Gas diffusion layer for improving battery performance and preparation method and application thereof
By designing a macroporous base layer, a self-hydrophobic mesoporous zone and a self-hydrophilic microporous zone in the gas diffusion layer of the fuel cell, and using the hot pressing method to regulate its structure, the water management problem of the fuel cell under different operating conditions is solved. , improves battery performance and durability and avoids the impedance increase of additional additives.
Patent Information
- Application Number
- CN202310397806.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-14
- Publication Date
- 2024-10-18
AI Technical Summary
The gas diffusion layer of existing fuel cells is difficult to effectively manage moisture under different operating conditions, resulting in unstable battery performance, and commonly used hydrophilic or hydrophobic agent modification treatments increase impedance and reduce durability.
By designing a gas diffusion layer that includes a macroporous base layer, a self-hydrophobic mesoporous region, and a self-hydrophilic microporous region, the thermal pressing method is used to control the carbon particle packing density and pore structure to form regions with different degrees of hydrophobicity and depth. The stepped capillary force in the direction and the staggered hydrophilic and hydrophobic design avoid the impact of adding additional hydrophilic or hydrophobic agents.
It improves the water management capability and gas transmission performance of the fuel cell, reduces impedance and battery life issues, and ensures battery performance stability under different humidity and current density conditions.
Smart Images

Figure CN118800918A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of fuel cells, and in particular to a gas diffusion layer for improving battery performance, a preparation method and an application thereof. Background Art
[0002] As a secondary energy source, hydrogen energy has become a new alternative energy source that has attracted much attention today due to its abundant reserves, cleanliness, and high efficiency. Proton exchange membrane fuel cells use hydrogen as fuel and are energy conversion devices that directly convert chemical energy into electrical energy. They have the advantages of high energy density, low noise, high reliability, and high efficiency.
[0003] The main components of proton exchange membrane fuel cells are: catalyst layer, proton exchange membrane, gas diffusion layer and bipolar plate. Gas diffusion layer (GDL) is located between the catalyst layer and the bipolar plate, and plays an important role in conducting reaction gas, discharging excess water, conducting heat, and conducting electrons.
[0004] During the actual operation of fuel cells, different operating conditions will affect the performance of the fuel cell. Among them, the water management problem of fuel cells has become an important factor limiting the improvement of battery performance under low humidity and high current density. Under high humidity and high current, too much water is produced inside the fuel cell. If the water is not discharged in time, it is easy to cause the battery to be flooded, block the gas transmission channel, and cause the battery performance to be unstable or even decline. Therefore, it is necessary to improve the drainage capacity of the fuel cell; under low humidity and low current, the water production inside the fuel cell becomes less, and the membrane drying phenomenon is prone to occur, which affects the proton conductivity of the proton exchange membrane, causing the battery impedance to increase and thus affecting the battery performance.
[0005] As an important structure closely combined with the catalyst layer, the microporous layer plays an important role in water and gas transmission to the interior of the catalyst. The mass transfer capacity of the microporous layer is closely related to the water management capacity of the fuel cell. Generally, the larger the porosity of the microporous layer, the more conducive it is to fuel and gas transmission; but the larger pore structure, on the one hand, leads to weak capillary action of the pores, which is not conducive to the back diffusion of cathode water into the anode; on the other hand, the adsorption effect on water is small and the water retention capacity is weak, which limits the further improvement of battery performance under low humidity or high current density. In particular, water needs to be discharged in time after it is generated at the three-phase interface, otherwise the accumulated water will be retained at the contact interface between the catalyst layer and the microporous layer, blocking the pores and affecting the fuel from continuing to pass through the microporous layer into the catalyst layer to participate in the reaction. Therefore, at the interface between the microporous layer and the catalyst layer, good transition and matching properties on the pore scale are required.
[0006] Based on the above problems, Chinese patent 200610167389.4 proposes a fuel cell membrane electrode, which comprises an anode gas diffusion layer, a cathode gas diffusion layer, a proton exchange membrane, an anode catalyst layer and a cathode catalyst layer in sequence, wherein the gas diffusion layer comprises a conductive carrier and a conductive agent and an adhesive loaded on the conductive carrier, wherein the adhesive in the anode gas diffusion layer is a hydrophilic adhesive, specifically a sulfonic acid resin or a fluorinated sulfonic acid resin. Although the scheme utilizes a polymer resin as a hydrophilic substance to achieve the effect of water balance, the polymer resin will cause an increase in impedance and a decrease in battery performance. At the same time, after a long period of operation, the polymer resin is prone to displacement or fall off, causing a sharp decrease in battery durability.
[0007] Chinese patent CN202120819395.3 proposes a multi-layer drainage gas diffusion layer, which is used in fuel cells. The multi-layer drainage gas diffusion layer is installed between the electrode plate and the membrane assembly, including: a first density layer, a water-conducting layer, and a second density layer. The gas passes through the water-conducting layer, the second density layer, and the first density layer in turn from the flow channel to the membrane assembly. The material gap of the second density layer is larger than the material gap of the first density layer. The liquid on the membrane assembly passes through the first density layer, the second density layer, and the water-conducting layer in turn to enter the flow channel and flow out of the electrode plate. This solution uses multiple layers of materials with different densities to drain water, which can indeed avoid the problem of water accumulating in the gas diffusion layer. However, the density layers with different material gaps are prone to loose bonding, which can easily cause peeling between layers, increase the contact resistance on the interface, and affect battery performance.
[0008] In summary, a gas diffusion layer with a simple preparation process and good water management performance is urgently needed to be developed. Summary of the invention
[0009] The purpose of the present invention is to overcome the defects of the above-mentioned prior art and to provide a gas diffusion layer and its preparation method and application for improving battery performance. The gas diffusion layer does not require the use of additional hydrophilic agents and hydrophobic agents to modify the carbon powder or microporous layer, but instead designs the hydrophilic and hydrophobic regions stacked in sequence by regulating the three-dimensional network of carbon powder accumulation, and constructs an interface pore structure with good pore matching with the catalyst layer.
[0010] The gas diffusion layer of the present invention includes a macroporous base layer, a self-hydrophobic mesoporous region and a self-hydrophilic microporous region stacked in sequence. The stacking density and form of carbon particles are regulated by hot pressing, and the pore structures in different regions of the microporous layer are given different degrees of hydrophilicity and hydrophobicity, so as to achieve matching optimization between the stepped capillary force in the depth direction of the microporous layer and the hydrophilic and hydrophobic staggered design areas, thereby avoiding the effects of increased impedance and increased battery instability caused by adding additional hydrophilic or hydrophobic agents during the preparation of the microporous layer slurry.
[0011] The purpose of the present invention can be achieved by the following technical solutions:
[0012] A gas diffusion layer for improving battery performance comprises a macroporous substrate layer, a self-hydrophobic mesoporous region and a self-hydrophilic microporous region, wherein the self-hydrophobic mesoporous region is attached to the surface of the macroporous substrate layer, and the self-hydrophilic microporous region is attached to the surface of the self-hydrophobic mesoporous region.
[0013] Furthermore, according to different working conditions, the self-hydrophobic mesoporous regions and the self-hydrophilic microporous regions are stacked alternately.
[0014] The self-hydrophobic mesoporous region and the self-hydrophilic microporous region are structures with different hydrophilicity and hydrophobicity formed by controlling the packing density and particle gaps of the carbon particles through hot pressing treatment. The hydrophilicity and hydrophobicity of the two structures depend on the apparent density, porosity and pore size after hot pressing treatment. The coordinated design of the hydrophilic and hydrophobic pore regions in the gas diffusion layer can staggeredly stack the self-hydrophobic mesoporous regions and the self-hydrophilic microporous regions according to different working conditions, while satisfying the matching optimization of the stepped capillary force in the depth direction and the hydrophilic and hydrophobic staggered regions, thereby improving the mass transfer capacity of the gas diffusion layer and improving the battery performance.
[0015] Furthermore, the loading of the self-hydrophilic microporous region accounts for 10%-60% of the mass of the gas diffusion layer.
[0016] Furthermore, the macroporous substrate layer is selected from any one of carbon fiber paper, carbon paper, carbon cloth or carbon felt.
[0017] Furthermore, the self-hydrophobic mesoporous region is composed of carbon powder, deionized water and an additive, the ratio of the carbon powder to the additive is 1:9 to 9:1, and the amount of the deionized water added is 10-50 times the mass of the carbon powder.
[0018] Furthermore, the self-hydrophilic microporous area is composed of carbon powder, deionized water and an auxiliary agent, the ratio of the carbon powder to the auxiliary agent is 1:9 to 9:1, and the amount of the deionized water added is 10-30 times the mass of the carbon powder.
[0019] Furthermore, the carbon powder is selected from any one or more combinations of conductive carbon black, conductive graphite, Ketjen black, carbon nanotubes, carbon fibers or graphene.
[0020] Furthermore, the auxiliary agent is selected from any one of polydimethylguanidine salt, alkyl glycoside, alkylphenol polyoxyethylene ether, dodecyl dimethyl betaine or polyethylene glycol.
[0021] Furthermore, the porosity of the self-hydrophobic mesoporous region is above 45%, and the proportion of pores above 50 nm in the total pore size is 40%-60%.
[0022] Furthermore, the porosity of the self-hydrophilic microporous region is above 65%, and the proportion of pores with a diameter of 2-30 nm to the total pore diameter is 30%-50%.
[0023] The present invention also provides a method for preparing a gas diffusion layer for improving battery performance, the specific steps are as follows:
[0024] S1, preparing a carbon powder dispersion A, wherein the carbon powder dispersion A is prepared by mixing carbon powder, deionized water and an additive;
[0025] S2, coating the carbon powder dispersion A obtained in step S1 on the surface of the macroporous base layer to obtain a mesoporous structure after a first treatment;
[0026] S3, subjecting the mesoporous structure obtained in step S2 to a second treatment to obtain a self-hydrophobic mesoporous region;
[0027] S4, preparing a carbon powder dispersion B, wherein the carbon powder dispersion B is prepared by mixing carbon powder, deionized water and an additive;
[0028] S5, coating the carbon powder dispersion B obtained in step S4 on the surface of the self-hydrophobic mesoporous region obtained in step S3, and obtaining a microporous structure after a third treatment;
[0029] S6, subjecting the microporous structure obtained in step S5 to a fourth treatment to obtain a self-hydrophilic microporous region, thereby forming a gas diffusion layer.
[0030] Furthermore, in step S1, appropriate amounts of carbon powder, deionized water and additives are weighed, and the carbon powder and additives are slowly added to the deionized water while stirring, and emulsified at 25-60° C. for 2-6 hours. After the carbon powder is emulsified, it is stirred at room temperature for 5-10 hours to obtain carbon powder dispersion A.
[0031] Furthermore, in step S2, the coating load of the carbon powder dispersion A is 0.1 to 15 mg / cm 2 The coating method of the carbon powder dispersion A is any one or more combinations of blade coating, screen printing, high-pressure gas spraying, ultrasonic spraying, transfer coating, extrusion coating or casting.
[0032] Furthermore, in step S2, the first treatment includes a drying treatment and a sintering treatment.
[0033] The drying conditions are as follows: drying temperature 65-180°C, air atmosphere, and drying time 5-10 minutes;
[0034] The sintering conditions are as follows: sintering temperature of 250° C.-500° C., sintering atmosphere of inert gas, and sintering time of 1-6 hours.
[0035] Furthermore, in step S3, the second treatment includes drying treatment and hot pressing treatment, and the temperature, pressure, and time of the hot pressing treatment are related to the selected carbon powder model and loading.
[0036] The drying conditions are as follows: drying temperature 65-180°C, air atmosphere, and drying time 5-10 minutes;
[0037] The conditions of the hot pressing treatment are as follows: hot pressing temperature of 500° C.-1250° C., hot pressing atmosphere of inert gas, hot pressing time of 2-60s, hot pressing pressure of 0.2-5Mpa.
[0038] Further, in step S4, appropriate amounts of carbon powder, deionized water and additives are weighed, and the carbon powder and additives are slowly added to the deionized water while stirring, and stirred at 3500 rpm for 3 hours in a cold water bath, and then stirred at 8000 rpm for 5 hours to obtain carbon powder dispersion B.
[0039] Furthermore, in step S5, the coating load of the carbon powder dispersion B is 0.1 to 6 mg / cm 2 The coating method of the carbon powder dispersion A is any one or more combinations of blade coating, screen printing, high-pressure gas spraying, ultrasonic spraying, transfer coating, extrusion coating or casting.
[0040] Furthermore, in step S5, the third treatment includes a drying treatment and a sintering treatment.
[0041] The drying conditions are as follows: drying temperature 65-135°C, air atmosphere, and drying time 5-10 minutes;
[0042] The sintering conditions are as follows: sintering temperature of 350° C.-450° C., sintering atmosphere of inert gas, and sintering time of 0.5-3 h.
[0043] Furthermore, in step S6, the fourth treatment includes drying treatment and hot pressing treatment, and the temperature, pressure, and time of the hot pressing treatment are related to the selected carbon powder model and loading.
[0044] The drying conditions are as follows: drying temperature 65-135°C, air atmosphere, and drying time 5-10 minutes;
[0045] The conditions of the hot pressing treatment are: hot pressing temperature of 500° C.-1000° C., hot pressing atmosphere of inert gas, hot pressing time of 2-30s, hot pressing pressure of 2.5-5Mpa.
[0046] In addition, the present invention also provides an application of a gas diffusion layer for improving battery performance, and the gas diffusion layer is applied to a proton exchange membrane fuel cell.
[0047] Furthermore, the proton exchange membrane fuel cell consists of a catalyst layer, a proton exchange membrane, a gas diffusion layer and a bipolar plate, the gas diffusion layer is located between the catalyst layer and the bipolar plate, the macroporous substrate layer is attached to the surface of the bipolar plate, and the self-hydrophilic microporous area is connected to the catalyst layer.
[0048] The principle of the present invention is as follows:
[0049] The existing invention mainly improves the gas diffusion layer by adding additional hydrophobic agents and surfactants. On the one hand, it ignores the effect of the pore structure of the gas diffusion layer itself on the water management ability. On the other hand, it ignores the role of the pore size matching at the interface between the gas diffusion layer and the catalyst layer in effectively removing water.
[0050] The present invention is based on the way that carbon particles in the gas diffusion layer are accumulated to form a pore structure, aiming to obtain a three-dimensional pore network with different pore sizes and hydrophilic and hydrophobic degrees. The present invention can endow the pore structure with self-hydrophilic and hydrophobic capabilities, effectively realize the removal or adsorption of water by the pore structure, and achieve matching optimization of the stepped capillary force in the microporous layer and the hydrophilic and hydrophobic staggered design area. This setting can simultaneously meet the requirements of gas and liquid transmission for pore structure, effectively improve the water retention capacity of the anode and the water removal capacity of the cathode, and greatly reduce the adverse effects of chemical substances introduced by hydrophilic and hydrophobic treatment on battery impedance and durability, and achieve stable output of battery performance at low humidity or high current density, and the preparation method is simple.
[0051] During the preparation of the gas diffusion layer, the temperature, pressure and time of the hot pressing treatment will affect the packing density and particle gaps of different types of carbon particles, and thermal desorption of oxygen-containing functional groups will also occur. Therefore, through hot pressing treatment, the packing density of carbon particles in the gas diffusion layer and the gaps between different types of carbon particles can be changed, thereby changing the porosity and apparent density, pore size, and surface free energy of the pore structure, and obtaining a three-dimensional pore network with different hydrophilic and hydrophobic degrees, achieving a good transition and matching with the catalyst layer at the pore scale, and achieving efficient removal of generated water.
[0052] The first and second treatments are preferably used to prepare highly loose and hydrophobic mesoporous regions. The final self-hydrophobic mesoporous structure is filled with a large amount of air, with a reduced surface free energy, capable of quickly draining excess water, thereby improving the battery's water management capabilities and maintaining extremely low impedance under low humidity or high current density, thereby achieving high-performance and stable output of the battery.
[0053] The third and fourth treatments are preferably used to prepare microporous areas with dense and hydrophilic surfaces. The self-hydrophilic microporous structure finally obtained has a small specific surface area and contains a large number of micropores. The capillary force has a strong adsorption effect on water, which effectively improves the hydrophilicity and water retention capacity of the microporous layer, maintains the extremely low impedance of the battery itself under low humidity or high current density and the good wettability of the gas inside the gas diffusion layer, and realizes high performance and stable output of the battery.
[0054] Especially at the interface with the catalyst layer, the presence of the dense surface microporous layer, on the one hand, reduces the contact resistance between the gas diffusion layer and the catalytic layer, and effectively reduces the surface porosity of the porous support layer, preventing the catalyst coating from invading the gas diffusion layer, thereby improving the utilization rate of the catalyst; on the other hand, it has a good match and transition with the pores of the catalyst layer, effectively realizing the migration and discharge of water at two pore scales.
[0055] The loading and thickness of the self-hydrophobic mesoporous area and the self-hydrophilic microporous area on the gas diffusion layer can be flexibly adjusted according to the different gas flow channel designs and actual operating conditions in the fuel cell. By adjusting the pore structure, loading and thickness of the self-hydrophobic mesoporous area and the self-hydrophilic microporous area during the coating process, the depth of the hydrophilic and hydrophobic areas can be controlled in the depth direction, thereby achieving the matching optimization of the stepped capillary force in the microporous layer and the hydrophilic and hydrophobic staggered design area.
[0056] Compared with the prior art, the present invention has the following advantages:
[0057] (1) The hydrophobic structure and hydrophilic structure of the gas diffusion layer of the present invention are designed independently of each other, and no additional hydrophobic agent or hydrophilic agent needs to be added or treated to the gas diffusion layer, thereby avoiding the impact on the slurry stability caused by the addition of hydrophobic agent or hydrophilic agent during the preparation of the support layer and microporous layer slurry of the gas diffusion layer, greatly reducing the workload required for optimizing the slurry, and avoiding the potential risk of agglomeration of the hydrophobic agent and the hydrophilic agent.
[0058] (2) The self-hydrophobic mesoporous region described in the present invention is obtained by regulating the packing density of carbon particles and the gap between particles through hot pressing treatment, so that the interior of the mesoporous structure is filled with air, which reduces the free energy of the surface of the pore structure, and gives the highly loose mesoporous region excellent hydrophobicity, thereby constructing a self-hydrophobic pore structure. The strength of its hydrophobicity depends on the type of carbon particles in the pore structure, the packing density and the gaps between different types of carbon particles, thereby avoiding the defects of increased resistance and decreased durability caused by the addition of traditional oxides, organic matter and other materials.
[0059] (3) The self-hydrophilic microporous region of the present invention is formed by regulating the packing density of carbon particles and the gap between particles through hot pressing treatment, and has structural characteristics such as smaller specific surface area and a large number of micropores. These structures make the capillary force in the microporous structure obvious, improve the adsorption of water by capillary force, give the microporous region excellent hydrophilic and water-retaining ability, and construct a self-hydrophilic pore structure. The strength of its hydrophilicity depends on the type of carbon particles in the pore structure, the packing density and the gaps between different types of carbon particles.
[0060] (4) Under low humidification conditions, the hydrophilic microporous area can actively adsorb the water generated by the fuel cell and use it to moisten the proton exchange membrane, thereby preventing the proton conductivity of the proton exchange membrane from decreasing due to dehydration. Under high humidification conditions, the hydrophilic area can serve as a preferential drainage channel for water, thereby discharging excess water from the battery and preventing the battery from being flooded.
[0061] (5) The hydrophobic mesoporous region still retains high hydrophobicity and gas permeability. Therefore, the gas diffusion layer can be divided into different hydrophilic and hydrophobic functional regions, providing a realistic basis for multi-physics field coupling to optimize fuel cell performance.
[0062] (6) At the interface with the catalyst layer, the dense microporous structure can reduce the contact resistance between the gas diffusion layer and the catalyst layer, and effectively reduce the surface porosity of the gas diffusion layer, preventing the catalyst coating from invading the gas diffusion layer, thereby improving the utilization rate of the catalyst; on the other hand, it satisfies the good matching and transition with the pores of the catalyst layer, effectively realizing the migration and discharge of water at two pore scales. BRIEF DESCRIPTION OF THE DRAWINGS
[0063] Figure 1 is a schematic diagram of the cross section of the gas diffusion layer;
[0064] Figure 2 Schematic diagram of the self-hydrophobic mesoporous region formed on the surface of the gas diffusion layer;
[0065] Figure 3 Schematic diagram of the self-hydrophilic microporous area formed on the surface of the gas diffusion layer;
[0066] Figure 4 Polarization curves of Examples 1-5 under low humidification conditions (relative humidity: 35%);
[0067] Figure 5 The impedance curves of Examples 1-5 under low humidification conditions (relative humidity: 35%);
[0068] Figure 6 is the polarization curve of Example 1-5 under high temperature conditions (T=85°C);
[0069] Figure 7The impedance curve of Example 1-5 under high temperature conditions (T = 85°C);
[0070] Explanation of the accompanying drawings: 1. macroporous substrate layer, 2. self-hydrophobic microporous region, 3. self-hydrophilic microporous region, 4. catalyst layer. DETAILED DESCRIPTION
[0071] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0072] A gas diffusion layer for improving battery performance comprises a macroporous substrate layer 1, a self-hydrophobic mesoporous region 2 and a self-hydrophilic microporous region 3, wherein the self-hydrophobic mesoporous region 2 is attached to the surface of the macroporous substrate layer 1, and the self-hydrophilic microporous region 3 is attached to the surface of the self-hydrophobic mesoporous region 2.
[0073] In some specific embodiments, according to different working conditions, the self-hydrophobic mesoporous region 2 and the self-hydrophilic microporous region 3 are stacked alternately.
[0074] The self-hydrophobic mesoporous region 2 and the self-hydrophilic microporous region 3 are formed by controlling the packing density of carbon particles and the inter-particle gaps through hot pressing treatment to form structures with different hydrophilicity and hydrophobicity. The hydrophilicity and hydrophobicity of the two structures depend on the apparent density, porosity and pore size after hot pressing treatment. The coordinated design of the hydrophilic and hydrophobic pore regions in the gas diffusion layer can staggeredly stack the self-hydrophobic mesoporous region 2 and the self-hydrophilic microporous region 3 according to different working conditions, while satisfying the matching optimization of the stepped capillary force in the depth direction and the hydrophilic and hydrophobic staggered regions, thereby improving the mass transfer capacity of the gas diffusion layer and improving the battery performance.
[0075] In some specific embodiments, the loading amount of the self-hydrophilic microporous region 3 accounts for 10%-60% of the mass of the gas diffusion layer.
[0076] In some specific embodiments, the macroporous substrate layer 1 is selected from any one of carbon fiber paper, carbon paper, carbon cloth or carbon felt.
[0077] In some specific embodiments, the self-hydrophobic mesoporous region 2 is composed of carbon powder, deionized water and additives, the ratio of the carbon powder to the additives is 1:9 to 9:1, and the amount of deionized water added is 10-50 times the mass of the carbon powder.
[0078] In some specific embodiments, the self-hydrophilic microporous area 3 is composed of carbon powder, deionized water and additives, the ratio of the carbon powder to the additives is 1:9 to 9:1, and the amount of deionized water added is 10-30 times the mass of the carbon powder.
[0079] In some specific embodiments, the carbon powder is selected from any one or more combinations of conductive carbon black, conductive graphite, Ketjen black, carbon nanotubes, carbon fibers or graphene.
[0080] In some specific embodiments, the auxiliary agent is selected from any one of polydimethylguanidine salt, alkyl glycoside, alkylphenol polyoxyethylene ether, dodecyl dimethyl betaine or polyethylene glycol.
[0081] In some specific embodiments, the porosity of the self-hydrophobic mesoporous region 2 is greater than 45%, and the proportion of pores greater than 50 nm in the total pore size is 40%-60%.
[0082] In some specific embodiments, the porosity of the self-hydrophilic microporous region 3 is above 65%, and the proportion of pores with a diameter of 2-30 nm in the total pore diameter is 30%-50%.
[0083] The present invention also provides a method for preparing a gas diffusion layer for improving battery performance, the specific steps are as follows:
[0084] S1, preparing a carbon powder dispersion A, wherein the carbon powder dispersion A is prepared by mixing carbon powder, deionized water and an additive;
[0085] S2, coating the carbon powder dispersion A obtained in step S1 on the surface of the macroporous substrate layer 1, and obtaining a mesoporous structure after a first treatment;
[0086] S3, subjecting the mesoporous structure obtained in step S2 to a second treatment to obtain a self-hydrophobic mesoporous region 2;
[0087] S4, preparing a carbon powder dispersion B, wherein the carbon powder dispersion B is prepared by mixing carbon powder, deionized water and an additive;
[0088] S5, coating the carbon powder dispersion B obtained in step S4 on the surface of the self-hydrophobic mesoporous region 2 obtained in step S3, and obtaining a microporous structure after a third treatment;
[0089] S6, subjecting the microporous structure obtained in step S5 to a fourth treatment to obtain a self-hydrophilic microporous region 3, thereby forming a gas diffusion layer.
[0090] In some specific embodiments, in step S1, appropriate amounts of carbon powder, deionized water and additives are weighed, and the carbon powder and additives are slowly added to the deionized water while stirring, and emulsified at 25-60° C. for 2-6 hours. After the carbon powder is emulsified, it is stirred at room temperature for 5-10 hours to obtain a carbon powder dispersion A.
[0091] In some specific embodiments, in step S2, the coating loading of the carbon powder dispersion A is 0.1 to 15 mg / cm 2 The coating method of the carbon powder dispersion A is any one or more combinations of blade coating, screen printing, high-pressure gas spraying, ultrasonic spraying, transfer coating, extrusion coating or casting.
[0092] In some specific embodiments, in step S2, the first treatment includes a drying treatment and a sintering treatment.
[0093] The drying conditions are as follows: drying temperature 65-180°C, air atmosphere, and drying time 5-10 minutes;
[0094] The sintering conditions are as follows: sintering temperature of 250° C.-500° C., sintering atmosphere of inert gas, and sintering time of 1-6 hours.
[0095] In some specific embodiments, in step S3, the second treatment includes drying treatment and hot pressing treatment, and the temperature, pressure, and time of the hot pressing treatment are related to the selected carbon powder model and loading.
[0096] The drying conditions are as follows: drying temperature 65-180°C, air atmosphere, and drying time 5-10 minutes;
[0097] The conditions of the hot pressing treatment are as follows: hot pressing temperature of 500° C.-1250° C., hot pressing atmosphere of inert gas, hot pressing time of 2-60s, hot pressing pressure of 0.2-5Mpa.
[0098] In some specific embodiments, in step S4, appropriate amounts of carbon powder, deionized water and additives are weighed, and the carbon powder and additives are slowly added to the deionized water while stirring, and stirred at 3500 rpm for 3 hours in a cold water bath, and then stirred at 8000 rpm for 5 hours to obtain carbon powder dispersion B.
[0099] In some specific embodiments, in step S5, the coating loading of the carbon powder dispersion B is 0.1 to 6 mg / cm 2 The coating method of the carbon powder dispersion A is any one or more combinations of blade coating, screen printing, high-pressure gas spraying, ultrasonic spraying, transfer coating, extrusion coating or casting.
[0100] In some specific embodiments, in step S5, the third treatment includes a drying treatment and a sintering treatment.
[0101] The drying conditions are as follows: drying temperature 65-135°C, air atmosphere, and drying time 5-10 minutes;
[0102] The sintering conditions are as follows: sintering temperature of 350° C.-450° C., sintering atmosphere of inert gas, and sintering time of 0.5-3 h.
[0103] In some specific embodiments, in step S6, the fourth treatment includes drying treatment and hot pressing treatment, and the temperature, pressure, time and the load of the hot pressing treatment are related to the selected carbon powder type and loading.
[0104] The drying conditions are as follows: drying temperature 65-135°C, air atmosphere, and drying time 5-10 minutes;
[0105] The conditions of the hot pressing treatment are: hot pressing temperature of 500° C.-1000° C., hot pressing atmosphere of inert gas, hot pressing time of 2-30s, hot pressing pressure of 2.5-5Mpa.
[0106] In addition, the present invention also provides an application of a gas diffusion layer for improving battery performance, and the gas diffusion layer is applied to a proton exchange membrane fuel cell.
[0107] In some specific embodiments, the proton exchange membrane fuel cell is composed of a catalyst layer 4, a proton exchange membrane, a gas diffusion layer and a bipolar plate, the gas diffusion layer is located between the catalyst layer 4 and the bipolar plate, the macroporous substrate layer 1 is attached to the surface of the bipolar plate, and the self-hydrophilic microporous region 3 is connected to the catalyst layer 4.
[0108] The above implementation modes are described in more detail below in conjunction with specific examples.
[0109] Example 1
[0110] Design of self-hydrophobic mesoporous region 2: 10 parts of acetylene black, 1 part of polyethylene glycol and 100 parts of deionized water were mixed and emulsified at room temperature for 3 hours, and continued to stir for 5 hours, thereby obtaining a uniformly dispersed first mixture slurry. After that, the first mixture slurry was evenly coated on the carbon fiber paper, and the coating thickness was controlled to be 100-150μm. After the coating was completed, it was dried in a drying furnace at 100℃ for 10 minutes and sintered in a sintering furnace at 300℃ for 60 minutes to complete the first treatment; then it was dried in a drying furnace at 80℃ for 10 minutes, and hot pressed in a hot press furnace under nitrogen atmosphere at 500℃ with a pressure of 1Mpa for 10s to complete the second treatment, thereby obtaining a mesoporous region with self-hydrophobicity.
[0111] Design of self-hydrophilic microporous area 3: 8 parts of carbon black, 1 part of polyethylene glycol and 50 parts of deionized water are mixed and stirred at 3500rpm for 3h in a cold water bath by a stirrer, then dispersed at 4000rpm for 3 hours, and then stirred at 8000rpm for 5h, thereby obtaining a uniformly dispersed second mixture slurry. After that, the second mixture slurry is evenly coated on the self-hydrophilic mesoporous area 2, and the coating thickness is controlled to be 100-150μm. After the coating is completed, it is dried in a drying furnace at 80℃ for 8 minutes and sintered in a sintering furnace at 300℃ for 60 minutes to complete the third treatment; then it is dried in a drying furnace at 80℃ for 6 minutes again, and hot pressed at 5MPa pressure for 15s in a hot pressing furnace under nitrogen atmosphere protection at 500℃ to complete the fourth treatment, thereby obtaining a microporous area with self-hydrophilicity.
[0112] The loading of the obtained self-hydrophilic microporous region 3 accounts for 60% of the mass of the low-pressure and low-humidity fuel cell gas diffusion layer.
[0113] The contact angle between the gas diffusion layer of the fuel cell and water is 145°.
[0114] like Figure 2 As shown, the surface of the hydrophobic mesoporous region 2 is loose, the porosity is 60%, and the proportion of pores larger than 50 nm in the total pore size is 57%.
[0115] like Figure 3 As shown, the surface of the self-hydrophilic microporous region 3 is dense, the porosity is 65%, and the proportion of pores with a diameter of 2-30 nm in the total pore diameter is 40%.
[0116] The prepared gas diffusion layer was assembled and tested for membrane electrode. Test conditions: the hydrogen and air ratio was 1.5:2.0; the back pressure of the cathode and anode was 0.3 bar; the battery test temperature was 80°C; and the polarization curve test was pre-activated for 4 hours. The polarization curve test results are shown in Figure 4 and Figure 6 As shown, when both cathode and anode are humidified by 35%, 1.52A / cm2 can be obtained at a voltage of 0.6V. 2 ; When the cathode and anode are both at 85℃, 0.4V voltage can obtain 2.18A / cm 2 .
[0117] Example 2
[0118] Design of self-hydrophobic mesoporous region 2: Graphite powder, polydimethylguanidine salt and deionized water were mixed in a ratio of 4:1:250 and emulsified at room temperature for 3.5 hours, and then stirred for 5.5 hours to obtain a uniformly dispersed first mixture slurry. Then the first mixture slurry was evenly coated on a 25 cm 2The carbon fiber paper is coated with a coating thickness of 150-200 μm. After coating, it is dried in a drying furnace at 85°C for 10 minutes and sintered in a sintering furnace at 300°C for 150 minutes to complete the first treatment; then it is dried in a drying furnace at 60°C for 8 minutes and hot-pressed in a hot pressing furnace at 500°C under nitrogen atmosphere at a pressure of 1 MPa for 15 seconds to complete the second treatment, thereby obtaining a mesoporous region with self-hydrophobicity.
[0119] Design of self-hydrophilic microporous region 3: After mixing graphene, polydimethylguanidine salt and deionized water at a ratio of 10:1:400, stir at 3500rpm in a cold water bath with a stirrer for 3 hours, disperse at 4000rpm for 3 hours, and stir at 8000rpm for 5 hours, thereby obtaining a uniformly dispersed second mixture slurry. Then the second mixture slurry is evenly coated on the self-hydrophilic mesoporous region 2, and the coating thickness is controlled to be 50-100μm. After coating, it is dried in a drying furnace at 85℃ for 5-10 minutes and sintered in a sintering furnace at 300℃ for 120 minutes to complete the third treatment; then it is dried in a drying furnace at 60℃ for 7 minutes, and hot pressed in a hot press furnace at 700℃ under nitrogen atmosphere for 10s at 3Mpa pressure to complete the fourth treatment, thereby obtaining a microporous region with self-hydrophilicity.
[0120] The loading of the obtained self-hydrophilic microporous region 3 accounts for 30% of the mass of the low-pressure and low-humidity fuel cell gas diffusion layer.
[0121] The contact angle of the fuel cell gas diffusion layer finally obtained with water is 142°;
[0122] The prepared gas diffusion layer was assembled and tested for membrane electrode. The parameters of the commercial catalyst / membrane complex (CCM) used were: proton exchange membrane thickness 15 μm, anode catalyst (Pt / C) loading 0.1 mg / cm 2 , cathode catalyst (Pt / C) loading 0.3 mg / cm 2 Test conditions: The hydrogen and air ratio is 1.5:2.0; the back pressure of the cathode and anode is 0.3 bar; the battery test temperature is 80°C; the battery is pre-activated for 4 hours before the polarization curve test. Figure 4 and Figure 6 As shown, when both cathode and anode are humidified by 35%, 1.89A / cm2 can be obtained at a voltage of 0.6V. 2 ; The temperature of the cathode and anode was 85℃, and the voltage of 0.4V could obtain 1.34A / cm 2 .
[0123] Example 3
[0124] Design of self-hydrophobic mesoporous region 2: acetylene black, polydimethylguanidine salt and deionized water were mixed in a ratio of 4:1:20 and emulsified at room temperature for 5 hours, and then stirred for 5 hours to obtain a first mixture slurry with uniform dispersion. Then the first mixture slurry was evenly coated on a 25 cm 2 The carbon fiber paper is coated with a thickness of 200-250 μm. After coating, it is dried in a drying furnace at 85°C for 10 minutes and sintered in a sintering furnace at 300°C for 150 minutes to complete the first treatment; then it is dried in a drying furnace at 85°C for 10 minutes and hot-pressed in a hot-pressing furnace at 800°C under nitrogen atmosphere at a pressure of 3 MPa for 20 seconds to complete the second treatment, thereby obtaining a mesoporous region with self-hydrophobicity.
[0125] Design of self-hydrophilic microporous region 3: After mixing graphene, polyethylene glycol and deionized water in a ratio of 5:1:20, stir at 3500rpm in a cold water bath with a stirrer for 3 hours, disperse at 4000rpm for 3 hours, and stir at 8000rpm for 5 hours, thereby obtaining a uniformly dispersed second mixture slurry. The second mixture slurry is evenly coated on the self-hydrophilic mesoporous region 2, and the coating thickness is controlled to be 20-50μm. After coating, it is dried in a drying furnace at 85℃ for 5 minutes and sintered in a sintering furnace at 300℃ for 120 minutes to complete the third treatment; then it is dried in a drying furnace at 85℃ for 5 minutes again, and hot pressed at 5Mpa pressure for 45s in a hot pressing furnace under the protection of helium atmosphere at 800℃ to complete the fourth treatment, thereby obtaining a microporous region with self-hydrophilicity.
[0126] The loading of the obtained self-hydrophilic microporous region 3 accounts for 10% of the mass of the low-pressure and low-humidity fuel cell gas diffusion layer.
[0127] The contact angle of the fuel cell gas diffusion layer finally obtained with water is 145°;
[0128] The prepared gas diffusion layer was assembled and tested for membrane electrode. The parameters of the commercial catalyst / membrane complex (CCM) used were: proton exchange membrane thickness 15 μm, anode catalyst (Pt / C) loading 0.3 mg / cm 2 , cathode catalyst (Pt / C) loading 0.4 mg / cm 2 Test conditions: The hydrogen and air ratio is 1.5:2.0; the back pressure of the cathode and anode is 0.3 bar; the battery test temperature is 80°C; the battery is pre-activated for 4 hours before the polarization curve test. Figure 4 and Figure 6 As shown, when both cathode and anode are humidified by 35%, 2.18A / cm2 can be obtained at a voltage of 0.6V. 2; Under the condition of 100% humidification at both cathode and anode, 2.17A / cm can be obtained at 0.4V voltage 2 .
[0129] Example 4
[0130] Design of self-hydrophobic mesoporous region 2: 10 parts of Ketjen black, 1 part of polyethylene glycol and 100 parts of deionized water were mixed and emulsified at room temperature for 3 hours, and continued to stir for 6 hours, thereby obtaining a uniformly dispersed first mixture slurry. After that, the first mixture slurry was evenly coated on the carbon fiber paper, and the coating thickness was controlled to be 100-150μm. After the coating was completed, it was dried in a drying furnace at 75°C for 10 minutes and sintered in a sintering furnace at 400°C for 60 minutes to complete the first treatment; then it was dried in a drying furnace at 75°C for 10 minutes, and hot pressed in a hot press furnace at 450°C under nitrogen atmosphere protection at 1Mpa pressure for 10s to complete the second treatment, thereby obtaining a mesoporous region with self-hydrophobicity.
[0131] Design of self-hydrophilic microporous area 3: After mixing 8 parts of carbon black, 1 part of polydimethylguanidine salt and 50 parts of deionized water, stir at 3500rpm in a cold water bath with a stirrer for 3 hours, disperse at 4000rpm for 3 hours, and stir at 8000rpm for 5 hours to obtain a uniformly dispersed second mixture slurry. Then, the second mixture slurry is evenly coated on the self-hydrophilic mesoporous area 2, and the coating thickness is controlled to be 100-150μm. After the coating is completed, it is dried in a drying furnace at 80℃ for 8 minutes and sintered in a sintering furnace at 300℃ for 60 minutes to complete the third treatment; then it is dried in a drying furnace at 80℃ for 6 minutes again, and the fourth treatment is completed in a hot pressing furnace under nitrogen atmosphere at 550℃ with a pressure of 5Mpa for 15s to obtain a microporous area with self-hydrophilicity.
[0132] The loading of the obtained self-hydrophilic microporous region 3 accounts for 50% of the mass of the low-pressure and low-humidity fuel cell gas diffusion layer.
[0133] The contact angle of the fuel cell gas diffusion layer finally obtained with water is 144°;
[0134] The prepared gas diffusion layer was assembled and tested for membrane electrode. Test conditions: the hydrogen and air ratio was 1.5:2.0; the back pressure of the cathode and anode was 0.3 bar; the battery test temperature was 80°C; and the polarization curve test was pre-activated for 4 hours. The polarization curve test results are shown in Figure 4 and Figure 6 As shown, under the condition of 35% humidification for both cathode and anode, 2A / cm 2 The current density can reach 0.551V; the cathode and anode are both at 85℃, 2A / cm 20.487V can be obtained at the current density;
[0135] Example 5
[0136] Design of self-hydrophobic mesoporous region 2: 10 parts of acetylene black, 1 part of polydimethylguanidine salt and 100 parts of deionized water were mixed and emulsified at room temperature for 5 hours, and continued to stir for 3 hours, thereby obtaining a uniformly dispersed first mixture slurry. After that, the first mixture slurry was evenly coated on the carbon fiber paper, and the coating thickness was controlled to be 100-150μm. After the coating was completed, it was dried in a drying furnace at 80°C for 10 minutes and sintered in a sintering furnace at 300°C for 60 minutes to complete the first treatment; then it was dried in a drying furnace at 80°C for 10 minutes, and hot pressed in a hot press furnace at 650°C under nitrogen atmosphere with a pressure of 1Mpa for 10s to complete the second treatment, thereby obtaining a mesoporous region with self-hydrophobicity.
[0137] Design of self-hydrophilic microporous area 3: After mixing 8 parts of Ketjen black, 1 part of polyethylene glycol and 50 parts of deionized water, stir at 3500rpm in a cold water bath with a stirrer for 3 hours, disperse at 4000rpm for 3 hours, and stir at 8000rpm for 5 hours, thereby obtaining a uniformly dispersed second mixture slurry. After that, the first mixture slurry is evenly coated on the self-hydrophilic mesoporous area 2, and the coating thickness is controlled to be 100-150μm. After the coating is completed, it is dried in a drying furnace at 80℃ for 8 minutes and sintered in a sintering furnace at 300℃ for 60 minutes to complete the third treatment; then it is dried in a drying furnace at 80℃ for 6 minutes again, and hot pressed at 5Mpa pressure for 15s in a hot pressing furnace under nitrogen atmosphere protection at 600℃ to complete the fourth treatment, thereby obtaining a microporous area with self-hydrophilicity.
[0138] The loading of the obtained self-hydrophilic microporous region 3 accounts for 40% of the mass of the low-pressure and low-humidity fuel cell gas diffusion layer.
[0139] The contact angle of the fuel cell gas diffusion layer finally obtained with water is 142°;
[0140] The prepared gas diffusion layer was assembled and tested for membrane electrode. Test conditions: the hydrogen and air ratio was 1.5:2.0; the back pressure of the cathode and anode was 0.3 bar; the battery test temperature was 80°C; and the polarization curve test was pre-activated for 4 hours. The polarization curve test results are shown in Figure 4 and Figure 6 As shown, under the condition of 35% humidification for both cathode and anode, 2A / cm 2 The current density can reach 0.525V; the cathode and anode are both at 85℃, 2A / cm 2 0.458V can be obtained at the current density;
[0141] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.
Claims
1. A gas diffusion layer for improving battery performance, It is characterized in that The invention comprises a macroporous substrate layer (1), a self-hydrophobic mesoporous region (2) and a self-hydrophilic microporous region (3), wherein the self-hydrophobic mesoporous region (2) is attached to the surface of the macroporous substrate layer (1), and the self-hydrophilic microporous region (3) is attached to the surface of the self-hydrophobic mesoporous region (2).
2. A gas diffusion layer for improving battery performance according to claim 1, It is characterized in that The self-hydrophobic mesoporous region (2) and the self-hydrophilic microporous region (3) are stacked alternately; The loading of the self-hydrophilic microporous region (3) accounts for 10%-60% of the mass of the gas diffusion layer.
3. A gas diffusion layer for improving battery performance according to claim 1, It is characterized in that The macroporous substrate layer (1) is selected from any one of carbon fiber paper, carbon paper, carbon cloth or carbon felt; The self-hydrophobic mesoporous region (2) is composed of carbon powder, deionized water and an additive, wherein the ratio of the carbon powder to the additive is 1:9 to 9:1, and the amount of deionized water added is 10 to 50 times the mass of the carbon powder; The self-hydrophilic microporous area (3) is composed of carbon powder, deionized water and an auxiliary agent, wherein the ratio of the carbon powder to the auxiliary agent is 1:9 to 9:1, and the amount of deionized water added is 10 to 30 times the mass of the carbon powder.
4. A gas diffusion layer for improving battery performance according to claim 3, It is characterized in that The carbon powder is selected from any one or more combinations of conductive carbon black, conductive graphite, Ketjen black, carbon nanotubes, carbon fibers or graphene; The auxiliary agent is selected from any one of polydimethylguanidine salt, alkyl glycoside, alkylphenol polyoxyethylene ether, dodecyl dimethyl betaine or polyethylene glycol.
5. A gas diffusion layer for improving battery performance according to claim 1, It is characterized in that The porosity of the self-hydrophobic mesoporous region (2) is greater than 45%, and the proportion of pores greater than 50 nm in the self-hydrophobic mesoporous region (2) accounts for 40%-60% of the total pore size; The porosity of the self-hydrophilic microporous region (3) is above 65%, and the proportion of pores with a diameter of 2-30 nm in the self-hydrophilic microporous region (3) accounts for 30%-50% of the total pore diameter.
6. A method for preparing a gas diffusion layer for improving battery performance as claimed in any one of claims 1 to 5, It is characterized in that The specific steps are as follows: S1, preparing a carbon powder dispersion A, wherein the carbon powder dispersion A is prepared by mixing carbon powder, deionized water and an additive; S2, coating the carbon powder dispersion A obtained in step S1 on the surface of the macroporous substrate layer (1), and obtaining a mesoporous structure after a first treatment; S3, subjecting the mesoporous structure obtained in step S2 to a second treatment to obtain a self-hydrophobic mesoporous region (2); S4, preparing a carbon powder dispersion B, wherein the carbon powder dispersion B is prepared by mixing carbon powder, deionized water and an additive; S5, coating the carbon powder dispersion B obtained in step S4 on the surface of the self-hydrophobic mesoporous region (2) obtained in step S3, and obtaining a microporous structure after a third treatment; S6, subjecting the microporous structure obtained in step S5 to a fourth treatment to obtain a self-hydrophilic microporous region (3), thereby forming a gas diffusion layer.
7. A method for preparing a gas diffusion layer for improving battery performance according to claim 6, It is characterized in that In step S1, appropriate amounts of carbon powder, deionized water and additives are weighed, and the carbon powder and additives are slowly added to the deionized water while stirring, and emulsified at 25-60° C. for 2-6 hours. After the carbon powder is emulsified, it is stirred at room temperature for 5-10 hours to obtain a carbon powder dispersion A; In step S2, the coating load of the carbon powder dispersion A is 0.1-15 mg / cm 2 The coating method of the carbon powder dispersion A is any one or more combinations of blade coating, screen printing, high-pressure gas spraying, ultrasonic spraying, transfer coating, extrusion coating or casting; In step S2, the first treatment includes a drying treatment and a sintering treatment. The drying conditions are as follows: drying temperature 65-180°C, air atmosphere, drying time 5-10 minutes, The sintering conditions are as follows: sintering temperature 250°C-500°C, sintering atmosphere using inert gas, sintering time 1-6h; In step S3, the second treatment includes drying treatment and hot pressing treatment, The drying conditions are as follows: drying temperature 65-180°C, air atmosphere, drying time 5-10 minutes, The conditions of the hot pressing treatment are as follows: hot pressing temperature of 500° C.-1250° C., hot pressing atmosphere of inert gas, hot pressing time of 2-60s, hot pressing pressure of 0.2-5Mpa.
8. A method for preparing a gas diffusion layer for improving battery performance according to claim 6, It is characterized in that In step S4, appropriate amounts of carbon powder, deionized water and additives are weighed, and the carbon powder and additives are slowly added to the deionized water while stirring, and stirred at 3500 rpm for 3 hours in a cold water bath, and then stirred at 8000 rpm for 5 hours to obtain a carbon powder dispersion B; In step S5, the coating load of the carbon powder dispersion B is 0.1-6 mg / cm 2 The coating method of the carbon powder dispersion A is one or more of a doctor blade coating method, a screen printing method, a high-pressure gas spraying method, an ultrasonic spraying method, a transfer coating method, an extrusion coating method or a casting method; In step S5, the third process includes a drying process and a sintering process. The drying conditions are as follows: drying temperature 65-135°C, air atmosphere, drying time 5-10 minutes, The sintering conditions are as follows: sintering temperature 350°C-450°C, sintering atmosphere using inert gas, sintering time 0.5-3h; In step S6, the fourth treatment includes drying treatment and hot pressing treatment, The drying conditions are as follows: drying temperature 65-135°C, air atmosphere, drying time 5-10 minutes, The conditions of the hot pressing treatment are: hot pressing temperature of 500° C.-1000° C., hot pressing atmosphere of inert gas, hot pressing time of 2-30s, hot pressing pressure of 2.5-5Mpa.
9. Application of a gas diffusion layer to improve battery performance, It is characterized in that The gas diffusion layer described in any one of claims 1 to 5 is applied to a proton exchange membrane fuel cell.
10. Application of a gas diffusion layer for improving battery performance according to claim 9, It is characterized in that The proton exchange membrane fuel cell consists of a catalyst layer (4), a proton exchange membrane, a gas diffusion layer and a bipolar plate, wherein the gas diffusion layer is located between the catalyst layer (4) and the bipolar plate, the macroporous substrate layer (1) is attached to the surface of the bipolar plate, and the self-hydrophilic microporous region (3) is connected to the catalyst layer (4).
Citation Information
Cited By
Integrated fuel cell gas diffusion layer structure and preparation method thereof
CN120854591A