Method for solving wrinkling of flange face of integral vehicle door inner plate
By optimizing the door inner panel model through the CAE program and analysis system, adjusting the bead and mold parameters, the problem of wrinkling of the flange surface of the integral door inner panel was solved, achieving more efficient debugging and cost savings, and improving the cost competitiveness of the vehicle. .
Patent Information
- Application Number
- CN202410776969.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-02-27
- Filing Date
- 2024-06-17
- Publication Date
- 2024-10-18
AI Technical Summary
The flange surface of the integral door inner panel is prone to wrinkles, resulting in long on-site rectification cycles and high costs, affecting the planned schedule.
The door inner panel model was established through the CAE program, and the bead geometry and mold inflow were adjusted. Combined with the BEM-5 and EPS-11 analysis systems, the formability and wrinkle risk were verified, and the process parameters were optimized to reduce the number of debugging times and costs.
It effectively reduces the number of debugging times and costs caused by wrinkling of the drawing die by 50%, solves the problem of wrinkling of the flange surface of the inner door panel, and improves molding quality and material utilization.
Smart Images

Figure CN118797798A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of automobile processing, and in particular relates to a method for solving the wrinkling of the flange surface of an integral vehicle door inner panel. Background Art
[0002] With the rapid development of the automobile industry, the competition in the industry is becoming increasingly fierce. The requirements for automobile stamping process solutions are getting higher and higher. Not only must the dimensional accuracy of automobile parts be met, but also the surface quality requirements must be guaranteed. In order to improve the overall consistency requirements of the door assembly during installation, the flange edge of the door inner panel also needs to be audited. This puts higher requirements on the wrinkling problem of the flange edge of the car panel inner panel. The inner panels of automobile doors are roughly divided into two categories: half-section type and integral type. Among them, the integral door is prone to wrinkling of the flange edge during the molding process due to the large curvature of the part, which affects the surface quality and is unacceptable to customers. At the same time, due to the long time period and high cost of on-site rectification, it affects the planned progress nodes and has become a key issue of concern in the industry. Summary of the invention
[0003] In view of this, the present invention aims to propose a method for solving the wrinkling of the flange surface of the integral door inner panel, so as to solve the problem of long on-site rectification period, high cost and impact on the planned progress nodes.
[0004] To achieve the above object, the technical solution of the present invention is achieved as follows:
[0005] A method for solving the wrinkling of the flange surface of an integral door inner panel comprises the following steps:
[0006] S1: Collect CATIA data of the door inner panel and build the door inner panel model using CAE program;
[0007] S2: Compare the obtained material parameter values with the actual plate performance measurement data, compare the forming force and blank holding force of the door inner panel model with the on-site debugging data, and compare the analyzed material inflow of the door inner panel model with the actual inflow of the on-site parts;
[0008] S3: Adjust the geometric dimensions of the ribs according to the BEM-5 analysis results, and then establish the door inner panel model through the BEM program;
[0009] S4: The adjusted BEM program establishes a door inner panel model to determine wrinkles. If wrinkles occur, proceed to step S3; otherwise, proceed to step S5;
[0010] S5: In step S5, BEM-5 is converted to EPS-11 for formability verification. The AutoForm software calculates the page option button. This function is only used to evaluate the wrinkling of the flange plane and determine whether the forming cracks. The AutoForm software crack check, when the MaxFailure value is greater than 0.75, it is determined that the part is cracked. If cracked, proceed to step S3.
[0011] The CATIA data in step S1 are the product 3D digital model, part material, part thickness, and the overlap relationship between the door outer panel and the part assembly.
[0012] When using CAE programs to build door inner panel models, it is necessary to achieve the most ideal formability, the least number of molds, and the highest material utilization rate while meeting the customer's production equipment requirements. Under the premise of ensuring quality, the material utilization rate of parts is maximized to achieve cost savings and improve the cost competitiveness of automobiles.
[0013] Furthermore, the analysis of the material inflow of the door inner panel model in step S2 is compared with the actual inflow of the on-site component, and the error does not exceed ±3%. When the inflow is less than 3%, the material required for molding is insufficient, resulting in thinning or even cracking of the component. When the inflow is greater than 3%, there is too much material stored for molding, resulting in wrinkling of the molding. The mold inflow is adjusted by adjusting the gap between the mold concave die and the pressure regulating pad of the blank holder. The smaller the gap, the more difficult it is for the material to flow in, and the larger the gap, the more material can flow in.
[0014] Furthermore, the parameters compared in step S2 include yield strength, tensile strength, strain hardening index, and the ratio of transverse deformation to longitudinal deformation of the metal material during the stretching process.
[0015] Yield strength: The smaller the stress yield strength of metal materials to resist micro plastic deformation, the easier it is for the material to yield, so it will rebound less after forming, and it will be less likely to crack if it has good formability. However, materials with low yield strength are prone to wrinkling during compression deformation. Tensile strength: The maximum bearing capacity of metals under static tension. Tensile strength is the resistance to the maximum uniform plastic deformation of the material. Before the tensile specimen is subjected to the maximum tensile stress, the deformation is uniform, but after exceeding it, the metal begins to neck, that is, concentrated deformation occurs. Strain hardening index n: The true plastic strain index in the mathematical equation of true stress and true plastic strain under uniaxial tensile stress is also called strain hardening index n. It reflects the ability of metal materials to resist uniform plastic deformation. The larger the n value, the better the safety performance, processability, and mechanical properties. Anisotropy r refers to the ratio of transverse deformation to longitudinal deformation of metal materials during stretching: the larger the r value, the easier it is to deform in the width direction (in the plane) of the plate than in the thickness direction. Therefore, the material tends to stretch in the plane rather than thin in the thickness direction, and the thinning of thickness is the cause of fracture during the stamping process. Therefore, the larger the r value, the lower the possibility of fracture. The above parameters are compared to analyze whether the selected material parameters are consistent with the actual purchased sheet material parameters and performance. Eliminate the influence of sheet material parameter differences on drawing formability.
[0016] Furthermore, in step S3, the drawbead height adjustment range is 1.5 mm-3.5 mm.
[0017] In step S3, the forming force and blank holder force of the door inner panel model are compared with the on-site debugging data. The pressure parameters input by the machine tool during the drawing die debugging must be consistent with the values set by CAE analysis. Otherwise, the authenticity of the inflow of the drawing material will be affected. The inflow of the drawing CAE analysis is the basis for guiding production debugging: the drawing die will mark the inflow position of the CAE analysis on the blank holder ring surface through CNC machining. The mold debugging needs to adjust the actual inflow to be consistent with the inflow of the CAE analysis. Too much inflow causes wrinkling, and too little inflow causes cracking.
[0018] Furthermore, the wrinkling judgment in step S4 includes that there is no wrinkling tendency in the forming process, otherwise it is wrinkled.
[0019] Furthermore, the wrinkle judgment in step S4 includes the PotentialWrinkles parameter value of the side wall and flange of the door inner panel being less than 0.01, otherwise it is wrinkled. The draw rib adjustment is a fine adjustment between wrinkle and cracking, which is optimized by adding the molding ribs supplemented by the process to meet the judgment value.
[0020] Furthermore, the wrinkle determination in step S4 includes that the SurfceDefect Height parameter value of the pressing surface, side wall and flange surface of the door inner panel cannot exceed 0.1, otherwise it is wrinkled.
[0021] In order to control the target to a smaller range and achieve the best balance of formability, this application requires a large amount of data analysis and comparison in the CAE analysis stage, by setting the fluctuation range of important parameters, such as the clamping force ±10%, the mold surface friction coefficient ±10%, and the sheet size fluctuation ±10%. The automatic sorting and matching of the software requires the calculation of 48 analysis results. From a large number of data, data collection is carried out to meet the CAE forming judgment criteria and is more robust, referring to the index requirements in S2 and S4. While ensuring that the evaluation values are met, the fluctuation range of on-site production and how to design it to be more conducive to on-site debugging must also be considered. CAE analysis is not 100% accurate, but it can guide us to achieve ideal results without CNC machining, only simple optimization by fitters.
[0022] Compared with the prior art, the method for solving the wrinkling of the flange surface of the integral door inner panel described in the present invention has the following advantages:
[0023] This patent aims at the wrinkling problem of flat areas of parts. For example, BEM-5 analysis is used for the flange edge area of the inner door panel, and EPS-11 analysis results are used for other areas. The risk of wrinkling is eliminated by combining the BEM-5 system with the EPS-11 system for confirmation and double verification. It can reduce the number of debugging times caused by wrinkling of the drawing die, save cycles, and reduce costs. It is 50% of the money cost and time cost of the traditional process method, and solves the wrinkling problem of the flange surface of the inner door panel as a whole. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] The accompanying drawings constituting a part of the present invention are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the accompanying drawings:
[0025] Figure 1 This is a schematic diagram of the BEM-5 analysis results when the drawbead height described in Example 1 of the present invention is increased to 3.5 mm;
[0026] Figure 2 This is a schematic diagram of the wrinkling analysis results of BEM-5 with a rib height of 1.5 mm in Example 1 of the present invention;
[0027] Figure 3 Schematic diagram of wrinkling analysis results of BEM-5 with rib height of 3.5 mm in Example 1 of the present invention
[0028] Figure 4 This is a schematic diagram of the inflow analysis results of BEM-5 with a rib height of 1.5 mm in Example 1 of the present invention;
[0029] Figure 5 This is a schematic diagram of the inflow analysis results of BEM-5 with a rib height of 3.5 mm in Example 1 of the present invention;
[0030] Figure 6 This is a schematic diagram of a BEM-5 with a rib height of 3.5 mm in Example 1 of the present invention being drawn to 10 mm before the bottom;
[0031] Figure 7 This is a schematic diagram of a BEM-5 with a rib height of 3.5 mm in Example 1 of the present invention being drawn to 5 mm before the bottom;
[0032] Figure 8 This is a schematic diagram of BEM-5 with a rib height of 3.5 mm being drawn to the bottom in Example 1 of the present invention;
[0033] Fig. 9 This is a schematic diagram of Potential Wrinkles evaluation in Example 1 of the present invention;
[0034] Fig.10 This is a schematic diagram of Surface Defect Heigh evaluation in Example 1 of the present invention;
[0035] Fig.11 This is a schematic diagram of the draw bead height increased to 3.5 mm (EPS-11 formability) in Example 1 of the present invention;
[0036] Fig.12 Schematic diagram of eliminating flange surface wrinkles after rectification in Example 1 of the present invention;
[0037] Fig.13 This is a schematic diagram of the BEM-5 analysis results in Example 1 of the present invention;
[0038] Fig.14 This is a schematic diagram of the existing results in Example 1 of the present invention;
[0039] Fig.15 This is a schematic diagram of the CAE analysis result troubleshooting process for Comparative Example 1 of the present invention;
[0040] Fig.16 This is a schematic diagram of the CAE analysis parameters of the sheet material of Comparative Example 1 of the present invention;
[0041] Fig.17 This is a schematic diagram of the measured sheet material parameters of Comparative Example 1 of the present invention;
[0042] Fig.18 This is a schematic diagram of the blank holding force and forming force of CAE analysis of Comparative Example 1 of the present invention;
[0043] Fig.19 This is a schematic diagram of the measured and debugged blank holding force and forming force of Comparative Example 1 of the present invention;
[0044] Fig. 20 This is a schematic diagram of the material inflow of CAE analysis of Comparative Example 1 of the present invention;
[0045] Fig.21 This is a schematic diagram of the thick shell unit EPS-11 of Comparative Example 1 of the present invention;
[0046] Fig. 22 This is a BEM schematic diagram of the enhanced membrane unit of Comparative Example 1 of the present invention;
[0047] Fig.23 This is a schematic diagram of actual parts of Comparative Example 1 of the present invention.
[0048] Fig.24 This is a schematic diagram of the drawing process of the integral door inner panel of the vehicle model of Comparative Example 2 of the present invention;
[0049] Fig.25 This is a schematic diagram of the drawing to the first 10 mm of the bottom of comparative example 2 of the present invention;
[0050] Fig.26 This is a schematic diagram of the drawing to the first 5 mm of the bottom of comparative example 2 of the present invention;
[0051] Fig. 27 This is a schematic diagram of the bottom drawing of Comparative Example 2 of the present invention;
[0052] Fig.28 The wrinkle inspection after drawing for comparative example 2 of the present invention meets the CAE evaluation requirements;
[0053] Fig.29 This is a schematic diagram of the wrinkling of the flange surface area of comparative example 2 of the present invention. DETAILED DESCRIPTION
[0054] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present invention can be combined with each other. The present invention aims to propose a method for solving the wrinkling of the flange surface of the integral door inner panel, so as to solve the problem of long on-site rectification period, high cost and impact on the planned progress node.
[0055] The present invention will be described in detail below with reference to the accompanying drawings and in conjunction with embodiments.
[0056] A method for solving the wrinkling of the flange surface of an integral door inner panel comprises the following steps:
[0057] S1: Collect CATIA data of the door inner panel and use CAE program to build the door inner panel model. The CATIA data in step S1 is the product 3D digital model, part material, part thickness, and the overlap relationship between the door outer panel and the part assembly. When using CAE program to build the door inner panel model, it is necessary to achieve the most ideal formability, the least number of molds, and the highest material utilization rate under the premise of meeting the customer's production equipment requirements. Under the premise of ensuring quality, maximize the material utilization rate of parts to achieve cost savings and improve the cost competitiveness of automobiles.
[0058] S2: Compare the obtained material parameter values with the actual plate performance measurement data, compare the forming force and blank holding force of the door inner panel model with the on-site debugging data, and compare the analyzed material inflow of the door inner panel model with the actual inflow of the on-site parts;
[0059] The parameters compared in step S2 include yield strength, tensile strength, strain hardening index, and the ratio of transverse deformation to longitudinal deformation of the metal material during the stretching process.
[0060] Yield strength: The smaller the stress yield strength of metal materials to resist micro plastic deformation, the easier it is for the material to yield, so it will rebound less after forming, and it will be less likely to crack if it has good formability. However, materials with low yield strength are prone to wrinkling during compression deformation. Tensile strength: The maximum bearing capacity of metals under static tension. Tensile strength is the resistance to the maximum uniform plastic deformation of the material. Before the tensile specimen is subjected to the maximum tensile stress, the deformation is uniform, but after exceeding it, the metal begins to neck, that is, concentrated deformation occurs. Strain hardening index n: The true plastic strain index in the mathematical equation of true stress and true plastic strain under uniaxial tensile stress is also called strain hardening index n. It reflects the ability of metal materials to resist uniform plastic deformation. The larger the n value, the better the safety performance, processability, and mechanical properties. Anisotropy r refers to the ratio of transverse deformation to longitudinal deformation of metal materials during stretching: the larger the r value, the easier it is to deform in the width direction (in the plane) of the plate than in the thickness direction. Therefore, the material tends to stretch in the plane rather than thin in the thickness direction, and the thinning of thickness is the cause of fracture during the stamping process. Therefore, the larger the r value, the lower the possibility of fracture. The above parameters are compared to analyze whether the selected material parameters are consistent with the actual purchased sheet material parameters and performance. Eliminate the influence of sheet material parameter differences on drawing formability.
[0061] The analysis of the material inflow of the door inner panel model in step S2 is compared with the actual inflow of the on-site part, and the error does not exceed ±3%. When the inflow is less than 3%, the material required for molding is insufficient, resulting in thinning or even cracking of the part. When the inflow is greater than 3%, there is too much material stored for molding, resulting in wrinkling. The mold inflow is adjusted by adjusting the gap between the mold cavity and the pressure ring. The smaller the gap, the more difficult it is for the material to flow in, and the larger the gap, the more material will flow in.
[0062] S3: Adjust the geometric dimensions of the ribs according to the BEM-5 analysis results, and then establish the door inner panel model through the BEM program;
[0063] In step S3, the drawbead height increases from 1.5 mm to 3.5 mm, which is the best value range. The specific parameter settings are adjusted and corrected according to the actual situation.
[0064] In step S3, the forming force and blank holder force of the door inner panel model are compared with the on-site debugging data. The pressure parameters input by the machine tool during the drawing die debugging must be consistent with the values set by CAE analysis, otherwise it will affect the authenticity of the inflow of the drawing material. The inflow of the drawing CAE analysis is the basis for guiding production debugging: the drawing die marks the inflow position of the CAE analysis on the blank holder ring surface through CNC machining. The mold debugging needs to adjust the actual inflow to be consistent with the inflow of CAE analysis. Too much inflow causes wrinkling, and too little inflow causes cracking.
[0065] S4: The adjusted BEM program establishes a door inner panel model to determine wrinkles. If wrinkles occur, proceed to step S3; otherwise, proceed to step S5;
[0066] The wrinkle determination in step S4 includes that there is no wrinkle tendency in the forming process, otherwise it is wrinkled.
[0067] In step S4, the wrinkle judgment includes the Potential Wrinkles parameter value of the side wall and flange of the door inner panel is less than 0.01, otherwise it is wrinkled. The draw rib adjustment is a fine adjustment between wrinkling and cracking, which is optimized by adding the molding ribs supplemented by the process to meet the judgment value.
[0068] Furthermore, the wrinkle determination in step S4 includes that the SurfceDefect Height parameter value of the pressing surface, side wall and flange surface of the door inner panel cannot exceed 0.1, otherwise it is wrinkled.
[0069] S5: In step S5, BEM-5 is converted to EPS-11 for formability verification. The AutoForm software calculates the page option button. This function is only used to evaluate the wrinkling of the flange plane and determine whether the forming cracks. The AutoForm software crack check, when the MaxFailure value is greater than 0.75, it is determined that the part is cracked. If cracked, proceed to step S3.
[0070] AUTOFORM uses the CAE analysis results of the thick shell unit EPS-11 to determine that there is no wrinkling risk. Wrinkling judgment factors: wrinkle risk molding process judgment, no wrinkling trend and no ripples 10mm before drawing to the end; wrinkle risk numerical judgment at the end of molding: the judgment standard product area is not greater than 0.02, and the analysis results meet the standards.
[0071] In order to control the target to a smaller range and achieve the best balance of formability, this application requires a large amount of data analysis and comparison in the CAE analysis stage, by setting the fluctuation range of important parameters, such as the clamping force ±10%, the mold surface friction coefficient ±10%, and the sheet size fluctuation ±10%. The automatic sorting and matching of the software requires the calculation of 48 analysis results. From a large number of data, data collection is carried out to meet the CAE forming judgment criteria and is more robust, referring to the index requirements in S2 and S4. While ensuring that the evaluation values are met, the fluctuation range of on-site production and how to design it to be more conducive to on-site debugging must also be considered. CAE analysis is not 100% accurate, but it can guide us to achieve ideal results without CNC machining, only simple optimization by fitters.
[0072] Example 1: The inner door panel is a typical inner panel part in the automobile covering. It usually requires 4 mold processes to complete, and the delivery cycle from the design to the mold acceptance is about 6 months. It is combined with the outer door panel through hemming or rolling to form the overall frame structure of the door assembly. With the improvement of the perceived quality of appearance in the automotive industry, although the inner door panel is an inner panel part without an appearance surface, since part of the inner door panel is visible after the door is opened, the quality of the inner door panel is now increasingly valued by automobile manufacturers. The wrinkles in the flange surface area are located in the visible area when the door is opened, so this problem must be completely eliminated to meet the current needs of customers.
[0073] Readjusted according to the BEM-5 analysis results, such as Figure 1 As shown. The geometric dimensions of the drawbeads in the corresponding area were adjusted, and the drawbead height was increased by multiples of 0.5mm. The analysis results were compared after each increase. The drawbead height increased from 1.5mm to 3.5mm. There was no wrinkling trend or value on the flange edge during the BEM-5 analysis process and results. EPS-11 analysis verified that there was no risk of cracking.
[0074] like Figure 2 , Figure 3 As shown, by comparing the BEM-5 analysis before and after the change, Figure 3 The wrinkling problem was solved after the local drawbeads were raised.
[0075] like Figure 4 , Figure 5 As shown in the figure, the inflow volume changes due to the heightening of the drawbead, and the maximum position differs by 26 mm. Other parameters remain unchanged.
[0076] like Figure 6-8 As shown, the wrinkling judgment after adjustment according to the BEM-5 analysis results: there is no wrinkling tendency in the molding process.
[0077] like Fig. 9As shown, the stress-strain judgment method Potential Wrinkles product area <0.03, the product area detection value less than 0.03 meets the judgment standard.
[0078] like Fig.10 As shown, the characteristic value judgment method Surface Defect Heigh product area <±0.1. The product area detection value is less than 0.03, which meets the judgment standard.
[0079] According to the result of increasing the local drawbead height by 3.5mm in BEM-5, the result is converted into EPS-11 for formability verification to determine whether the forming cracks are caused by increasing the drawbead height. Fig.11 As shown, there is no cracking.
[0080] The drawing die processes the drawbead according to the process rectification plan, and the parts are re-produced after the drawbead is rectified on site. The wrinkling problem of the flange edge is solved. Fig.12 shown.
[0081] This patent changes the original AUTO-FORM software to only use the thick shell unit EPS-11 using the CAE analysis results of 11 layers of elastic plastic shell (EPS) to determine, and also refers to the wrinkle analysis results of BEM-5 using 5 layers of bending enhanced membrane (BEM). By comparison, it can be found that the wrinkle trend at the flange edge of the door inner panel is closer to the BEM-5 analysis results, such as Fig.13 , Fig.14 As shown. In the Autoform software, BEM (bending enhanced membrane) is a unit algorithm, which is endowed with a certain bending stiffness. Therefore, the application of membrane unit analysis has low calculation accuracy, exaggerated wrinkling results, and relatively mild cracking problems. Therefore, only in the fast Autoform shell unit based on the traditional shell unit theory, the results of shell unit analysis will be different, and the accuracy of shell units is much higher than that of membrane units. With the improvement of computer capabilities, CAE analysis is usually carried out using the more accurate EPS-11 shell unit. At present, only the wrinkling problem of the flat area of the part is discussed. For example, the flange edge area of the inner door panel is analyzed using BEM-5, and other areas are still subject to the EPS-11 analysis results.
[0082] The CAE analysis structure of EPS-11 material shell unit meets the evaluation criteria, but wrinkles still occur in the area where the inflow of the inner door panel is greater than 50mm. The analysis results of EPS-11 material shell unit cannot identify such problems. After optimizing the process according to the BEM-5 analysis results, there is no wrinkle risk problem on site if the CAE analysis of EPS-11 material shell unit is passed, as detailed in the following situations.
[0083] EPS-11 (material shell element) CAE analysis OK - there is still a risk of wrinkling on site;
[0084] BEM-5 (material membrane unit) CAE analysis OK - there is still risk of thinning on site;
[0085] EPS-11 (material shell unit) CAE analysis is OK, BEM-5 (material membrane unit) CAE analysis is OK;
[0086] Before adopting this analysis method, the overall door inner panel drawing die needed to be designed to change the processing technology according to the on-site situation, partially weld the surface, perform CNC machining, and re-grind and debug by fitters. The cost of adjusting one cycle is shown in Table 1;
[0087] Table 1
[0088] department design programming Repair welding CNC debug total Working hours / working hours 8 16 8 24 40 96 Cost / Yuan 300 600 2000 20000 20000 42900
[0089] In the prior art, 1-2 times of debugging is required. After adopting the double verification method of this application, the risk of wrinkling is eliminated, and the drawing mold does not need to be debugged for the second time due to wrinkling problems, which saves cycles and reduces costs, reducing costs and time by half. A single set of molds weighs about 16 tons, with a unit price of 38,000 yuan / ton, and a price of about 608,000 yuan. The secondary cost of rectification accounts for about 14%, and the cycle is 24 working days. At present, customers define the position that can be seen when the door is opened as a level 2 appearance surface for the inner panel of the car door. The level 2 appearance surface has strict requirements, no ripples can be seen visually, and no short lines can be found in the oilstone inspection. Refer to the Class A surface inspection standard.
[0090] In addition, the automotive industry is highly competitive and implements a short-cycle strategy. The total cycle from project launch to mold return to the factory is 6 months. During the mold manufacturing process, there are only 10-12 working days to improve the dimensional accuracy. There is no time for wrinkling and cracking rectification. This requires us to solve this kind of wrinkling problem in one go, without time and opportunity for rework.
[0091] Comparative Example 1:
[0092] In order to find out the reasons why the CAE analysis results are inconsistent with the actual wrinkling state of the parts, the elimination method is used to check the key factors that affect the wrinkling of the parts one by one: 1: Comparison of CAE analysis material card with actual sheet material performance measurement data. 2: Comparison of CAE analysis forming force and blank holder force with on-site debugging data. 3: Comparison of AE analysis material inflow with actual inflow of on-site parts. 4: Comparison of CAE analysis BEM mold unit EPS shell unit analysis results with on-site parts. See Fig.15 (CAE analysis result troubleshooting flow chart).
[0093] go through Fig.16 and Fig.17It can be seen that the CAE analysis values of the material parameters of the parts are basically consistent with the actual measured sheet material values on site, and will not affect the analysis results.
[0094] go through Fig.18 and Fig.19 It can be seen that the values of the blank holding force and forming force obtained by CAE analysis of the workpiece are consistent with the actual measurements on site. The on-site debugging personnel make on-site mold adjustments according to the values given by CAE analysis.
[0095] go through Fig. 20 It can be seen that the comparison shows that the error between the CAE analysis material inflow and the measured material is within 3%, which meets the requirement that the inflow in step S2 does not exceed 3%. Figure 21-23 In Comparative Example 1, since the solution of this patent was not discovered at that time, the CAE analysis in the early process design stage failed to find the wrinkling of the flange surface. The wrinkling problem can only be solved through on-site experience. By increasing the height of the drawing supplementary profile to absorb the excess wrinkled material, the design changes the height of the supplementary modeling surplus meat by 15mm according to the on-site suggestions, and the programming is written according to the modified modeling. The fitter welds the mold, and the drawing punch is partially welded with an area of 300mm*50mm*15mm before processing. The concave model surface is directly processed, and the mold press is re-grinded and debugged after processing. After one round of debugging, it was found that the supplementary height was too high, and another round of debugging was carried out to solve the problem. The two rectifications totaled about 200 hours of working time, which caused a huge waste, which not only affected the construction period, but also generated costs.
[0096] Later, by comparing the analysis results of AUTOFORM thick shell element EPS-11 and bending enhanced membrane (BEM), it can be found that the results of BEM membrane element Fig. 22 The actual field results Fig.23 Basically the same. If it is discovered in the early stage, it can avoid wasted time and cost.
[0097] Comparative Example 2:
[0098] Fig.24 Supplement the drawing process of the whole door inner panel of a certain car model. CAE analysis conducted by AUTOFORM in the early stage showed no wrinkling risk.
[0099] Wrinkle risk is judged during the forming process. There is no wrinkle tendency and no ripples in the first 10mm of the drawing. This condition is the key factor in wrinkle judgment. Figure 25-27 .
[0100] Numerical judgment of wrinkle risk at the bottom of the molding. The judgment standard product area is not greater than 0.02, and the analysis results meet the standard, such as Fig.28 As shown,
[0101] The actual production of the door inner panel flange area is seriously wrinkled, which is inconsistent with the CAE analysis results. Fig.29 As shown. In the later review, by comparing the analysis results of AUTOFORM thick shell element EPS-11 and bending enhanced membrane (BEM), the existence of wrinkling problems can be found. If it is discovered in the early stage, the waste of time and cost can be avoided.
[0102] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for solving the wrinkling of the flange surface of the integral door inner panel, characterized in that: The steps include: S1: Collect CATIA data of the door inner panel and build the door inner panel model using CAE program; S2: Compare the obtained material parameter values with the actual plate performance measurement data, compare the forming force and blank holding force of the door inner panel model with the on-site debugging data, and compare the analyzed material inflow of the door inner panel model with the actual inflow of the on-site parts; S3: According to the BEM-5 analysis results, the geometric dimensions of the ribs are adjusted, and after the adjustment, the door inner panel model is established through the BEM program; S4: The adjusted BEM program establishes a door inner panel model to determine whether wrinkles occur. If wrinkles occur, proceed to step S3; otherwise, proceed to step S5. S5: BEM-5 is converted to EPS-11 for formability verification to determine whether cracking occurs. If the Max Failure is less than 0.75, cracking occurs. If cracking occurs, proceed to step S3. If there is no cracking, the drawing die will process the drawbead according to the data in the final rectification plan, and the part will be re-produced after the drawbead is rectified.
2. A method for solving the wrinkling of the flange surface of the integral door inner panel according to claim 1, characterized in that: The CATIA data in step S1 are the product 3D digital model, part material, part thickness, and the overlap relationship between the door outer panel and the part assembly.
3. The method for solving the wrinkling of the flange surface of the integral door inner panel according to claim 1, characterized in that: The analyzed material inflow of the door inner panel model in step S2 is compared with the actual inflow of the on-site component, and the error does not exceed 3%. The mold inflow is adjusted by adjusting the gap between the mold cavity and the pressure regulating pad.
4. The method for solving the wrinkling of the flange surface of the integral door inner panel according to claim 1, characterized in that: The parameters compared in step S2 include yield strength, tensile strength, strain hardening index, and the ratio of transverse deformation to longitudinal deformation of the metal material during the stretching process. By comparing the parameters, the influence of the difference in sheet material parameters on the drawing formability is eliminated.
5. The method for solving the wrinkling of the flange surface of the integral door inner panel according to claim 1, characterized in that: In step S3, the forming force and the blank holding force of the door inner panel model are compared with the on-site debugging data. The pressure parameters input by the machine tool during the drawing die debugging are consistent with the values set by the CAE analysis. The drawing die uses CNC machining to mark the inflow position analyzed by CAE on the blank holding ring surface as a basis for guiding production debugging. When debugging the mold, the actual inflow is adjusted to be consistent with the inflow analyzed by CAE.
6. The method for solving the wrinkling of the flange surface of the integral door inner panel according to claim 1, characterized in that: In step S3, the drawbead height adjustment range is 1.5 mm-3.5 mm.
7. The method for solving the wrinkling of the flange surface of the integral door inner panel according to claim 1, characterized in that: The wrinkle determination in step S4 includes that there is no wrinkle tendency in the forming process, otherwise it is wrinkled.
8. The method for solving the wrinkling of the flange surface of the integral door inner panel according to claim 1, characterized in that: The wrinkle judgment in step S4 includes that the Potential Wrinkles parameter value of the door inner panel flange is less than 0.01, otherwise it is wrinkled, and the draw rib adjustment is between wrinkling and cracking to be optimized by adding the molding ribs supplemented by the process to meet the judgment value.
9. The method for solving the wrinkling of the flange surface of the integral door inner panel according to claim 1, characterized in that: The wrinkle determination in step S4 includes that the Surfce Defect Height parameter value of the pressing surface, side wall and flange surface of the door inner panel cannot exceed 0.1, otherwise it is wrinkled.
10. The method for solving the wrinkling of the flange surface of the integral door inner panel according to claim 1, characterized in that: AUTOFORM uses the CAE analysis results of the thick shell unit EPS-11 to determine that there is no wrinkling risk. Wrinkling judgment factors: Wrinkling risk molding process judgment, no wrinkling trend and no ripples before drawing to the bottom 10mm; Numerical judgment of wrinkling risk at the bottom of molding: the judgment standard product area is not greater than 0.02, and the analysis results meet the standards.