Soft magnetic composite metal material for integrally formed inductor and preparation method of soft magnetic composite metal material

By using aerosolized iron-nickel powder and carbonyl iron powder combined with modified γ-Fe2O3 and glass fiber insulating agents, the problem of magnetic dilution and loss of soft magnetic composite metal materials in one-piece molded inductors is solved, achieving high superposition performance and The low-loss effect meets the requirements for efficient operation in low-voltage and high-current scenarios.

CN118800543APending Publication Date: 2024-10-18XUANCHENG MAIWEI NEW MATERIAL TECH CO LTD
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202410786995.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-18
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

Existing soft magnetic composite metal materials have problems with magnetic dilution and increased losses in integrated inductors, making it difficult to meet the low-loss and high-efficiency working requirements in low-voltage and high-current scenarios.

Method used

Using aerosolized iron-nickel powder and carbonyl iron powder as metal powder, combined with modified γ-Fe2O3 and modified glass fiber insulating agents, through passivation, coating and lubrication processes, the density and filling rate of the material are increased, and the eddy current is reduced loss, and improve the uniformity and moisture resistance of the material through powder mixing and modification of different particle sizes.

Benefits of technology

It achieves high superposition performance and low power loss of soft magnetic composite metal materials, ensuring the efficient operation of the inductor in low voltage and high current scenarios, avoiding increased losses due to damage to the insulation layer, and maintaining high reliability under high temperature conditions. sex.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004898889370000101
    Figure BDA0004898889370000101
Patent Text Reader

Abstract

The invention provides a soft magnetic composite metal material for an integrally formed inductor. The soft magnetic composite metal material comprises metal powder and an insulating agent, the metal powder is gas-atomized iron-nickel powder and carbonyl iron powder, the gas-atomized iron-nickel powder and the carbonyl iron powder are mixed according to the mass ratio of 55-65: 35-45, and the gas-atomized iron-nickel powder is at least two kinds of gas-atomized iron-nickel powder with different particle sizes; the insulating agent is a mixed solution of modified gamma-Fe2O3 and modified glass fibers, and the modified gamma-Fe2O3 is obtained by modifying gamma-Fe2O3 in magnesium acrylate and ammonia water; the modified glass fiber is prepared by modifying glass fiber in zirconium boride, aluminum nitride, a silane coupling agent and carboxylated polyethylene wax; and the mass of the water is 8-10% of that of the metal powder. According to the method, the atomized iron nickel powder and the carbonyl iron powder are mixed to serve as the metal powder, the overall filling rate of the metal powder is increased, the density of the metal powder is increased, the number of atomic magnetic moments in unit volume can be increased, and high superposition performance is achieved under the condition that the magnetic conductivity is close.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of magnetic functional materials, and in particular relates to a soft magnetic composite metal material for an integrally formed inductor and a preparation method thereof. Background Art

[0002] Inductors are one of the three major components and play an indispensable and key role in electrical and electronic equipment and systems. One-piece molded inductors are obtained by embedding coils in soft magnetic composite metal powder materials through molding. They have the advantages of small size, wide operating frequency band, good magnetic shielding, and easy automated production. They have broad market prospects. With the development of miniaturization, integration, and high efficiency of circuits, higher requirements are also put forward for one-piece molded inductors, such as low voltage and high current usage scenarios, and high-efficiency work with low loss and low heat. This requires the materials used to have high superposition and low loss performance. Therefore, the current research on soft magnetic composite metal materials is still the focus.

[0003] One-piece molded inductors mostly use carbonyl iron powder, iron-silicon-chromium alloy powder, and amorphous nanocrystalline powder as raw materials. After passivation and organic resin coating, a composite film layer can be formed on the powder surface. This film layer can not only reduce the catalytic aging effect of metal materials on organic resin materials, but more importantly, it has certain insulation properties and can reduce eddy current losses between powders and between powders and coils, thereby achieving the purpose of reducing inductor losses.

[0004] At present, the more commonly used passivation and coating methods are acid passivation, metal and non-metal oxide coating, and resin coating. For example, a low-loss and high-temperature-resistant FeSiCr one-piece molded inductor and a preparation method thereof disclosed in a Chinese patent with publication number CN117936215A uses an orthophosphoric acid solution to passivate FeSiCr powder, and achieves the purpose of low loss by adjusting the surface modifier and the organic coating agent. However, after microscopic observation and analysis such as scanning electron microscopy, a flocculent iron phosphate passivation layer will be formed on the surface of FeSiCr, FeSiAl and other iron-based soft magnetic metal powders passivated with pure phosphoric acid, and cracks will appear in the local film layer. The passivation layer cannot achieve the goal of uniformity and integrity. Therefore, the pressed inductor still has the problem of increased overall loss due to the high local eddy current of the powder.

[0005] A Chinese patent with publication number CN115240971A discloses a high magnetic permeability one-piece molding material and a preparation method thereof. The method is to sinter iron, silicon, boron, carbon and other materials in an oxygen-nitrogen atmosphere to form an oxide film layer, and then add epoxy resin and a curing agent to form the required powder. The sintered materials used in this method contain a large proportion of non-magnetic materials. Regardless of whether all of them are sintered into soft magnetic alloys or some non-magnetic materials remain, it will bring serious magnetic dilution problems, resulting in reduced material magnetic permeability and superposition performance, which still does not conform to the development trend of one-piece molding inductors. Summary of the invention

[0006] The technical problem to be solved by the present invention is how to provide a magnetic composite metal material with higher DC superposition performance and lower loss.

[0007] The present invention solves the above technical problems through the following technical means:

[0008] The first aspect of the present invention provides a soft magnetic composite metal material for integrally molded inductors, comprising metal powder and an insulating agent; the metal powder is atomized iron-nickel powder and carbonyl iron powder, the atomized iron-nickel powder and the carbonyl iron powder are mixed in a mass ratio of 55-65:35-45, and the atomized iron-nickel powder is atomized iron-nickel powder of at least two different particle sizes; the insulating agent is a mixed solution of modified γ-Fe2O3 and modified glass fiber, the modified γ-Fe2O3 is γ-Fe2O3 modified in magnesium acrylate and ammonia water; the modified glass fiber is glass fiber modified in zirconium boride, aluminum nitride, silane coupling agent, and carboxylated polyethylene wax; the mass of water is 8-10% of the metal powder.

[0009] Beneficial effects: The present invention mixes aerosolized iron-nickel powder and carbonyl iron powder as metal powder, which can improve the overall filling rate and density of the metal powder, thereby increasing the number of atomic magnetic moments per unit volume, and achieving high superposition performance under conditions of similar magnetic permeability; increasing the density of the metal powder can also reduce the power loss of the material.

[0010] γ-Fe2O3 is a magnetic iron oxide. Compared with the paramagnetism of other metal or non-metal oxides, the addition of γ-Fe2O3 can make up for the magnetic dilution effect caused by the addition of insulating coating, ensuring that the soft magnetic composite metal material has high superposition performance. In addition, the use of modified γ-Fe2O3 improves the dispersibility, making the performance of the soft magnetic composite metal material more uniform.

[0011] Conventional glass fibers have strong silanol groups on their surfaces. In the present invention, after modification with a coupling agent, the hydroxyl groups on the glass fibers condense with the hydrolyzate of silane, and the condensation between silanes converts the hydroxyl groups on the fiber surfaces with higher polarity into ether bonds with lower polarity. Carboxylated polyethylene wax is used to assist in dispersion, further improving the wettability, surface energy, and moisture resistance of the glass fibers. After coating the surface of the metal powder, the film layer will be more uniform and the filling performance will be significantly improved. After zirconium boride and aluminum nitride are added to the glass fibers for modification, the purpose of dispersion strengthening can be achieved, so that the mesh structure mainly composed of glass fibers still has higher strength and toughness during heating or pressing, avoiding the problem of increased loss due to damage to the insulating layer.

[0012] Preferably, the two aerosolized iron-nickel powders of different particle sizes are coarse iron-nickel powder and fine iron-nickel powder, the particle size D50 of the coarse iron-nickel powder is 15-25um, the particle size D50 of the fine iron-nickel powder is 4-6um; the particle size D50 of the carbonyl iron powder is 8-10um.

[0013] Beneficial effects: This application uses "coarse-grained iron-nickel powder + medium-grained carbonyl iron powder + fine-grained iron-nickel powder" as metal powder. When the carbonyl iron powder with an intermediate particle size is compressed, it produces a slight deformation, which increases the overall filling rate and density, increases the number of magnetic moments per unit volume, and achieves further improvement in the superposition performance under the condition of similar magnetic permeability; by using atomized iron-nickel powder and carbonyl iron powder with different particle sizes, the density of metal powder is increased, eddy current loss is reduced, and the power loss of soft magnetic composite metal materials is further reduced.

[0014] Preferably, the mass ratio of the coarse iron-nickel powder to the fine iron-nickel powder is 35-45:10-30.

[0015] Preferably, the mass of the γ-Fe2O3 is 0.2-0.6% of the metal powder, the mass of the magnesium acrylate is 0.05-0.1% of the metal powder, and the mass of the ammonia water is 0.08-0.1% of the metal powder.

[0016] Preferably, the mass of the glass fiber is 0.1-0.4%, the mass of the zirconium boride is 0.01-0.05% of the metal powder, the mass of the aluminum nitride is 0.02-0.04% of the metal powder, the mass of the silane coupling agent is 0.01-0.04% of the metal powder, and the mass of the carboxylated polyethylene wax is 0.01-0.05% of the metal powder.

[0017] Preferably, the aspect ratio of the glass fiber is (1.5-2):1, and the mesh size of the glass fiber is 5000 mesh.

[0018] Preferably, a passivator is also included, which is a mixed solution of aluminum chromium phosphate and aluminum dihydrogen phosphate, wherein the mass of the aluminum chromium phosphate is 0.3-0.8% of the metal powder, the mass of the aluminum dihydrogen phosphate is 0.2-0.6% of the metal powder, and the mass of water is 8-10% of the metal powder.

[0019] Preferably, the coating agent is also included, which is diphenyldichlorosilane, dialkylsilicyl dimelamine and a silane coupling agent dissolved in acetone, the mass of the diphenyldichlorosilane is 2.5-3.5% of the metal powder, the mass of the dialkylsilicyl dimelamine is 1-2% of the metal powder, and the mass of the silane coupling agent is 0.2-0.4% of the metal powder.

[0020] Preferably, a lubricant is also included, and the lubricant is a mixture of oxidized polyethylene wax and ethylene dioleyl amide, the mass of the oxidized polyethylene wax is 0.01-0.03% of the metal powder, and the mass of the ethylene dioleyl amide is 0.01-0.03% of the metal powder.

[0021] The second aspect of the present invention provides a method for preparing the above-mentioned soft magnetic composite metal material, comprising the following steps:

[0022] (1) mixing aerosolized iron-nickel powder of different particle sizes with carbonyl iron powder according to a mass ratio to obtain metal powder; adding the metal powder to a passivating agent, stirring, baking, and cooling to room temperature to obtain a passivated powder;

[0023] (2) Preparation of insulating agent: magnesium acrylate, ammonia water and γ-Fe2O3 are mixed, stirred, baked and cooled to room temperature to obtain modified γ-Fe2O3; glass fiber, zirconium boride, aluminum nitride, silane coupling agent and carboxylated polyethylene wax are mixed in anhydrous ethanol, stirred and heated continuously until the powder is dry and then cooled to room temperature to obtain modified glass fiber; then the modified γ-Fe2O3 and the modified glass fiber are mixed with water to obtain an insulating agent;

[0024] (3) adding the passivation powder to the insulating agent, stirring, baking, and cooling to room temperature to obtain insulating powder;

[0025] (4) Coating and granulation: adding the insulating powder to the coating agent, stirring evenly, granulating, and baking to obtain granulated powder;

[0026] (5) Lubrication and sieving: The lubricant is mixed with the granulated powder and sieved to obtain a soft magnetic composite metal material.

[0027] Preferably, in step (1), the stirring time is 15-25 min; the baking temperature is 120-150° C., and the baking time is 20-30 min.

[0028] Preferably, the mass of the anhydrous ethanol in step (2) is 3-5% of the metal powder, and the heating temperature is 50-60°C.

[0029] The advantages of the present invention are:

[0030] 1. The present invention uses "coarse-grained iron-nickel powder + medium-grained carbonyl iron powder + fine-grained iron-nickel powder" as metal powder. When the carbonyl iron powder with an intermediate particle size is compressed, it produces a slight deformation, which increases the overall filling rate and density, and increases the number of magnetic moments per unit volume, thereby achieving an improvement in the superposition performance of the soft magnetic composite metal material. Increasing the density of the metal powder can also reduce eddy current losses, thereby reducing the power loss of the soft magnetic composite metal material.

[0031] 2. γ-Fe2O3 is a magnetic iron oxide. Compared with the paramagnetism of other metal or non-metal oxides, the addition of γ-Fe2O3 can make up for the magnetic dilution effect caused by the addition of insulating coating, ensuring that the soft magnetic composite metal material has high superposition performance. And the unmodified γ-Fe2O3 has a large specific surface area and specific surface energy, is easy to agglomerate, and inhibits the performance of its ultrafine effect. After the modification of the present invention, the dispersibility of γ-Fe2O3 is improved, the dispersion will be more uniform, and the performance of the soft magnetic composite metal material is more uniform.

[0032] 3. Conventional glass fiber has strong silanol groups on its surface. After modification with a coupling agent in the present invention, the hydroxyl groups on the surface of the glass fiber condense with the hydrolyzate of silane. At the same time, the condensation between silanes converts the hydroxyl groups on the fiber surface with higher polarity into ether bonds with lower polarity. At the same time, carboxylated polyethylene wax is used to assist in dispersion, further improving the wettability, surface energy, and moisture resistance of the glass fiber. After coating the surface of the metal powder, the film layer will be more uniform and the filling performance will be significantly improved. After adding zirconium boride and aluminum nitride to the glass fiber for modification, the purpose of dispersion strengthening can be achieved, so that the mesh structure mainly composed of glass fiber still has high strength and toughness during heating or pressing, avoiding the problem of increased loss caused by the destruction of the insulating layer.

[0033] 4. The passivator of the present invention is a mixed solution of aluminum chromium phosphate and aluminum dihydrogen phosphate. During the passivation reaction, since the two are hydrolyzed into weak acid, the reaction is not violent and will not cause problems such as cracking of the film layer. In addition, during the passivation reaction, flocculent iron phosphate and smooth aluminum oxide and chromium oxide film layers are generated. Aluminum oxide and chromium oxide are attached to the iron phosphate, which improves the integrity of the film layer and achieves the uniformity of the film layer.

[0034] 5. Diphenyldichlorosilane and dialkylsilicyl dimelamine have high thermal stability, heat resistance, and even flame retardancy. Therefore, they can ensure that the one-piece molded inductor pressed by soft magnetic composite metal materials can maintain high reliability under continuous high-temperature working conditions without problems such as burning or spontaneous combustion.

[0035] 6. The melting points of oxidized polyethylene wax and ethylene dioleamide are around 110°C, and their microscopic morphology is spherical. The use of these two lubricants can lubricate the gaps between the powders. At the same time, during the pressing process of the one-piece molded inductor, a large friction force is generated between the mold and the mold, the powder and the powder, and the powder and the mold, causing the contact points to heat up rapidly, achieving rapid liquefaction and lubrication effects, thereby improving the density of the one-piece molded inductor. DETAILED DESCRIPTION

[0036] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0037] Unless otherwise specified, the test materials and reagents used in the following examples can be obtained from commercial sources.

[0038] If no specific techniques or conditions are specified in the examples, they can be carried out according to the techniques or conditions described in the literature in the art or according to the product instructions.

[0039] The present invention provides a soft magnetic composite metal material for an integrally formed inductor. The soft magnetic composite metal material comprises metal powder, a passivator, an insulating agent, a coating agent and a lubricant.

[0040] The metal powder is atomized iron-nickel powder and carbonyl iron powder. The atomized iron-nickel powder includes at least two iron-nickel powders with different particle sizes, specifically, the particle size D50 of the coarse iron-nickel powder is 15-25um, and the particle size D50 of the fine iron-nickel powder is 4-6um; the D50 of the carbonyl iron powder is 8-10um; the mass ratio of the coarse iron-nickel powder, carbonyl iron powder and fine iron-nickel powder is 35-45:35-45:10-30.

[0041] The passivator is a mixed solution of aluminum chromium phosphate and aluminum dihydrogen phosphate, wherein the mass of the aluminum chromium phosphate is 0.3-0.8% of the metal powder, the mass of the aluminum dihydrogen phosphate is 0.2-0.6% of the metal powder, and the water is 8-10% of the metal powder.

[0042] The insulating agent is a mixed solution of modified γ-Fe2O3 and modified glass fiber, and the mass of water is 8-10% of the metal powder.

[0043] The modified γ-Fe2O3 is prepared by modifying γ-Fe2O3 in magnesium acrylate and ammonia water; the mass of the γ-Fe2O3 is 0.2-0.6% of the metal powder, the mass of the magnesium acrylate is 0.05-0.1% of the metal powder, and the mass of the ammonia water is 0.08-0.1% of the metal powder.

[0044] The modified glass fiber is prepared by modifying the glass fiber in zirconium boride, aluminum nitride, silane coupling agent and carboxylated polyethylene wax; the mass of the glass fiber is 0.1-0.4% of the metal powder, the mass of the zirconium boride is 0.01-0.05% of the metal powder, the mass of the aluminum nitride is 0.02-0.04% of the metal powder, the mass of the silane coupling agent is 0.01-0.04% of the metal powder, and the mass of the carboxylated polyethylene wax is 0.01-0.05% of the metal powder.

[0045] The modified glass fiber is modified by using anhydrous ethanol as a solvent, the mass of the anhydrous ethanol is 3-5% of the metal powder, the aspect ratio of the glass fiber is (1.5-2):1, and the mesh number of the glass fiber is 5000 meshes.

[0046] The coating agent is diphenyldichlorosilane, dialkylsilicyl dimelamine and silane coupling agent dissolved in acetone, wherein the mass of the diphenyldichlorosilane is 2.5-3.5% of the metal powder, the mass of the dialkylsilicyl dimelamine is 1-2% of the metal powder, and the mass of the silane coupling agent is 0.2-0.4% of the metal powder.

[0047] The lubricant is a mixture of oxidized polyethylene wax and ethylene dioleyl amide, wherein the mass of the oxidized polyethylene wax is 0.01-0.03% of the metal powder, and the mass of the ethylene dioleyl amide is 0.01-0.03% of the metal powder.

[0048] Example 1

[0049] The present embodiment provides a method for preparing a soft magnetic composite metal material for an integrally formed inductor and a soft magnetic composite metal material, which specifically includes the following steps:

[0050] 1. Raw materials for preparing soft magnetic composite metal materials

[0051] Metal powder was obtained by mixing 35 g of atomized iron-nickel powder with D50=18 um, 35 g of carbonyl iron powder with D50=8 um, and 30 g of atomized iron-nickel powder with D50=4 um.

[0052] 0.4 g of aluminum chromium phosphate and 0.3 g of aluminum dihydrogen phosphate were dissolved in 8 g of water and stirred to obtain a passivating agent.

[0053] 0.06 g of magnesium acrylate, 0.08 g of ammonia water and 0.3 g of γ-Fe2O3 were mixed, stirred, dried and cooled to room temperature to obtain modified γ-Fe2O3;

[0054] 0.1 g of glass fiber with an aspect ratio of 1.5:1 and a mesh size of 5000, 0.01 g of zirconium boride, 0.02 g of aluminum nitride, 0.01 g of silane coupling agent, and 0.01 g of carboxylated polyethylene wax are dissolved in 3 g of anhydrous ethanol, stirred continuously, and heated at 50-60° C. until the powder is dry and then cooled to room temperature to obtain modified glass fiber; then the modified γ-Fe2O3 and the modified glass fiber are dissolved in 8 g of water and stirred to obtain an insulating agent.

[0055] 2.5 g of diphenyldichlorosilane, 1 g of dihydrocarbylsilicyl dimelamine and 0.2 g of a silane coupling agent were dissolved in 5 g of acetone and stirred to obtain a coating agent.

[0056] A lubricant was obtained by mixing 0.03 g of oxidized polyethylene wax and 0.01 g of ethylene dioleamide.

[0057] 2. Preparation of soft magnetic composite metal materials

[0058] The above-mentioned metal powder is added to a passivator, stirred for 15 minutes, baked at 120°C for 20 minutes, and cooled to room temperature to obtain a passivated powder; the passivated powder is then added to an insulating agent, stirred, dried, and cooled to room temperature to obtain an insulating powder; the insulating powder is added to a coating agent, stirred evenly, granulated, and dried to obtain a granulated powder; the granulated powder is mixed with a lubricant, and sieved through a 60-mesh sieve to obtain a soft magnetic composite metal material.

[0059] Example 2

[0060] The present embodiment provides a method for preparing a soft magnetic composite metal material for an integrally formed inductor and a soft magnetic composite metal material, which specifically includes the following steps:

[0061] 1. Raw materials for preparing soft magnetic composite metal materials

[0062] Metal powder was obtained by mixing 40 g of atomized iron-nickel powder with D50=18 um, 40 g of carbonyl iron powder with D50=8 um, and 20 g of atomized iron-nickel powder with D50=4 um.

[0063] 0.6 g of aluminum chromium phosphate and 0.4 g of aluminum dihydrogen phosphate were dissolved in 9 g of water and stirred to obtain a passivating agent.

[0064] 0.08 g of magnesium acrylate, 0.09 g of ammonia water and 0.5 g of γ-Fe2O3 were mixed, stirred, dried and cooled to room temperature to obtain modified γ-Fe2O3;

[0065] 0.2 g of glass fiber with an aspect ratio of 1.8:1 and a mesh size of 5000, 0.03 g of zirconium boride, 0.03 g of aluminum nitride, 0.02 g of a silane coupling agent, and 0.03 g of carboxylated polyethylene wax are dissolved in 4 g of anhydrous ethanol, stirred continuously, and heated at 50-60° C. until the powder is dry and then cooled to room temperature to obtain modified glass fiber; then the modified γ-Fe2O3 and the modified glass fiber are dissolved in 9 g of water and stirred to obtain an insulating agent.

[0066] 2.6 g of diphenyldichlorosilane, 1.5 g of dihydrocarbylsilicyl dimelamine and 0.3 g of a silane coupling agent were dissolved in 8 g of acetone and stirred to obtain a coating agent.

[0067] A lubricant was obtained by mixing 0.02 g of oxidized polyethylene wax and 0.01 g of ethylene dioleamide.

[0068] 2. Preparation of soft magnetic composite metal materials

[0069] The above-mentioned metal powder is added to a passivator, stirred for 20 minutes, baked at 120°C for 20 minutes, and cooled to room temperature to obtain a passivated powder; the passivated powder is then added to an insulating agent, stirred, dried, and cooled to room temperature to obtain an insulating powder; the insulating powder is added to a coating agent, stirred evenly, granulated, and dried to obtain a granulated powder; the granulated powder is mixed with a lubricant, and sieved through a 100-mesh sieve to obtain a soft magnetic composite metal material.

[0070] Example 3

[0071] The present embodiment provides a method for preparing a soft magnetic composite metal material for an integrally formed inductor and a soft magnetic composite metal material, which specifically includes the following steps:

[0072] 1. Raw materials for preparing soft magnetic composite metal materials

[0073] Metal powder was obtained by mixing 45 g of atomized iron-nickel powder with D50=18 um, 35 g of carbonyl iron powder with D50=8 um, and 20 g of atomized iron-nickel powder with D50=4 um.

[0074] 0.8 g of chromium aluminum phosphate and 0.5 g of aluminum dihydrogen phosphate were dissolved in 10 g of water and stirred to obtain a passivating agent.

[0075] 0.09 g of magnesium acrylate, 0.1 g of ammonia water and 0.6 g of γ-Fe2O3 were mixed, stirred, dried and cooled to room temperature to obtain modified γ-Fe2O3;

[0076] 0.3 g of glass fiber with an aspect ratio of 2:1 and a mesh size of 5000, 0.04 g of zirconium boride, 0.04 g of aluminum nitride, 0.03 g of a silane coupling agent, and 0.05 g of carboxylated polyethylene wax are dissolved in 4 g of anhydrous ethanol, stirred continuously, and heated at 50-60° C. until the powder is dry and then cooled to room temperature to obtain modified glass fiber; then the modified γ-Fe2O3 and the modified glass fiber are dissolved in 9 g of water and stirred to obtain an insulating agent.

[0077] 3 g of diphenyldichlorosilane, 2 g of dihydrocarbylsilicyl dimelamine and 0.4 g of a silane coupling agent were dissolved in 10 g of acetone and stirred to obtain a coating agent.

[0078] A lubricant was obtained by mixing 0.01 g of oxidized polyethylene wax and 0.03 g of ethylene dioleamide.

[0079] 2. Preparation of soft magnetic composite metal materials

[0080] The above-mentioned metal powder is added to a passivator, stirred for 25 minutes, baked at 150°C for 30 minutes, and cooled to room temperature to obtain a passivated powder; the passivated powder is then added to an insulating agent, stirred, dried, and cooled to room temperature to obtain an insulating powder; the insulating powder is added to a coating agent, stirred evenly, granulated, and dried to obtain a granulated powder; the granulated powder is mixed with a lubricant, and sieved through a 200-mesh sieve to obtain a soft magnetic composite metal material.

[0081] Comparative Example 1

[0082] This comparative example provides a method for preparing a soft magnetic composite metal material for an integrally formed inductor and a soft magnetic composite metal material. The difference between this comparative example and Example 1 is that the metal powder is 100 g of carbonyl iron powder with D50=8 um.

[0083] Comparative Example 2

[0084] This comparative example provides a method for preparing a soft magnetic composite metal material for an integrally formed inductor and a soft magnetic composite metal material. The difference between this comparative example and Example 1 is that the metal powder is 100 g of an iron-silicon-chromium alloy powder with D50=18 um.

[0085] Comparative Example 3

[0086] This comparative example provides a method for preparing a soft magnetic composite metal material for an integrally formed inductor and a soft magnetic composite metal material. The difference between this comparative example and Example 1 is that the passivating agent is obtained by dissolving 0.7 g of phosphoric acid in 8 g of water and stirring.

[0087] Comparative Example 4

[0088] This comparative example provides a method for preparing a soft magnetic composite metal material for an integrally formed inductor and a soft magnetic composite metal material. The difference between this comparative example and Example 1 is that: no modified γ-Fe2O3 is added to the insulating agent.

[0089] Comparative Example 5

[0090] This comparative example provides a method for preparing a soft magnetic composite metal material for an integrally formed inductor and a soft magnetic composite metal material. The difference between this comparative example and Example 1 is that: no modified glass fiber is added to the insulating agent.

[0091] Comparative Example 6

[0092] This comparative example provides a method for preparing a soft magnetic composite metal material for an integrally molded inductor and a soft magnetic composite metal material. The difference between this comparative example and Example 1 is that the coating agent is 3.5g of epoxy resin and 0.2g of diethylenetriamine dissolved in 5g of acetone and stirred.

[0093] Comparative Example 7

[0094] This comparative example provides a method for preparing a soft magnetic composite metal material for an integrally molded inductor and a soft magnetic composite metal material. The difference between this comparative example and Example 2 is that the metal powder is obtained by mixing 60g of atomized iron-nickel powder with D50=18um and 40g of carbonyl iron powder with D50=8um.

[0095] Comparative Example 8

[0096] This comparative example provides a method for preparing a soft magnetic composite metal material for an integrally molded inductor and a soft magnetic composite metal material. The difference between this comparative example and Example 2 is that the γ-Fe2O3 in the insulating agent is not modified and is in a naturally agglomerated state.

[0097] Comparative Example 9

[0098] This comparative example provides a method for preparing a soft magnetic composite metal material for an integrally molded inductor and a soft magnetic composite metal material. The difference between this comparative example and Example 2 is that the glass fiber in the insulating agent is not modified and is in a naturally stacked state.

[0099] Comparative Example 10

[0100] This comparative example provides a method for preparing a soft magnetic composite metal material for an integrally molded inductor and a soft magnetic composite metal material. The difference between this comparative example and Example 2 is that the coating agent is obtained by dissolving 2.6 g of diphenyldichlorosilane, 1.5 g of silicone resin and 0.3 g of silane coupling agent in 8 g of acetone and stirring.

[0101] Comparative Example 11

[0102] This comparative example provides a method for preparing a soft magnetic composite metal material for an integrally formed inductor and a soft magnetic composite metal material. The difference between this comparative example and Example 2 is that the lubricant is 0.03 g of zinc stearate.

[0103] Comparative Example 12

[0104] This comparative example provides a method for preparing a soft magnetic composite metal material for an integrally formed inductor and a soft magnetic composite metal material. The difference between this comparative example and Example 2 is that the lubricant is 0.03 g of magnesium stearate.

[0105] Comparative Example 13

[0106] This comparative example provides a method for preparing a soft magnetic composite metal material for an integrally molded inductor and a soft magnetic composite metal material. The difference between this comparative example and Example 3 is that the metal powder is obtained by mixing 45g of water-atomized iron-nickel powder with D50=18um, 35g of carbonyl iron powder with D50=8um and 20g of water-atomized iron-nickel powder with D50=4um.

[0107] Comparative Example 14

[0108] This comparative example provides a method for preparing a soft magnetic composite metal material for an integrally formed inductor and a soft magnetic composite metal material. The difference between this comparative example and Example 3 is that the passivator is obtained by dissolving 1.3 g of aluminum dihydrogen phosphate in 10 g of water and stirring.

[0109] Comparative Example 15

[0110] This comparative example provides a method for preparing a soft magnetic composite metal material for an integrally formed inductor and a soft magnetic composite metal material. The difference between this comparative example and Example 3 is that the γ-Fe2O3 in the insulating agent is replaced by Fe3O4.

[0111] Experimental Example: The soft magnetic composite metal materials obtained in Examples 1-3 and Comparative Examples 1-15 were treated with 6t / cm 2 The magnetic ring with an outer diameter of 14.00mm, an inner diameter of 8.00mm and a height of 3.5±0.2mm was pressed with a pressure. After drying, the magnetic ring was wrapped into a coil. The inductance value of the magnetic ring was tested using WK6500BLCR tester and the inductance value under the superposition condition of 100Oe.

[0112] According to the formula μe=(L*Le) / (4*3.14*Ae*N 2 ) Calculate the effective magnetic permeability of the magnetic ring, where μe: effective magnetic permeability, L: inductance (μH), Le: effective magnetic path length (mm), Ae: effective cross-sectional area (mm 2), N: number of coil turns, and finally the magnetic ring loss is tested. The characteristic test results of Examples 1-3 and Comparative Examples 1-15 are shown in Table 1 below.

[0113] Table 1: Test results of properties of Examples 1-3 and Comparative Examples 1-15

[0114]

[0115] Compared with Comparative Example 1, the power loss of Example 1 of the present invention has obvious advantages. The present invention utilizes the advantage of low impurity content of atomized iron-nickel powder and carbonyl iron powder to maintain low hysteresis loss, and then utilizes atomized iron-nickel powder and carbonyl iron powder of different particle sizes to increase material density to reduce eddy current loss. Therefore, the power loss of Example 1 is low.

[0116] Compared with Comparative Example 2, Example 1 has obvious advantages in superposition performance when the effective magnetic permeabilities are similar. The present invention uses "coarse-grained iron-nickel powder + medium-grained carbonyl iron powder + fine-grained iron-nickel powder" as metal powder. When the carbonyl iron powder with intermediate grains is compressed, it produces a slight deformation, which improves the overall filling rate and density, and can achieve an increase in the number of magnetic moments per unit volume. Therefore, the superposition performance of Example 1 is significantly better.

[0117] Comparing Example 1 with Comparative Examples 3-6, there is no obvious change in the superposition performance when the effective permeability is similar. However, since the passivation agent, insulating agent, and coating agent of Example 1 and Comparative Examples 3-6 are changed, the power loss is very different. Therefore, it is difficult to achieve the purpose of low loss by conventional passivation, insulation, and coating processes.

[0118] Compared with Example 7, the stacking performance and power loss of Example 7 are reduced. Although Example 7 mixes aerosolized iron-nickel powder and carbonyl iron powder of two different particle sizes, the overall filling rate and density need to be improved, so the performance is slightly worse than that of Example 2.

[0119] Compared with comparative examples 8-12, Example 2 shows that the materials prepared by passivation, insulation, coating and lubrication processes of the metal powder used in the present invention have the best superposition performance and power loss when the magnetic permeabilities are similar.

[0120] Compared with Example 3 and Comparative Example 13, Comparative Example 13 also uses "coarse-grained iron-nickel powder + medium-grained carbonyl iron powder + fine-grained iron-nickel powder" as metal powder, but the types of iron-nickel powder are different. Since the iron-nickel powder obtained by water atomization has irregular shapes, the overall filling rate and density of the metal powder are poorer than those of Example 3. Compared with gas-atomized iron-nickel powder, water-atomized iron-nickel powder has more impurities. Therefore, the stacking performance and power loss of Comparative Example 13 are reduced.

[0121] Compared with Example 3 and Comparative Examples 14-15, the materials prepared from the metal powder used in the present invention after passivation, insulation, coating and lubrication processes have the best superposition performance and power loss in Example 3 when the magnetic permeabilities are similar.

[0122] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A soft magnetic composite metal material for integrally formed inductors, characterized in that: Includes metal powder and insulating agent; The metal powder is atomized iron-nickel powder and carbonyl iron powder, the atomized iron-nickel powder and the carbonyl iron powder are mixed in a mass ratio of 55-65:35-45, and the atomized iron-nickel powder is at least two atomized iron-nickel powders with different particle sizes; The insulating agent is a mixed solution of modified γ-Fe2O3 and modified glass fiber, and the water mass is 8-10% of the metal powder; the modified γ-Fe2O3 is obtained by modifying γ-Fe2O3 in magnesium acrylate and ammonia water; the modified glass fiber is obtained by modifying glass fiber in zirconium boride, aluminum nitride, silane coupling agent and carboxylated polyethylene wax.

2. The soft magnetic composite metal material according to claim 1, characterized in that: The two aerosolized iron-nickel powders with different particle sizes are coarse iron-nickel powder and fine iron-nickel powder. The particle size D50 of the coarse iron-nickel powder is 15-25um, and the particle size D50 of the fine iron-nickel powder is 4-6um; the particle size D50 of the carbonyl iron powder is 8-10um.

3. The soft magnetic composite metal material according to claim 2, characterized in that: The mass ratio of the coarse iron-nickel powder to the fine iron-nickel powder is 35-45:10-30.

4. The soft magnetic composite metal material according to claim 1, characterized in that: The mass of the γ-Fe2O3 is 0.2-0.6% of the metal powder, the mass of the magnesium acrylate is 0.05-0.1% of the metal powder, and the mass of the ammonia water is 0.08-0.1% of the metal powder; the mass of the glass fiber is 0.1-0.4%, the mass of the zirconium boride is 0.01-0.05% of the metal powder, the mass of the aluminum nitride is 0.02-0.04% of the metal powder, the mass of the silane coupling agent is 0.01-0.04% of the metal powder, and the mass of the carboxylated polyethylene wax is 0.01-0.05% of the metal powder.

5. The soft magnetic composite metal material according to claim 1, characterized in that: It also includes a passivator, which is a mixed solution of aluminum chromium phosphate and aluminum dihydrogen phosphate. The mass of the aluminum chromium phosphate is 0.3-0.8% of the metal powder, the mass of the aluminum dihydrogen phosphate is 0.2-0.6% of the metal powder, and water is 8-10% of the metal powder.

6. The soft magnetic composite metal material according to claim 5, characterized in that: The invention also comprises a coating agent, which is diphenyldichlorosilane, dialkylsilicyl dimelamine and a silane coupling agent dissolved in acetone, wherein the mass of the diphenyldichlorosilane is 2.5-3.5% of the metal powder, the mass of the dialkylsilicyl dimelamine is 1-2% of the metal powder, and the mass of the silane coupling agent is 0.2-0.4% of the metal powder.

7. The soft magnetic composite metal material according to claim 6, characterized in that: The invention also comprises a lubricant, which is a mixture of oxidized polyethylene wax and ethylene dioleyl amide. The weight of the oxidized polyethylene wax is 0.01-0.03% of the metal powder, and the weight of the ethylene dioleyl amide is 0.01-0.03% of the metal powder.

8. The method for preparing a soft magnetic composite metal material according to any one of claims 1 to 7, characterized in that: The following steps are involved: (1) mixing aerosolized iron-nickel powder of different particle sizes with carbonyl iron powder according to a mass ratio to obtain metal powder; adding the metal powder to a passivating agent, stirring, baking, and cooling to room temperature to obtain a passivated powder; (2) Preparation of insulating agent: magnesium acrylate, ammonia water and γ-Fe2O3 are mixed, stirred, baked and cooled to room temperature to obtain modified γ-Fe2O3; glass fiber, zirconium boride, aluminum nitride, silane coupling agent and carboxylated polyethylene wax are mixed in anhydrous ethanol, stirred and heated continuously until the powder is dry and then cooled to room temperature to obtain modified glass fiber; then the modified γ-Fe2O3 and the modified glass fiber are mixed with water to obtain an insulating agent; (3) adding the passivation powder to the insulating agent, stirring, baking, and cooling to room temperature to obtain insulating powder; (4) Coating and granulation: adding the insulating powder to the coating agent, stirring evenly, granulating, and baking to obtain granulated powder; (5) Lubrication and sieving: The lubricant is mixed with the granulated powder and sieved to obtain a soft magnetic composite metal material.

9. The method for preparing a soft magnetic composite metal material according to claim 8, characterized in that: The stirring time in step (1) is 15-25 minutes; the baking temperature is 120-150° C., and the baking time is 20-30 minutes.

10. The method for preparing a soft magnetic composite metal material according to claim 8, characterized in that: In the step (2), the mass of the anhydrous ethanol is 3-5% of the metal powder, and the heating temperature is 50-60°C.

Citation Information

Cited By

  • Loss characteristic negative temperature coefficient integrated inductor and preparation method thereof

    CN119252644A

  • One-piece molded inductor with negative temperature coefficient of loss characteristics and preparation method thereof

    CN119252644B

  • Preparation method of composite magnetic powder core of iron-nickel doped carbonyl iron powder

    CN119786239A

  • Soft magnetic composite powder material for integrally-formed inductor and preparation method and device of soft magnetic composite powder material

    CN121662582A