated on the surface of the composite polymer layer, with a coating thickness of 0.4mm, and a lap width of 120mm is reserved on one side of the membrane width, and an isolation edge film is covered; then, a 0.5mm thick HDPE corona-treated sheet layer is covered on the adhesive film; finally, the double-layer composite non-asphalt-based polymer waterproofing membrane is rolled up and packaged;
[0021] The overall waterproof system structure from bottom to top is as follows: 1) Lay a double layer of composite non-asphalt-based polymer waterproof membrane on the cushion layer; 2) Spray a pre-sprayed anti-adhesive waterproof coating on 1), which will evaporate and undergo photocatalytic curing. The curing time takes 12 to 24 hours, and the specific curing time can be appropriately extended according to the weather; 3) Pour concrete after structural reinforcement on the pre-sprayed anti-adhesive waterproof coating. Under the action of pressure, the concrete slurry can form full adhesion with the post-poured concrete through creep, coupling, chelation and other effects, thereby achieving an excellent pre-paved anti-adhesive effect of waterproofing and preventing water seepage.
[0022] Embodiment 2:
[0023] A method for waterproofing an underground floor, comprising a pre-sprayed anti-adhesive waterproof coating and a double-layer composite non-asphalt-based polymer waterproofing coiled material, wherein the weight formula of each component of the coating is as follows: 6 parts of water, 0.5 parts of dispersant GAXSN G5106, 0.8 parts of defoamer GAXSN G900, 27.5 parts of polyurethane emulsion, 24 parts of surface-treated 800-mesh wollastonite powder, 6 parts of flame retardant diphenyl cresyl phosphate, 3 parts of flame retardant synergist ultrafine zinc borate, 27.5 parts of polyurethane emulsion, 0.3 parts of photosensitive initiator Irgacure-1700, 0.8 parts of silane coupling agent KH560, and 0.3 parts of polyurethane thickener GAXSN G400.
[0024] The solid content of the polyurethane emulsion is 45%, the glass transition temperature is -45°C, and the branching degree is 0.80.
[0025] Preparation method of pre-spray anti-stick waterproof coating: weigh water, 1 / 2 polyurethane emulsion, dispersant, and defoamer in parts by weight, add them into the barrel, and start stirring; after uniform dispersion, increase the stirring rate, add modified filler, flame retardant, and flame retardant synergist, and stir until uniform; slowly add the remaining polyurethane emulsion, photosensitive initiator, and silane coupling agent, stir evenly, then add polyurethane thickener, continue stirring evenly, and filter the material to obtain;
[0026] Preparation method of double-layer composite non-asphalt-based polymer waterproofing membrane: firstly, the lower main material layer is formed: a 1.0mm modified and toughened HDPE composite polymer layer; then, the hot-melt pressure-sensitive adhesive is melted and evenly coated on the surface of the composite polymer layer, with a coating thickness of 0.4mm, and a lap width of 110mm is reserved on one side of the width of the membrane, and an isolation edge film is covered; then, a 0.4mm thick HDPE corona-treated sheet layer is covered on the adhesive film; finally, the double-layer composite non-asphalt-based polymer waterproofing membrane is rolled up and packaged;
[0027] The overall waterproof system structure from bottom to top is as follows: 1) Lay a double layer of composite non-asphalt-based polymer waterproof membrane on the cushion layer; 2) Spray a pre-sprayed anti-adhesive waterproof coating on 1), which will evaporate and undergo photocatalytic curing. The curing time takes 12 to 24 hours, and the specific curing time can be appropriately extended according to the weather; 3) Pour concrete after structural reinforcement on the pre-sprayed anti-adhesive waterproof coating. Under the action of pressure, the concrete slurry can form full adhesion with the post-poured concrete through creep, coupling, chelation and other effects, thereby achieving an excellent pre-paved anti-adhesive effect of waterproofing and preventing water seepage.
[0028] Embodiment 3:
[0029] A method for waterproofing an underground floor, comprising a pre-sprayed anti-adhesive waterproof coating and a double-layer composite non-asphalt-based polymer waterproofing coiled material, wherein the components of the coating are formulated by weight as follows: 8 parts of water, 0.4 parts of dispersant GAXSN G5106, 0.7 parts of defoamer GAXSN G900, 32.5 parts of polyurethane acrylate composite emulsion, 25 parts of surface-treated 800-mesh wollastonite powder, 8 parts of flame retardant diphenyl cresyl phosphate, 4 parts of flame retardant synergist ultrafine zinc borate, 32.5 parts of polyurethane acrylate composite emulsion, 0.5 parts of photosensitive initiator Irgacure-1700, 1.0 parts of silane coupling agent KH560, and 0.5 parts of polyurethane thickener GAXSN G400.
[0030] The polyurethane acrylate composite emulsion has a solid content of 40%, a glass transition temperature of -40°C, and a branching degree of 0.70.
[0031] Preparation method of pre-spray anti-stick waterproof coating: weigh water, 1 / 2 polyurethane acrylate composite emulsion, dispersant, and defoamer in parts by weight, add them into the barrel, and start stirring; after uniform dispersion, increase the stirring rate, add modified filler, flame retardant, and flame retardant synergist, and stir until uniform; slowly add the remaining polyurethane acrylate composite emulsion, photosensitive initiator, and silane coupling agent, stir evenly, then add polyurethane thickener, continue to stir evenly, and filter the material to obtain;
[0032] Preparation method of double-layer composite non-asphalt-based polymer waterproofing membrane: firstly, the lower main material layer is formed: a 0.9mm modified and toughened HDPE composite polymer layer; then, the hot-melt pressure-sensitive adhesive is melted and evenly coated on the surface of the composite polymer layer, with a coating thickness of 0.3mm, and a lap width of 90mm is reserved on one side of the membrane width, and an isolation edge film is covered; then, a 0.4mm thick HDPE corona-treated sheet layer is covered on the adhesive film; finally, the double-layer composite non-asphalt-based polymer waterproofing membrane is rolled up and packaged;
[0033] The overall waterproof system structure from bottom to top is as follows: 1) Lay a double layer of composite non-asphalt-based polymer waterproof membrane on the cushion layer; 2) Spray a pre-sprayed anti-adhesive waterproof coating on 1), which will evaporate and undergo photocatalytic curing. The curing time takes 12 to 24 hours, and the specific curing time can be appropriately extended according to the weather; 3) Pour concrete after structural reinforcement on the pre-sprayed anti-adhesive waterproof coating. Under the action of pressure, the concrete slurry can form full adhesion with the post-poured concrete through creep, coupling, chelation and other effects, thereby achieving an excellent pre-paved anti-adhesive effect of waterproofing and preventing water seepage.
[0034] Embodiment 4:
[0035] A method for waterproofing an underground floor, comprising pre-spraying an anti-adhesive waterproof coating and a double-layer composite non-asphalt-based polymer waterproofing coiled material, wherein the weight formula of each component of the coating is as follows: 10 parts of water, 0.6 parts of dispersant GAXSNG5106, 0.7 parts of defoamer GAXSN G900, 30 parts of polymer emulsion, 22 parts of surface-treated 800-mesh wollastonite powder, 10 parts of flame retardant diphenyl cresyl phosphate, 5 parts of flame retardant synergist ultrafine zinc borate, 30 parts of polymer emulsion, 0.4 parts of photosensitive initiator Irgacure-1700, 0.6 parts of silane coupling agent KH560, and 0.6 parts of polyurethane thickener GAXSN G400.
[0036] The polymer emulsion is an acrylic emulsion with a solid content of 50%, a glass transition temperature of -40°C, and a branching degree of 0.85, and a polyurethane emulsion with a solid content of 45%, a glass transition temperature of -45°C, and a branching degree of 0.80, which are mixed in a mass ratio of 1:2.
[0037] Preparation method of pre-spray anti-stick waterproof coating: weigh water, 1 / 2 polymer emulsion, dispersant, and defoamer in parts by weight, add them into the barrel, and start stirring; after uniform dispersion, increase the stirring rate, add modified filler, flame retardant, and flame retardant synergist, and stir until uniform; slowly add the remaining polymer emulsion, photosensitive initiator, and silane coupling agent, stir evenly, then add polyurethane thickener, continue stirring evenly, and filter the material to obtain;
[0038] Preparation method of double-layer composite non-asphalt-based polymer waterproofing membrane: firstly, form the lower main material layer: 1.0mm modified and toughened HDPE composite polymer layer; then melt the hot-melt pressure-sensitive adhesive and evenly coat it on the surface of the lower main material polymer layer, with a coating thickness of 0.2mm, and reserve a lap width of 110mm on one side of the membrane width, and cover it with an isolation edge film; then cover the adhesive film with a 0.5mm thick HDPE sheet layer treated with corona; finally, roll up the double-layer composite non-asphalt-based polymer waterproofing membrane and package it;
[0039] The overall waterproof system structure from bottom to top is as follows: 1) Lay a double layer of composite non-asphalt-based polymer waterproof membrane on the cushion layer; 2) Spray a pre-sprayed anti-adhesive waterproof coating on 1), which will evaporate and undergo photocatalytic curing. The curing time takes 12 to 24 hours, and the specific curing time can be appropriately extended according to the weather; 3) Pour concrete after structural reinforcement on the pre-sprayed anti-adhesive waterproof coating. Under the action of pressure, the concrete slurry can form full adhesion with the post-poured concrete through creep, coupling, chelation and other effects, thereby achieving an excellent pre-paved anti-adhesive effect of waterproofing and preventing water seepage.
[0040] Comparative Example 1:
[0041] The preparation of a pre-sprayed anti-sticky waterproof coating involved in a method for waterproofing an underground floor and the overall waterproof system structure are the same as in Example 1, except that a photosensitive initiator is not added during the preparation process. Other aspects are the same as in Example 1. After the pre-sprayed anti-sticky waterproof coating is sprayed, the surface becomes sticky and the coating takes a long time to cure.
[0042] Comparative Example 2:
[0043] The preparation of a pre-sprayed anti-sticky waterproof coating involved in an underground floor waterproofing construction method and the overall waterproofing system structure are the same as in Example 1, except that the polymer emulsion is replaced with a conventional VAE emulsion during the preparation process. The rest is the same as in Example 1. After the pre-sprayed anti-sticky waterproof coating is sprayed, the surface becomes sticky and the coating takes a long time to cure.
[0044] Comparative Example 3:
[0045] The preparation of a pre-sprayed anti-sticky waterproof coating involved in a method for waterproofing an underground floor and the overall waterproof system structure are the same as in Example 1, except that the surface of the upper sheet layer of the double-layer composite non-asphalt-based polymer waterproof membrane is not specially treated. The rest is the same as in Example 1. After the pre-sprayed anti-sticky waterproof coating is sprayed, the coating and the double-layer composite polymer waterproof membrane are generally bonded, and the "skin-type waterproof" effect cannot be achieved.
[0046] Comparative Example 4:
[0047] The preparation of a pre-sprayed anti-sticky waterproof coating involved in an underground floor waterproofing construction method and the overall waterproofing system structure are the same as in Example 1, except that the pre-sprayed anti-sticky waterproof coating is replaced with a conventional acrylic waterproof coating. The other aspects are the same as in Example 1. The coating has general adhesion with the double-layer composite polymer waterproof membrane, and has low peeling strength with post-cast concrete, and cannot achieve a "skin-type waterproofing" effect.
[0048] The specific results of the peeling strength of the double-layer composite polymer waterproof membrane prepared in the above Examples 1 to 4 and Comparative Examples 1 to 4 and the post-cast concrete after being composited with the pre-sprayed anti-adhesive waterproof coating are shown in the following table:
[0049]
[0050] The above describes the specific embodiments of the present invention, but the present invention is not limited to the above description. For those skilled in the art, any equivalent modification and substitution of the technical solution is within the scope of the present invention. Therefore, the equalization and modification made without departing from the spirit and scope of the present invention should be included in the scope of the present invention.
Claims
1. A method for underground floor construction, characterized in that: The following steps are involved: S1. Lay a double layer of composite non-asphalt-based polymer waterproofing membrane on the cushion layer; S2. Spray the pre-sprayed anti-adhesive waterproof coating on the double-layer composite non-asphalt-based polymer waterproof membrane, and solidify it after construction to form a waterproof layer with an anti-adhesive effect; S3. After tying the steel bars on the waterproof layer described in S2, the poured concrete slurry forms effective interpenetrating bonding and intermolecular forces between the pre-sprayed anti-adhesive coating and the concrete layer under pressure through creep, coupling, chelation and other effects, thereby forming a "skin-type" overall waterproofing. The entire waterproof layer has no overlap, eliminating the risk of leakage caused by overlap seams.
2. An underground floor construction method according to claim 1, characterized in that: The double-layer composite non-asphalt-based polymer waterproofing membrane comprises a lower main material layer, an adhesive layer, and an upper main material layer; the lower main material layer is a 0.9-1.0 mm HDPE composite polymer layer that has been modified and toughened; the adhesive layer is a hot-melt pressure-sensitive adhesive layer; and the upper main material layer is a 0.4-0.5 mm HDPE sheet layer with a specially treated upper surface.
3. An underground floor construction method according to claim 2, characterized in that: The special treatment on the upper surface of the upper main material layer is corona treatment.
4. An underground floor construction method according to claim 2, characterized in that: The method for preparing the double-layer composite non-asphalt-based polymer waterproofing membrane comprises the following steps: S1, forming a 0.9-1.0 mm modified and toughened HDPE composite polymer layer on the lower main material layer; S2. After the hot-melt pressure-sensitive adhesive is melted, it is evenly coated on the surface of the composite polymer layer, with a coating thickness of 0.2 to 0.4 mm. A lap width of 90 to 120 mm is reserved on one side of the coil, and an isolation edge film is applied; S3, covering the film with a 0.4-0.5 mm thick HDPE sheet layer that has been corona treated; S4. Double-layer composite non-asphalt-based polymer waterproof membrane is rolled up and packaged.
5. An underground floor construction method according to claim 1, characterized in that: The pre-sprayed anti-stick waterproof coating is composed of the following raw materials in parts by weight: 45-65 parts of polymer emulsion, 20-25 parts of modified filler, 5-10 parts of water, 5-10 parts of flame retardant, 1-5 parts of flame retardant synergist, 0.3-0.6 parts of dispersant, 0.6-0.8 parts of defoaming agent, 0.2-0.5 parts of photoinitiator, 0.5-1.0 parts of silane coupling agent and 0.2-0.6 parts of thickener.
6. An underground floor construction method according to claim 5, characterized in that: The polymer emulsion is at least one of acrylic emulsion, polyurethane emulsion and polyurethane acrylate composite emulsion. The polymer emulsion has a solid content of 40-50%, a glass transition temperature of -40--45°C and a branching degree of 0.70-0.
85.
7. An underground floor construction method according to claim 5, characterized in that: The preparation method of the pre-sprayed anti-sticking waterproof coating comprises the following steps: S1. Weigh water, 1 / 2 polymer emulsion, dispersant, and defoamer in order by weight, add them into the barrel, and start stirring; S2, adding modified fillers, flame retardants, flame retardant synergists, increasing the stirring rate, and dispersing evenly; S3. Add the remaining polymer emulsion, photoinitiator, silane coupling agent and thickener, stir evenly, and filter out the material.
8. An underground floor construction method according to claims 1-7, characterized in that: The specific construction steps include: 1) Directly lay a double layer of composite non-asphalt-based polymer waterproofing membrane on the cushion layer, with the membranes bonded by the adhesive layer, and the corona-treated surface facing upwards; 2) Spraying construction: Pre-spray the anti-stick waterproof coating, which will volatilize and photocatalytically cure for 12 to 24 hours. The specific curing time can be appropriately extended according to the weather. The coating will be firmly bonded to the corona-treated HDPE sheet to form a continuous, uniform and seamless waterproof coating. 3) Pour concrete directly on the waterproof coating after the structural reinforcement. Under the action of pressure, the concrete slurry can form full adhesion with the post-poured concrete through creep, coupling, chelation and other effects, achieving an excellent pre-paving anti-adhesion effect of waterproofing and preventing water seepage.