Semiconductor structure and preparation method
Through ion beam deposition technology, the sputtering ion source and the auxiliary ion source are used to form an adhesive barrier layer and a seed layer on the inner wall of the trench, which solves the problems of low coverage and low deposition speed in the existing technology, and achieves high quality and high Trench fill for step coverage.
Patent Information
- Application Number
- CN202310380302.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-11
- Publication Date
- 2024-10-18
AI Technical Summary
The existing technology has challenges in preparing trench adhesion barrier layers and seed layers with high purity and high step coverage. The traditional magnetron sputtering process has low coverage, the ALD deposition rate is low, and the metal purity and performance are poor.
The sputtering ion source and auxiliary ion source of the ion beam deposition equipment are used to bombard the target with neutral ion beams to generate sputtering particles and change their incident direction to form an adhesion barrier layer and seed layer on the inner wall of the trench. The auxiliary ion source The angle with the normal direction of the substrate surface is an acute angle, which guides the sputtered particles to be incident along a certain angle to improve the step coverage and conformality.
The preparation of trench adhesion barrier layer and seed layer with high quality and high step coverage is achieved, which improves device performance and avoids the problems of trench top overhang and incomplete bottom filling.
Smart Images

Figure CN118800720A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of semiconductor technology, and in particular to a semiconductor structure and a preparation method thereof. Background Art
[0002] As the size of integrated circuit devices continues to shrink, their manufacturing process requirements are also facing major challenges. In the back-end copper interconnect and back gate wire connection, as the device size shrinks, the size of the through hole becomes smaller and smaller, and the aspect ratio becomes higher and higher. Uniform and void-free trench filling adhesion barrier layer and seed layer is a very important challenge in the existing integrated circuit manufacturing technology.
[0003] In conventional technology, people have always used magnetron sputtering, a PVD (Physical Vapor Deposition) technology to fill conventional trench adhesion barrier layers and seed layers. The step coverage of the film deposited in the trench by the traditional magnetron sputtering process is not high, and the overhang at the top of the trench will seriously affect the quality of subsequent electroplating, resulting in the inability to fill the bottom, thereby affecting the performance of the entire device.
[0004] The failure rate of ALD (Atomic layer deposition) metal deposition is very high and the purity and performance of the deposited metal are poor. It is also limited by the separation of the precursors and the ALD deposition rate is very low. Therefore, there are still great challenges in preparing high-purity, high-step coverage trench adhesion layers and seed layers. Summary of the invention
[0005] In view of this, this summary of the invention is provided to introduce the concepts in a brief form, which will be described in detail in the detailed description section below. This summary of the invention is not intended to identify the key features or essential features of the technical solution claimed for protection, nor is it intended to be used to limit the scope of the technical solution claimed for protection.
[0006] The purpose of the present application is to provide a semiconductor structure and a preparation method, which can prepare a trench adhesion barrier layer and a seed layer with high quality and high step coverage.
[0007] To achieve the above purpose, this application has the following technical solutions:
[0008] In a first aspect, an embodiment of the present application provides a method for preparing a semiconductor structure, comprising:
[0009] Step 1, providing a substrate with grooves;
[0010] Step 2: bombarding the first target material with a neutral ion beam generated by a sputtering ion source of an ion beam deposition device to generate first sputtered particles;
[0011] Step 3: using a neutral ion beam generated by an auxiliary ion source of the ion beam deposition device to change the incident direction of the first sputtered particles, so as to form an adhesion barrier layer on the inner wall of the groove;
[0012] Step 4: bombarding a second target material with the neutral ion beam generated by the sputtering ion source to generate second sputtered particles;
[0013] Step 5: Using the neutral ion beam generated by the auxiliary ion source, change the incident direction of the second sputtered particles to form a seed layer on the inner wall of the groove; the angle between the auxiliary ion source and the normal of the substrate surface is an acute angle.
[0014] In a possible implementation, providing a substrate with grooves includes:
[0015] providing an initial substrate;
[0016] Depositing a hard mask on the initial substrate to define structured regions by photolithography;
[0017] The initial substrate in the structure area is etched to form the substrate with grooves.
[0018] In a possible implementation manner, the opening width of the groove is equal to the bottom width of the groove.
[0019] In a possible implementation manner, the opening width of the groove is greater than the bottom width of the groove.
[0020] In a possible implementation, forming an adhesion barrier layer on an inner wall of the groove includes: forming an adhesion barrier layer on a side wall of the groove;
[0021] Forming a seed layer on the inner wall of the trench includes: forming a seed layer on the side wall of the trench.
[0022] In a possible implementation, after providing the substrate with grooves and before bombarding the first target material with a neutral ion beam generated by a sputtering ion source of an ion beam deposition device to generate first sputtered particles, the method further includes:
[0023] The groove is pre-cleaned by using a neutral ion beam generated by the auxiliary ion source to remove impurities on the surface of the groove.
[0024] In a possible implementation manner, during the forming of the adhesion barrier layer and the forming of the seed layer, the substrate is controlled to maintain self-rotation.
[0025] In a possible implementation, the neutral ion beam of the sputtering ion source includes: an ion beam formed by any one or more inert gases of He, Ne, Ar, Kr and Xe.
[0026] In a possible implementation, the neutral ion beam used by the auxiliary ion source includes: an ion beam formed by one or more inert gases.
[0027] In a possible implementation, the ion beam used by the auxiliary ion source includes a mixed gas of one or more inert gases and nitrogen.
[0028] In a possible implementation, the material of the adhesion barrier layer includes: one or more of titanium, tantalum, titanium nitride and tantalum nitride. In a possible implementation, the material of the seed layer includes: one or more of aluminum, copper and tungsten.
[0029] In a possible implementation, the aspect ratio of the trench is in the range of [2:1, 15:1].
[0030] In a possible implementation manner, the purity of the first target material and the second target material is greater than or equal to 99.9% and less than or equal to 99.9999%.
[0031] In a possible implementation, an angle between the auxiliary ion source and the normal direction of the substrate surface is greater than 0° and less than or equal to 30°.
[0032] In a possible implementation, the rotation speed range of the self-rotation is greater than or equal to 5 rpm and less than or equal to 200 rpm.
[0033] In a possible implementation manner, the thickness of the adhesion barrier layer is greater than or equal to 2 nm and less than or equal to 100 nm.
[0034] In a possible implementation, the thickness of the seed layer is greater than or equal to 2 nm and less than or equal to 100 nm.
[0035] In a possible implementation, the grid of the sputtering ion source is in an arc shape to focus the ion beam onto the target surface, and the radius of the arc is greater than or equal to 300 mm and less than or equal to 800 mm. In a possible implementation, the grid of the sputtering ion source is in a plane shape, and the grid is provided with a plurality of through holes, and the coverage range of the plurality of through holes is [0.25 times, 0.75 times] the area of the first target or the second target.
[0036] In a possible implementation manner, a deposition rate of the adhesion barrier layer is greater than or equal to 3 nm / min and less than or equal to 30 nm / min.
[0037] In a possible implementation, a deposition rate of the seed layer is greater than or equal to 3 nm / min and less than or equal to 30 nm / min.
[0038] In a possible implementation, the sample temperature for depositing the first target material is [50° C., 300° C.], and the sample temperature for depositing the second target material is (0° C., 100° C.].
[0039] In a second aspect, an embodiment of the present application provides a semiconductor structure, including a structure prepared using the method described above.
[0040] Compared with the prior art, the embodiments of the present application have the following beneficial effects:
[0041] The embodiment of the present application provides a semiconductor structure and a preparation method, the method comprising: providing a substrate with grooves; a neutral ion beam generated by a sputtering ion source of an ion beam deposition device bombards a first target material to generate first sputtering particles; a neutral ion beam generated by an auxiliary ion source of the ion beam deposition device changes the incident direction of the first sputtering particles to form an adhesion barrier layer on the inner wall of the groove; a neutral ion beam generated by the sputtering ion source bombards a second target material to generate second sputtering particles; a neutral ion beam generated by the auxiliary ion source changes the incident direction of the second sputtering particles to form a seed layer on the inner wall of the groove; the auxiliary ion source and the substrate surface normal angle are acute. Through ion beam deposition, the sputtering particles can be guided to be incident at a certain angle so that the sputtering particles can better enter the bottom of the groove and achieve better step coverage and conformality. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0043] Figure 1 A schematic diagram of a conventional trench structure is shown;
[0044] Figure 2 A flow chart showing a method for preparing a semiconductor structure provided in an embodiment of the present application is shown;
[0045] Figure 3 A schematic diagram showing a structure in a preparation process of a semiconductor structure provided in an embodiment of the present application;
[0046] Figure 4 A schematic diagram of an ion beam deposition device provided in an embodiment of the present application is shown;
[0047] Figure 5 A schematic diagram showing a structure in a preparation process of another semiconductor structure provided in an embodiment of the present application is shown;
[0048] Figure 6 A schematic diagram of a semiconductor structure provided by an embodiment of the present application is shown;
[0049] Figure 7 A schematic diagram of a grid structure in a sputtering ion source provided in an embodiment of the present application is shown;
[0050] Figure 8 A schematic diagram of another grid structure in a sputtering ion source provided in an embodiment of the present application is shown;
[0051] Fig. 9 A schematic diagram of another semiconductor structure provided by an embodiment of the present application is shown;
[0052] Fig.10 A schematic diagram of another semiconductor structure provided in an embodiment of the present application is shown. DETAILED DESCRIPTION
[0053] In order to make the above-mentioned objects, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are described in detail below with reference to the accompanying drawings.
[0054] In the following description, many specific details are set forth to facilitate a full understanding of the present application, but the present application may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present application. Therefore, the present application is not limited to the specific embodiments disclosed below.
[0055] As described in the background technology, the applicant has found through research that an integrated circuit (IC) often includes millions of electronic devices. With the development of technology and the continuous improvement of application requirements, integrated circuits are developing towards miniaturization, multi-layering, flattening and thinning. Ultra-large-scale integrated circuit trench filling is an important link in three-dimensional integrated circuits.
[0056] As the size of integrated circuit devices continues to shrink, their manufacturing process requirements are also facing major challenges. In the back-end copper interconnect and back gate wire connection, as the device size shrinks, the size of the through hole becomes smaller and smaller, and the aspect ratio becomes higher and higher. Uniform and void-free trench filling adhesion barrier layer and seed layer is a very important challenge in the existing integrated circuit manufacturing technology.
[0057] In conventional technology, people have always used magnetron sputtering, a PVD (Physical Vapor Deposition) technology to fill conventional trench adhesion barrier layers and seed layers. The conventional magnetron sputtering process does not have high step coverage of the film deposited in the trench, for example, see Figure 1 As shown, it is a schematic diagram of a traditional groove structure, including a substrate 1, a groove 5 formed by etching the substrate 1, and a seed layer 3 formed on the inner wall of the groove 5. The overhang 4 of the seed layer 3 at the top of the groove 5 will seriously affect the quality of subsequent electroplating, resulting in the inability to fill the bottom, thereby affecting the performance of the entire device.
[0058] Although the new type of magnetron sputtering IMP (Ion Metal Plasma) improves the step coverage of the groove, the M + (charged metal particles) and Ar + At the same time, the magnetic field on the target and the magnetic field generated by the coil on the wafer cannot distinguish the M + and Ar + , which will affect the deposition effect. In addition, applying a negative bias on the sample surface will also attract M + with Ar + , cannot be screened, Ar + It will cause secondary sputtering of the film. Although ALD (Atomic layer deposition) has a good step coverage, the failure rate of deposited metal is very high and the purity and performance of the deposited metal are poor. It is also limited by the separation of the precursor, and the ALD deposition rate is very low. Therefore, there are still great challenges in preparing high-purity, high-step coverage groove adhesion layers and seed layers.
[0059] How to prepare a trench adhesion barrier layer and a seed layer with high quality and high step coverage is a technical problem that needs to be solved in this field.
[0060] Based on the above technical problems, the embodiment of the present application provides a semiconductor structure and a preparation method, which includes: providing a substrate with grooves; a neutral ion beam generated by a sputtering ion source of an ion beam deposition device bombards a first target material to generate first sputtering particles; a neutral ion beam generated by an auxiliary ion source of the ion beam deposition device changes the incident direction of the first sputtering particles to form an adhesion barrier layer on the inner wall of the groove; a neutral ion beam generated by the sputtering ion source bombards a second target material to generate second sputtering particles; a neutral ion beam generated by the auxiliary ion source changes the incident direction of the second sputtering particles to form a seed layer on the inner wall of the groove; the angle between the auxiliary ion source and the substrate surface normal is an acute angle. Through ion beam deposition, the sputtering particles can be guided to be incident at a certain angle so that the sputtering particles can better enter the bottom of the groove and achieve better step coverage and conformality.
[0061] In order to better understand the technical solution and technical effects of the present application, specific embodiments will be described in detail below with reference to the accompanying drawings.
[0062] Exemplary Methods
[0063] See also Figure 2 As shown, Figure 2 A flowchart of a method for preparing a semiconductor structure provided in an embodiment of the present application includes:
[0064] S101: Providing a substrate with grooves
[0065] In the examples of this application, see Figure 3 As shown, it is a schematic diagram of a structure in the preparation process of a semiconductor structure provided in an embodiment of the present application. The substrate 1 with grooves can be a semiconductor substrate, for example, it can be a Si substrate, a Ge substrate, a SiGe substrate, SOI (Silicon On Insulator) or GOI (Germanium On Insulator), etc. In other embodiments, the semiconductor substrate can also be a substrate including other element semiconductors or compound semiconductors, such as GaAs, InP or SiC, etc., and can also be a stacked structure, such as Si / SiGe, etc., and can also be other epitaxial structures, such as SGOI (Silicon Germanium On Insulator), etc. In a possible implementation, the substrate 1 with grooves provided in an embodiment of the present application can be obtained specifically by the following steps:
[0066] An initial substrate is provided, a hard mask is deposited on the initial substrate, a structure region is defined by photolithography, and the initial substrate in the structure region is etched to form a substrate 1 with grooves.
[0067] Optionally, the hard mask may be made of an insulating material, for example, may include at least one of a silicon oxide layer, a silicon nitride layer and a silicon oxynitride layer. Optionally, in this embodiment, the hard mask is a silicon oxide layer.
[0068] In order to form a subsequent interconnection structure or other structures, the embodiment of the present application can etch the initial substrate to form a groove 5, and the groove 5 is etched along the thickness direction of the initial substrate.
[0069] S102: bombarding a first target material with a neutral ion beam generated by a sputtering ion source of an ion beam deposition device to generate first sputtered particles.
[0070] S103: using a neutral ion beam generated by an auxiliary ion source of the ion beam deposition device to change the incident direction of the first sputtered particles, so as to form an adhesion barrier layer on the inner wall of the groove.
[0071] In the examples of this application, see Figure 4 Shown is a schematic diagram of an ion beam deposition device provided in an embodiment of the present application.
[0072] The ion beam deposition device provided in the embodiment of the present application may include a sputtering ion source 10 . The neutral ion beam generated by the sputtering ion source 10 of the ion beam deposition device may be used to bombard a first target material 11 to generate first sputtered particles.
[0073] For example, the sputtering ion source 10 and the first target 11 can be placed opposite to each other, the direction of the neutral ion beam generated by the sputtering ion source 10 can be as shown by arrow A in the figure, and the direction of the first sputtering particles generated after bombarding the first target 11 can be as shown by arrow B in the figure.
[0074] Combination Figure 4 and Figure 5 As shown, Figure 5 A schematic diagram of a structure during the preparation process of another semiconductor structure provided in an embodiment of the present application.
[0075] The ion beam deposition device provided in the embodiment of the present application may further include an auxiliary ion source 12. The neutral ion beam generated by the auxiliary ion source 12 of the ion beam deposition device may be used to change the incident direction of the first sputtered particles to form an adhesion barrier layer 6 on the inner wall of the groove 5 and the substrate 1 with the groove 5.
[0076] Therefore, the present application can guide the first sputtered particles to be incident along a certain angle through the auxiliary ion source 12, so that the first sputtered particles can better enter the bottom of the groove 5, achieve better step coverage and conformality, and prepare a groove adhesion barrier layer 6 with high quality and high step coverage.
[0077] The embodiment of the present application can prevent the subsequent sputtered material from diffusing into the substrate 1 with the groove 5 by means of the adhesion barrier layer 6, and can also prevent the impurities in the substrate 1 with the groove 5 from diffusing into the film layer structure deposited subsequently.
[0078] S104: bombarding a second target material with the neutral ion beam generated by the sputtering ion source to generate second sputtering particles;
[0079] S105: using the neutral ion beam generated by the auxiliary ion source to change the incident direction of the second sputtered particles, so as to form a seed layer on the inner wall of the groove; the angle between the auxiliary ion source and the normal of the substrate surface is an acute angle.
[0080] In the examples of this application, see Figure 4 As shown, the second target material 22 can be bombarded with a neutral ion beam generated by the sputtering ion source 10 to generate second sputtered particles.
[0081] That is, after depositing the adhesion barrier layer 6 in the embodiment of the present application, the neutral ion beam generated by the sputtering ion source 10 can be used to bombard the second target material 22 to generate second sputtered particles, and the second sputtered particles can be used to deposit and form the seed layer 7.
[0082] Specifically, in order to enable the second sputtered particles to better enter the bottom of the groove 5 to achieve a high step coverage, the auxiliary ion source 12 can be used to further control the direction of the second sputtered particles.
[0083] That is, in the embodiments of the present application, see Figure 4 and Figure 6 As shown, Figure 6 A schematic diagram of a semiconductor structure provided for an embodiment of the present application can utilize a neutral ion beam generated by an auxiliary ion source 12 to change the incident direction of the second sputtered particles so as to form a seed layer 7 on the inner wall of the groove 5 and the side of the adhesion barrier layer 6 away from the substrate 1; the angle C between the auxiliary ion source 12 and the surface normal of the substrate 1 is an acute angle.
[0084] Therefore, the present application can guide the second sputtered particles to be incident along a certain angle through the auxiliary ion source 12, so that the second sputtered particles can better enter the bottom of the groove 5, achieve better step coverage and conformality, and prepare a groove seed layer 7 with high quality and high step coverage.
[0085] In a possible implementation, after providing the substrate 1 with the groove 5, before bombarding the first target material 11 with a neutral ion beam generated by a sputtering ion source 10 of an ion beam deposition device to generate first sputtered particles, the method provided in the embodiment of the present application may further include:
[0086] The trench 5 is pre-cleaned using a neutral ion beam generated by the auxiliary ion source 12 to remove impurities on the surface of the trench 5 .
[0087] That is, in the embodiment of the present application, before preparing the two thin films of the adhesion barrier layer 6 and the seed layer 7, the groove 5 can first be pre-cleaned using the auxiliary ion source 12 of the ion beam deposition equipment (IBD, Ion Beam Deposition). This process can remove dirt and oxide layers on the surface of the groove 5, increase the adhesion of subsequent film layers, save transmission time and the risk of oxidation. This process can be cleaned in the same chamber, eliminating one chamber.
[0088] In a possible implementation, in the embodiment of the present application, when the adhesion barrier layer 6 and the seed layer 7 are formed, the substrate 1 can be controlled to keep rotating.
[0089] The substrate 1 and the film layer thereon provided in the embodiment of the present application maintain self-rotation during the deposition process, so that the particles can be evenly deposited on the sidewalls and bottom of the groove 5 to ensure the integrity of the filling of the groove 5 and achieve full filling of the groove 5 without holes.
[0090] The ion beam deposition method provided in the embodiment of the present application is used to fill the groove. Ion beam deposition is a type of physical vapor deposition (PVD). Through the grid of the ion source, a wide beam of ions can be drawn. High-energy ions bombard the surface of the target material, sputtering material particles, and depositing them on the surface of the sample sheet, growing a suitable film layer on the sample.
[0091] In a possible implementation, the neutral ion beam of the sputtering ion source 10 provided in the embodiment of the present application may include: an ion beam formed by any one or more inert gases of He, Ne, Ar, Kr and Xe. For example, an argon ion beam may be obtained by introducing argon gas through a grid, and optionally, the flow rate of the argon gas introduced into the reaction chamber is greater than or equal to 10 sccm and less than or equal to 100 sccm.
[0092] The grid can adjust the direction and energy of the plasma so that the plasma is evenly focused and bombards the inside of the target material. The deposited film will not introduce foreign elements. In addition, neutral particles are generated during the preparation process of the semiconductor structure of the embodiment of the present application. The plasma and the sputtered target particles will not be affected by electromagnetic interference from the outside world or inside the chamber, which effectively improves the purity of the prepared semiconductor structure.
[0093] In one possible implementation, see Figure 7 Shown is a schematic diagram of a grid structure in a sputtering ion source provided in an embodiment of the present application.
[0094] The grid of the sputtering ion source 10 provided in the embodiment of the present application can be arc-shaped, and the target material is arranged on one side of the arc grid 101 close to the center of the arc to focus the ion beam onto the target surface. The radius of the arc is greater than or equal to 300 mm and less than or equal to 800 mm.
[0095] In one possible implementation, see Figure 8 , which is a schematic diagram of another grid structure in a sputtering ion source provided in an embodiment of the present application.
[0096] The grid of the sputtering ion source 10 provided in the embodiment of the present application can also be plane, and the plane grid 102 is provided with a plurality of through holes, and the coverage of the plurality of through holes is [0.25 times, 0.75 times] of the area of the first target or the second target. Optionally, the plurality of through holes can be arranged in the central area of the plane grid 102 to achieve focusing of the ion beam.
[0097] In a possible implementation manner, the material of the adhesion barrier layer 6 provided in the embodiment of the present application may include: one or more materials selected from titanium, tantalum, titanium nitride, and tantalum nitride.
[0098] The above materials have a higher step coverage and can be better deposited on the inner wall of the trench 5 , that is, the material of the adhesion barrier layer 6 can be: Ti, Ta, TiN or TaN, or a combination of Ti / TiN, Ta / TaN, etc.
[0099] In a possible implementation, in the embodiment of the present application, when the deposited adhesion barrier layer 6 does not contain N element, the neutral ion beam used by the auxiliary ion source 12 may include: an ion beam formed by one or more inert gases.
[0100] In one possible implementation, in an embodiment of the present application, when the deposited adhesion barrier layer 6 contains N elements, such as TiN or TaN, the ion beam used by the auxiliary ion source 12 may include one or more of the inert gases and a mixed gas of nitrogen, so as to deposit an adhesion barrier layer 6 containing N elements such as TiN or TaN.
[0101] In a possible implementation manner, the material of the seed layer 7 provided in the embodiment of the present application may include: one or more of aluminum, copper and tungsten.
[0102] The above materials have good electrical conductivity, so that the semiconductor structure prepared in the embodiment of the present application has good electrical conductivity.
[0103] In a possible implementation, the depth-to-width ratio range of the groove 5 provided in the embodiment of the present application is: [2:1, 15:1]. That is, in the embodiment of the present application, the method of ion beam deposition can adapt to the groove 5 with a wide range of depth-to-width ratios, which can adapt to the complete filling in shallow groove deposition and can also ensure the completeness of filling in the case of deep grooves.
[0104] Optionally, in the embodiment of the present application, for the groove 5 with a high aspect ratio, a structure with a wide top and a narrow bottom can be formed, see Fig. 9 , which is a schematic diagram of another semiconductor structure provided in an embodiment of the present application.
[0105] In a possible implementation, the purity of the first target material 11 and the second target material 22 provided in the embodiment of the present application is greater than or equal to 99.9% and less than or equal to 99.9999%.
[0106] That is, in the embodiment of the present application, since IBD is a physical vapor deposition, the quality of the deposited film is related to the purity of the target material. The higher the purity of the target material, the better the purity of the prepared film. At the same time, the quality of the film is related to the vacuum and leakage rate of the chamber, and these properties of IBD are better than CVD. Therefore, the embodiment of the present application uses a high-purity first target material 11 and a second target material 22 to prepare a higher purity film.
[0107] In a possible implementation, an angle C between the auxiliary ion source 12 and the surface normal of the substrate 1 is greater than 0° and less than or equal to 30°.
[0108] That is, in the embodiment of the present application, in order to ensure that the sputtered particles can be smoothly deposited into the groove 5 with a high aspect ratio, the relative positions of the IBD target, substrate and ion source can be adjusted, and the sputtered particles are incident at a certain angle with a low divergence angle. Adjusting the angle can allow the sputtered particles to enter the bottom of the groove, achieving better coverage and conformality. In addition, the auxiliary ion source can further regulate the direction of the sputtered particles.
[0109] Optionally, in the embodiments of this application, see Fig.10 , which is a schematic diagram of another semiconductor structure provided by an embodiment of the present application. In some semiconductor device structures, in order to avoid deposition of the adhesion barrier layer 6 and the seed layer 7 at the bottom of the groove 5, the angle can be adjusted so that the adhesion barrier layer 6 and the seed layer 7 are only deposited on the sidewall of the groove 5, to prevent the adhesion barrier layer 6 and the seed layer 7 on the sidewall from being connected, causing a short circuit in the semiconductor device and affecting the electrical performance of the device.
[0110] In a possible implementation, the rotation speed range of the substrate 1 in the embodiment of the present application is greater than or equal to 5 rpm and less than or equal to 200 rpm.
[0111] That is, in the embodiment of the present application, the rotation speed of the substrate 1 should not be set too small or too large. If the rotation speed is set too small, it is not conducive to the uniform deposition of the film layer; if the rotation speed is set too large, the centrifugal force is large, which may cause the sputtered particles to fail to deposit on the film layer.
[0112] In a possible implementation, the thickness of the adhesion barrier layer 6 provided in the embodiment of the present application is greater than or equal to 2 nm and less than or equal to 100 nm. The thickness of the seed layer 7 is greater than or equal to 2 nm and less than or equal to 100 nm.
[0113] That is, in the embodiment of the present application, the thickness of the adhesion barrier layer 6 and the seed layer 7 can be set according to the needs of the actual device. The embodiment of the present application is not specifically limited here, and can be specifically set by those skilled in the art according to actual conditions.
[0114] In one possible implementation, the energy range of the neutral ion beam generated by the sputtering ion source 10 of the embodiment of the present application is greater than or equal to 400V and less than or equal to 1000V; the energy range of the neutral ion beam generated by the auxiliary ion source 12 is greater than or equal to 50V and less than or equal to 500V.
[0115] That is, in the embodiment of the present application, the energy of the neutral ion beam generated by the sputtering ion source 10 can be set to be relatively large, so that the target material can be bombarded with a relatively large energy neutral ion beam to generate sputtering particles. The auxiliary ion source 12 does not need to bombard the target material to generate sputtering particles, but only needs to change the path of generating sputtering particles. Therefore, the neutral ion beam generated by the auxiliary ion source 12 does not need to be set to a relatively large energy, which can reduce the power consumption of the device.
[0116] In a possible implementation, the current range of the sputtering ion source 10 provided in the embodiment of the present application is greater than or equal to 0.5A and less than or equal to 1.5A. The current range of the auxiliary ion source 12 is greater than or equal to 0.1A and less than or equal to 1.5A.
[0117] Similarly, since the energy of the neutral ion beam generated by the sputtering ion source 10 is relatively large, the current of the sputtering ion source 10 can be set to be relatively large to generate a neutral ion beam with relatively large energy. The energy of the neutral ion beam generated by the current range of the auxiliary ion source 12 is relatively small to generate a neutral ion beam with relatively small energy.
[0118] In a possible implementation, in the embodiment of the present application, the deposition rate of the adhesion barrier layer 6 is greater than or equal to 3 nm / min and less than or equal to 30 nm / min. The deposition rate of the seed layer 7 is greater than or equal to 3 nm / min and less than or equal to 30 nm / min. Therefore, in the embodiment of the present application, the deposition rates of the adhesion barrier layer 6 and the seed layer 7 should not be set too fast or too slow. Setting the deposition rate at [3 nm / min, 30 nm / min] can improve the film density of the deposited adhesion barrier layer 6 and the seed layer 7, and deposition at this speed can accurately control the thickness of the film layer and improve the deposition efficiency of the film layer.
[0119] In a possible implementation, in the embodiment of the present application, the RF power of the sputtering ion source 10 and the auxiliary ion source 12 is greater than or equal to 200 W and less than or equal to 1000 W. Therefore, in the embodiment of the present application, by setting the RF power range of the sputtering ion source 10 and the auxiliary ion source 12, the energy density of the emitted ion beam can be guaranteed, the film density of the deposited adhesion barrier layer 6 and the seed layer 7 can be improved, and the efficiency of film deposition can be improved.
[0120] In a possible implementation, in the embodiment of the present application, the sample temperature for depositing the first target material 11 is [50°C, 300°C], and the sample temperature for depositing the second target material 22 is (0°C, 100°C]. Therefore, in the embodiment of the present application, since the material of the first target material 11 may need to react with nitrogen to generate the adhesion barrier layer 6, the deposition temperature of the first target material 11 is set higher to achieve reaction with nitrogen at high temperature. The second target material 22 does not need to react with other substances, and therefore can be deposited at a low temperature, which can effectively prevent the diffusion of the deposited seed layer 7 elements and improve the reliability of the semiconductor structure.
[0121] For example, see Figure 6 As shown, the width of the groove 5 provided in the embodiment of the present application can be 250nm and the depth is 500nm. There can be an insulating layer on the inner wall of the groove 5 (not shown in the figure). The distance between two adjacent grooves 5 is 500nm. The groove 5 can be a circular groove with the same width at the top and bottom, a square groove and a long strip groove. The adhesion barrier layer 6 and the seed layer 7 can be deposited on the side wall and the bottom of the groove 5 in sequence by an ion beam deposition process. The sample rotation speed during all deposition processes is 100rpm. The specific steps are as follows: (1) The auxiliary ion source 12 is used to pass Ar with an energy of 400eV for ion beam etching. The angle C between the auxiliary ion source 12 and the surface normal of the substrate 1 is 25°, and the impurities on the side wall and the bottom of the groove 5 are etched away by 10nm;
[0122] (2) Auxiliary ion source 12 low energy 50eV into O 2The trench 5 is modified to form an insulating layer, the angle C between the auxiliary ion source 12 and the surface normal of the substrate 1 is 25°, and a 10 nm insulating layer is deposited on the bottom and side of the trench 5;
[0123] (3) The sputtering ion source 10 is supplied with Ar at a high energy of 1000 eV to sputter the first target material 11, and the auxiliary ion source 12 is supplied with Ar at a low energy of 50 eV to adjust the movement direction of the sputtered particles to form a single element adhesion barrier layer 6 or to supply Ar and N 2 The mixed gas forms a nitride adhesion barrier layer 6 with a changed direction, the angle C between the auxiliary ion source 12 and the surface normal of the substrate 1 is 27°, and the thickness of the adhesion barrier layer 6 is 10 nm;
[0124] (4) The sputtering ion source 10 is provided with Ar at high energy of 1000 eV to sputter the second target material 22, and the auxiliary ion source is provided with Ar at low energy of 50 eV to adjust the movement direction of the sputtered particles to form a seed layer 7. The angle C between the auxiliary ion source 12 and the surface normal of the substrate 1 is 27°, and the thickness of the seed layer 7 is 10 nm.
[0125] That is, in the embodiment of the present application, the groove 5 with the same width from top to bottom can be formed by adjusting the angles of the sputtering ion source 10 and the auxiliary ion source 12 .
[0126] In addition, in one possible implementation, see Fig. 9 As shown, the top width of the groove 5 provided in the embodiment of the present application can be 300nm, the bottom width of the groove 5 is 250nm, the depth is 1500nm, the sidewall of the groove 5 has an insulating layer, and the distance between two adjacent grooves 5 is 600nm. The groove 5 is a circular groove with a wide top and a narrow bottom, a square groove and a long strip groove. The adhesion barrier layer 6 and the seed layer 7 are sequentially deposited on the sidewall and the bottom of the groove 5 by an ion beam deposition process. The sample rotation speed during all deposition processes is 100rpm. The specific steps are as follows:
[0127] (1) The auxiliary ion source 12 is used to ion-beam etch Kr with an energy of 400 eV. The angle C between the auxiliary ion source 12 and the surface normal of the substrate 1 is 5°, and the impurities on the sidewall and bottom of the trench 5 are etched away by 10 nm.
[0128] (2) Auxiliary ion source 12 low energy 50eV into O 2 The trench 5 is modified to form an insulating layer, the angle C between the auxiliary ion source 12 and the surface normal of the substrate 1 is 5°, and a 10 nm insulating layer is deposited on the bottom and side of the trench 5;
[0129] (3) The sputtering ion source 10 is charged with Kr at a high energy of 1000 eV to sputter the first target material 11, and the auxiliary ion source 12 is charged with Ar at a low energy of 50 eV to adjust the movement direction of the sputtered particles to form a single element adhesion barrier layer 6, or charged with Kr and N 2The mixed gas forms a nitride adhesion barrier layer 6 with a changed direction, the angle C between the auxiliary ion source 12 and the surface normal of the substrate 1 is 7°, and the thickness of the adhesion barrier layer 6 is 10 nm;
[0130] (4) The sputtering ion source 10 injects Kr at high energy of 1000 eV to sputter the second target material 22, and the auxiliary ion source 12 injects Kr at low energy of 50 eV to adjust the movement direction of the sputtered particles to form a seed layer 7. The angle C between the auxiliary ion source 12 and the surface normal of the substrate 1 is 7°, and the thickness of the seed layer 7 is 10 nm.
[0131] That is, in the embodiment of the present application, a groove 5 that is wide at the top and narrow at the bottom can be formed by adjusting the angles of the sputtering ion source 10 and the auxiliary ion source 12 , which is generally suitable for forming a groove 5 with a high aspect ratio.
[0132] In another possible implementation, see Fig.10 As shown, the width of the groove 5 provided in the embodiment of the present application can be 500nm, the depth is 1500nm, the side wall of the groove 5 has an insulating layer, the distance between two adjacent grooves 5 is 1000nm, the groove 5 is a circular groove with the same width at the top and bottom, a square groove and a long strip groove, and the adhesion barrier layer 6 and the seed layer 7 are sequentially deposited on the side wall of the groove 5 by an ion beam deposition process. In order to prevent the side walls on both sides from being connected, the adhesion barrier layer 6 and the seed layer 7 will not be deposited at the bottom of the groove 5. The sample rotation speed during all deposition processes is 100rpm, and the specific steps are as follows:
[0133] (1) The auxiliary ion source 12 is used to inject Xe with an energy of 400 eV for ion beam etching. The angle C between the auxiliary ion source 12 and the surface normal of the substrate 1 is 15°, and the impurities on the sidewall and bottom of the trench 5 are etched away by 10 nm;
[0134] (2) Auxiliary ion source 12 low energy 50eV into O 2 The trench 5 is modified to form an insulating layer, the angle C between the auxiliary ion source 12 and the surface normal of the substrate 1 is 15°, and a 10 nm insulating layer is deposited on the bottom and side of the trench 5;
[0135] (3) The sputtering ion source 10 is injected with Xe at a high energy of 1000 eV to sputter the first target material 11, and the auxiliary ion source 12 is injected with Ar at a low energy of 50 eV to adjust the movement direction of the sputtered particles to form a single element adhesion barrier layer 6 or to inject Xe and N 2 The mixed gas forms a nitride adhesion barrier layer 6 with a changed direction, the angle C between the auxiliary ion source 12 and the surface normal of the substrate 1 is 22°, and the thickness of the adhesion layer is 10 nm;
[0136] (4) The sputtering ion source 10 injects Xe at a high energy of 1000 eV to sputter the second target material 22, and the auxiliary ion source 12 injects Xe at a low energy of 50 eV to adjust the movement direction of the sputtered particles to form a seed layer 7. The angle C between the auxiliary ion source 12 and the surface normal of the substrate 1 is 22°, and the thickness of the seed layer 7 is 10 nm.
[0137] That is, in the embodiment of the present application, the angles of the sputtering ion source 10 and the auxiliary ion source 12 can be adjusted so that in certain semiconductor device structures, the adhesion barrier layer 6 and the seed layer 7 are only deposited on the side walls of the groove 5. To prevent the side walls on both sides from being connected, the adhesion barrier layer 6 and the seed layer 7 will not be deposited at the bottom of the groove 5, thereby avoiding causing a short circuit in the semiconductor device and affecting the electrical performance of the device.
[0138] The embodiment of the present application provides a method for preparing a semiconductor structure, which includes: providing a substrate with grooves; a neutral ion beam generated by a sputtering ion source of an ion beam deposition device bombards a first target material to generate first sputtering particles; a neutral ion beam generated by an auxiliary ion source of the ion beam deposition device changes the incident direction of the first sputtering particles to form an adhesion barrier layer on the inner wall of the groove; a neutral ion beam generated by the sputtering ion source bombards a second target material to generate second sputtering particles; a neutral ion beam generated by the auxiliary ion source changes the incident direction of the second sputtering particles to form a seed layer on the inner wall of the groove; the auxiliary ion source and the substrate surface normal angle are acute. Through ion beam deposition, the sputtering particles can be guided to be incident at a certain angle so that the sputtering particles can better enter the bottom of the groove and achieve better step coverage and conformality.
[0139] An embodiment of the present application also provides a semiconductor structure, including a structure prepared using the method described above.
[0140] Each embodiment in this specification is described in a progressive manner, and the same or similar parts between the embodiments can be referred to each other, and each embodiment focuses on the differences from other embodiments. In particular, for the structural embodiment, since it is basically similar to the method embodiment, the description is relatively simple, and the relevant parts can be referred to the partial description of the method embodiment.
[0141] The above is only a preferred implementation of the present application. Although the present application has been disclosed as a preferred embodiment, it is not intended to limit the present application. Any technician familiar with the art can use the above disclosed methods and technical contents to make many possible changes and modifications to the technical solution of the present application without departing from the scope of the technical solution of the present application, or modify it into an equivalent embodiment of equivalent changes. Therefore, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present application without departing from the content of the technical solution of the present application still falls within the scope of protection of the technical solution of the present application.
Claims
1. A method for preparing a semiconductor structure, characterized in that: include: Step 1, providing a substrate with grooves; Step 2: bombarding the first target material with a neutral ion beam generated by a sputtering ion source of an ion beam deposition device to generate first sputtered particles; Step 3: using a neutral ion beam generated by an auxiliary ion source of the ion beam deposition device to change the incident direction of the first sputtered particles, so as to form an adhesion barrier layer on the inner wall of the groove; Step 4: bombarding a second target material with the neutral ion beam generated by the sputtering ion source to generate second sputtered particles; Step 5: Using the neutral ion beam generated by the auxiliary ion source, change the incident direction of the second sputtered particles to form a seed layer on the inner wall of the groove; the angle between the auxiliary ion source and the normal of the substrate surface is an acute angle.
2. The method according to claim 1, characterized in that The method of providing a substrate with grooves comprises: providing an initial substrate; Depositing a hard mask on the initial substrate to define structured regions by photolithography; The initial substrate in the structure area is etched to form the substrate with grooves.
3. The method according to claim 1, characterized in that The opening width of the groove is equal to the bottom width of the groove.
4. The method according to claim 1, characterized in that: The opening width of the groove is greater than the bottom width of the groove.
5. The method according to claim 1, characterized in that: Forming an adhesion barrier layer on the inner wall of the groove includes: forming an adhesion barrier layer on the side wall of the groove; Forming a seed layer on the inner wall of the trench includes: forming a seed layer on the side wall of the trench.
6. The method according to claim 1, characterized in that After providing the substrate with grooves, and before bombarding the first target material with a neutral ion beam generated by a sputtering ion source of an ion beam deposition device to generate first sputtered particles, the method further includes: The groove is pre-cleaned by using a neutral ion beam generated by the auxiliary ion source to remove impurities on the surface of the groove.
7. The method according to claim 1, characterized in that During the forming of the adhesion barrier layer and the forming of the seed layer, the substrate is controlled to keep rotating.
8. The method according to claim 1, characterized in that The neutral ion beam of the sputtering ion source includes an ion beam formed by any one or more inert gases among He, Ne, Ar, Kr and Xe.
9. The method according to claim 1, characterized in that: The neutral ion beam used by the auxiliary ion source includes: an ion beam formed by one or more inert gases.
10. The method according to claim 1, wherein the ion beam used by the auxiliary ion source comprises a mixed gas of one or more inert gases and nitrogen.
11. The method according to claim 1, characterized in that: The material of the adhesion barrier layer includes one or more of titanium, tantalum, titanium nitride and tantalum nitride.
12. The method according to claim 1, characterized in that The material of the seed layer includes: one or more of aluminum, copper and tungsten.
13. The method according to claim 1, characterized in that The aspect ratio of the groove is in the range of [2:1, 15:1].
14. The method according to claim 1, characterized in that The purity of the first target material and the second target material is greater than or equal to 99.9% and less than or equal to 99.9999%.
15. The method according to claim 1, characterized in that The angle between the auxiliary ion source and the substrate surface normal is greater than 0° and less than or equal to 30°.
16. The method according to claim 7, characterized in that The rotation speed range of the rotation is greater than or equal to 5 rpm and less than or equal to 200 rpm.
17. The method according to claim 1, characterized in that The thickness of the adhesion barrier layer is greater than or equal to 2 nm and less than or equal to 100 nm.
18. The method according to claim 1, characterized in that The thickness of the seed layer is greater than or equal to 2 nm and less than or equal to 100 nm.
19. The method according to claim 1, characterized in that The grid of the sputtering ion source is in an arc shape to focus the ion beam onto the surface of the target material, and the radius of the arc is greater than or equal to 300 mm and less than or equal to 800 mm.
20. The method according to claim 1, characterized in that The grid of the sputtering ion source is in a plane, and the grid is provided with a plurality of through holes, wherein the coverage area of the plurality of through holes is [0.25 times, 0.75 times] the area of the first target material or the second target material.
21. The method according to claim 1, characterized in that The deposition rate of the adhesion barrier layer is greater than or equal to 3 nm / min and less than or equal to 30 nm / min.
22. The method according to claim 1, characterized in that The deposition rate of the seed layer is greater than or equal to 3 nm / min and less than or equal to 30 nm / min.
23. The method according to claim 1, characterized in that The sample temperature for depositing the first target material is [50°C, 300°C], and the sample temperature for depositing the second target material is (0°C, 100°C].
24. A semiconductor structure, characterized in that: include: A structure prepared by the method according to any one of claims 1 to 23.