Method for producing EUV-permeable film, and shield
By forming a permeable film on the side of the substrate cavity during EUV permeable film manufacturing and etching away the substrate from the opposite side of the cavity, the problem of eaves-like residue of the mask layer is solved, the strength and transmittance of the film are improved, and the film is ensured Exposure accuracy.
Patent Information
- Application Number
- CN202280083827.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-18
- Publication Date
- 2024-10-18
AI Technical Summary
In the existing EUV transmission film manufacturing method, the mask layer is easy to form eaves-shaped residues during the etching process, causing the film to be weak and easily damaged, affecting the transmittance and exposure accuracy.
An EUV permeable film is formed on the side of the cavity of the substrate, and the substrate is etched away from the opposite side of the cavity to make the film self-standing and avoid eaves-like residue of the mask layer.
It improves the quality and durability of the EUV transmission membrane, enhances the membrane's anti-particle adhesion ability, and ensures high transmittance and exposure accuracy.
Smart Images

Figure CN118805142A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for manufacturing an EUV transparent film and a protective member. Background Art
[0002] The miniaturization of semiconductor manufacturing processes is advancing year by year, and various improvements are being made to each process. In particular, in the photolithography process, EUV (extreme ultraviolet) light with a wavelength of 13.5nm has begun to be used instead of the existing ArF exposure wavelength of 193nm. As a result, the wavelength suddenly becomes less than 1 / 10, and its optical properties are completely different. However, there is no material with high transmittance for EUV light, so there is no practical component, such as a protective piece (pellicle) as a particle adhesion prevention film for a photomask (reticle). Therefore, device manufacturers currently manufacture semiconductor devices without using protective pieces.
[0003] Therefore, a Poly-Si-based pellicle has been proposed. For example, Patent Document 1 (Japanese Patent No. 6858817) discloses a pellicle comprising: a core layer comprising a material substantially transparent to EUV radiation, such as (Poly)Si; and an overlying layer comprising a material absorbing IR radiation. However, when the Poly-Si-based pellicle is set to a thickness for maintaining film strength, the EUV transmittance cannot reach the target, i.e., 90%, and has not been put into practical use to date.
[0004] In addition, carbon nanotube (CNT)-based pellicles have been developed (e.g., Patent Document 2 (Japanese Patent Publication No. 2018-194840)), with the expectation of higher EUV transmittance. The actual situation of CNT-based pellicles is that they lack durability in the environment in which the protective parts are used (low-pressure hydrogen atmosphere). When the pellicle is covered with metal to make it durable, the EUV transmittance decreases, and a transmittance at a practical level cannot be achieved.
[0005] Various methods for manufacturing protective films have been proposed. For example, non-patent document 1 (Dario L. Goldfarb, "Fabrication of a full size EUV pellicle based on silicon nitride", Volume 31, Issue 12, PHOTOMASK, SPIE, 2015) discloses a method for manufacturing a SiNx self-supporting film as a protective film. The basic method is as follows. First, a SiNx film to be a protective film is formed on both sides of a Si substrate (process A). Next, a reactive ion etching (RIE) mask for etching the formed SiNx is formed only on one side (process B). Using RIE, a portion of the SiNx is removed to expose the Si substrate (process C). After coating both sides of the Si substrate with amorphous Si, the outer shape of the Si substrate is cut (process D). Finally, the SiNx film is used as a mask to wet-etch the Si substrate to form a SiNx self-supporting film (process E).
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent No. 6858817
[0009] Patent Document 2: Japanese Patent Application Publication No. 2018-194840
[0010] Non-patent literature
[0011] Non-patent literature 1: Dario L. Goldfarb, "Fabrication of a full size EUV pellicle based on silicon nitride", Volume 31, Issue 12, PHOTOMASK, SPIE, 2015 Summary of the invention
[0012] When attempting to manufacture an EUV transparent film as a pellicle membrane with reference to the conventional manufacturing method disclosed in Non-Patent Document 1, it is conceivable to form the EUV transparent film on a substrate and then remove unnecessary portions of the substrate by etching to form a self-standing film. Figure 4A and Figure 4B An example of such a conventional manufacturing process is shown in FIG. In the conventional process, first, a substrate 110 (eg, a Si wafer) is prepared. Figure 4A(a) in the figure). A mask layer 112 such as a SiO2 layer is formed on both sides of the substrate 110. A resist is applied to one or both sides of the substrate 110, and exposure and development are performed in a manner that a hole of a predetermined size of the resist is formed on one side, thereby forming a resist mask for etching (not shown). One side of the substrate 110 is etched to remove the exposed portion of the mask layer 112, thereby forming an opening corresponding to the cavity region C ( Figure 4A (c) in the figure). After removing the resist mask, the substrate 110 is etched using an etching solution such as TMAH (tetramethylammonium hydroxide) solution to thin the cavity region C of the substrate 110 to a desired thickness, thereby forming a cavity 114 ( Figure 4A (d) in FIG. 1 ). The mask layer 112 on the surface opposite to the cavity 114 is etched away to obtain a cavity substrate 115 ( Figure 4B (e) in the figure). An EUV transparent film 116 is formed on the surface of the cavity substrate 115 on the opposite side to the cavity 114 ( Figure 4B Finally, the substrate 110 corresponding to the portion to be formed into a self-supporting film is etched away to form the EUV transparent film 116 into a self-supporting film ( Figure 4B (g) in FIG. 1 ). Thus, a protective member 118 is obtained. The protective member 118 includes a frame 117 and an EUV transparent film 116. The frame 117 includes the substrate 110 and the mask layer 112 remaining in a frame shape.
[0013] However, in the protective member 118 manufactured as described above, Figure 4B (g) and Figure 4C As shown, the inner edge 112a of the frame-shaped mask layer 112 remains in an eave shape extending toward the cavity 114. This is because: when the substrate 110 such as a Si wafer for forming the cavity 114 is etched from the bottom surface, as the etching progresses upward in the figure, side etching also occurs in the lateral direction. If the mask layer 112 is left in a state of extending in an eave shape toward the cavity 114, the weak eave-shaped inner edge 112a is easily damaged and particles (dust) are generated, and the particles adhere to the EUV transparent film 116. If particles adhere to the EUV transparent film 116, EUV light is blocked by the particles during exposure, and poor exposure occurs in which the mask pattern cannot be accurately transferred. On the other hand, it is also conceivable to remove the mask layer 112 after etching the substrate 110, but the time and cost for the removal are generated, and since the EUV transparent film 116 has been completed as a self-supporting film, it is equivalent to adding a process with a high risk of damage to the self-supporting film. Therefore, a manufacturing method is desired that avoids the mask layer 112 from remaining in an eave shape extending toward the cavity 114 .
[0014] The inventors of the present invention have recently obtained the following insight: by forming an EUV transparent film on the surface of the cavity side of the substrate and etching away the substrate from the surface on the opposite side of the cavity, the EUV transparent film is made into a self-standing film, and a high-quality EUV transparent film or protective part can be manufactured using an efficient method that avoids the mask layer from remaining in an eaves shape extending toward the cavity and is less likely to produce particles.
[0015] Therefore, an object of the present invention is to manufacture a high-quality EUV transparent film or protective member by an efficient method that avoids the mask layer from remaining in an eave shape extending toward a cavity and is less likely to generate particles.
[0016] According to one embodiment of the present invention, a method for manufacturing an EUV transparent film is provided, wherein the method comprises the following steps:
[0017] preparing a substrate having a first surface and a second surface;
[0018] Covering the entire area of the first surface and the peripheral area of the second surface except the cavity area located in the center with a mask layer;
[0019] Partially etching away the substrate exposed in the cavity region to form a cavity;
[0020] Etching away the mask layer covering the first surface;
[0021] forming an EUV transparent film on a surface of the substrate on the cavity side and a surface of the mask layer covering the second surface; and
[0022] The substrate is etched away from the first surface until the EUV transmitting film is exposed on the side opposite to the cavity, so that the EUV transmitting film in the cavity region is formed into a self-standing film.
[0023] According to another embodiment of the present invention, there is provided a method for manufacturing an EUV transparent film, comprising the following steps:
[0024] preparing a substrate having a first surface and a second surface;
[0025] Covering the entire area of the first surface and the peripheral area of the second surface except the cavity area located in the center with a mask layer;
[0026] Partially etching away the substrate exposed in the cavity region to form a cavity;
[0027] Etching away the mask layer covering the first surface and the mask layer covering the peripheral area of the second surface;
[0028] forming an EUV transparent film on a surface of the substrate on the cavity side; and
[0029] The substrate is etched away from the first surface until the EUV transmitting film is exposed on the side opposite to the cavity, so that the EUV transmitting film in the cavity region is formed into a self-standing film.
[0030] According to another embodiment of the present invention, there is provided a protective member, comprising:
[0031] a substrate having a first surface and a second surface and having a cavity in the center;
[0032] a mask layer, the mask layer covering the second surface of the substrate; and
[0033] An EUV transparent film continuously covers the surface of the mask layer and the inner surface of the cavity of the substrate and is exposed as a self-supporting film constituting a bottom surface of the cavity at the same height as the first surface.
[0034] According to another embodiment of the present invention, there is provided a protective member, comprising:
[0035] a substrate having a first surface and a second surface and having a cavity in the center; and
[0036] An EUV transparent film continuously covers the second surface of the substrate and the inner surface of the cavity and is exposed as a self-supporting film constituting a bottom surface of the cavity at the same height as the first surface. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1A This is a diagram showing an example of the first half of the process in the method for producing an EUV transmissive film according to one embodiment of the present invention.
[0038] Figure 1B The following is a method for manufacturing an EUV transparent film according to one embodiment of the present invention. Figure 1A A diagram showing an example of the second half of the process.
[0039] Figure 1C The following is a method for manufacturing an EUV transparent film according to one embodiment of the present invention. Figure 1A A diagram showing another example of the second half of the process.
[0040] Figure 2A This is a diagram showing another example of the first half of the process in the method for producing the EUV transparent film of the present invention.
[0041] Figure 2B The following is a diagram showing the method for manufacturing an EUV transparent film according to the present invention. Figure 2A A diagram showing an example of the second half of the process.
[0042] Figure 3AThis is a diagram showing an example of the first half of the process in the method for producing an EUV transmitting film using an SOI substrate according to the present invention.
[0043] Figure 3B The following is a diagram showing the method for manufacturing an EUV transparent film using an SOI substrate according to the present invention. Figure 3A A diagram showing an example of the second half of the process.
[0044] Figure 4A It is a diagram showing the first half of the process of a conventional method for manufacturing an EUV transparent film.
[0045] Figure 4B Next, a method for manufacturing a conventional EUV transparent film is shown. Figure 4A Figure 2 shows the second half of the process.
[0046] Figure 4C is a diagram showing the cavity bottom viewed from the mask layer. Figure 4B An SEM image of a portion of the protective member shown in (g) (region 4C surrounded by a solid line) is obtained. DETAILED DESCRIPTION
[0047] Method for manufacturing EUV permeable film
[0048] The method for manufacturing an EUV transparent film of the present invention includes the following steps: (1) preparation of a substrate, (2) formation of a mask layer, (3) formation of a cavity, (4) removal of the mask layer, (5) formation of an EUV transparent film, and (6) formation of a self-standing film of the EUV transparent film. In the present invention, an EUV transparent film is formed on the surface of the cavity side of the substrate, and the substrate is etched away from the surface on the opposite side of the cavity to form a self-standing film of the EUV transparent film. Accordingly, a high-quality EUV transparent film or protective member can be manufactured by an efficient method that avoids the mask layer from remaining in an eave shape extending toward the cavity and is less likely to generate particles. The details will be clarified in the following description.
[0049] Figure 1A to Figure 4B 1 and 2 show methods for producing EUV transparent films according to some aspects of the present invention.
[0050] (1) Preparation of substrate
[0051] like Figure 1A (a) and Figure 2AAs shown in (a) in the figure, a substrate 10 is prepared. The substrate 10 has a first surface 10a and a second surface 10b. The second surface 10b is the side on which a cavity is formed in a subsequent process, and the first surface 10a is the side on which a cavity is not formed in a subsequent process. The substrate 10 is a support body for forming an EUV transparent film 16 thereon. Finally, in order to make the EUV transparent film 16 self-supporting, the cavity area C is etched away, and the peripheral area P other than this remains in the form of a frame. Therefore, it is desired that the substrate 10 is a material that provides an ideal base for forming the EUV transparent film 16 and can be etched away. Such a substrate 10 is not particularly limited, and is preferably a Si substrate (e.g., a Si wafer).
[0052] The substrate 10 may be a SOI (Silicon on Insulator) substrate. Figure 3A As shown in (a), the SOI substrate 10' is composed of a Si substrate 10c, a SiO2 layer 10d, and a Si layer 10e, and the SiO2 layer 10d is between the Si substrate 10c and the Si layer 10e. In this case, the first surface 10a is the surface of the Si layer 10e, and the second surface 10b is the surface of the Si substrate 10c. By using the SOI substrate 10', the etching can be accurately stopped at the SiO2 layer 10d during the etching (Si etching) of the Si substrate 10c. Therefore, it has the advantage of easily avoiding adverse conditions caused by excessive Si etching (for example, relaxation of the self-supporting film caused by the substrate 10 being too thin).
[0053] (2) Formation of mask layer
[0054] like Figure 1A (b) and (c) and Figure 2A As shown in (b) and (c) in the figure, the entire area of the first surface 10a in the substrate 10 and the peripheral area P of the second surface 10b except the cavity area C located in the center are covered with a mask layer 12. The mask layer 12 can be made of a material that is resistant to corrosion by a wet etching solution for etching the substrate 10 (for example, TMAH for Si etching), and is not particularly limited. The preferred mask layer 12 is a SiO2 film. The mask layer 12 can be formed by any method. For example, the formation of the SiO2 film is preferably carried out by chemical vapor growth (CVD) or thermal oxidation. In addition, the thickness of the SiO2 film is preferably 100 to 1000 nm.
[0055] The mask layer 12 can be formed as follows. First, the mask layer 12 ( Figure 1A (b) and Figure 2A(b) in the figure). Next, a resist is applied to the first surface 10a and the second surface 10b, and exposure and development are performed in a manner that an opening of the resist corresponding to the cavity region C can be formed on the second surface 10b side, thereby forming a resist mask (not shown). The size of the cavity region C corresponds to the size of the EUV transparent film 16 to be produced. Wet etching is performed using an etching solution such as hydrofluoric acid to etch away the exposed portion of the mask layer 12 at the opening of the resist mask, and then the resist mask is removed. In this way, a mask layer 12 having an opening in the cavity region C is obtained ( Figure 1A (c) and Figure 2A (c) in the figure.
[0056] (3) Cavity formation
[0057] like Figure 1A (d) and Figure 2A As shown in (d) in the figure, the exposed cavity region C of the substrate 10 is partially etched away to form a cavity 14. That is, with respect to the cavity region C of the substrate 10, after the EUV transparent film 16 is formed thereon, it is removed by etching. Therefore, in order to perform etching efficiently and in a short time, it is desirable to thin the thickness of the substrate 10 in the region where the self-supporting film is to be formed (i.e., the cavity region C) in advance. Therefore, the cavity 14 is formed by etching the substrate 10 through the opening of the self-mask layer 12, so that the cavity region C of the substrate 10 is thinned. The etching of the substrate 10 may be either wet etching or dry etching, and there is no particular limitation. The etchant may be a substance that can etch the substrate 10, and there is no particular limitation. For example, in the case of etching using the DeepRIE method, which is a dry process, Figure 1A As in (d) in the figure, the Si substrate is etched perpendicularly to the mask layer 12, so the mask layer 12 is less likely to remain in the form of an eaves, which is preferred. In the case of wet etching of the Si substrate, a TMAH (tetramethylammonium hydroxide) solution is preferred. If the TMAH solution is used under appropriate conditions, very good etching can be achieved by utilizing anisotropic etching for Si. In particular, with regard to anisotropic etching, when forming the cavity 14, etching can be performed in a straight line along the thickness direction of the substrate 10 (it is less likely to go around to the bottom of the mask layer 12), so the mask layer 12 is less likely to remain in the form of an eaves, which is more advantageous than isotropic etching. Nevertheless, in the case of wet etching, as in Figure 2A As shown in (d) in FIG. 1 , the Si substrate is not only etched in the vertical direction, but also etched in the lateral direction due to the detour of the liquid. Therefore, the mask layer 12 sometimes temporarily remains in the form of an eave. Figure 2A and Figure 2B In the scheme shown, in the subsequent process, Figure 2AAs shown in (e) in FIG. 1 , the mask layer 12 is removed, so that the mask layer 12 can be prevented from remaining in an eaves shape.
[0058] When the SOI substrate 10' is used, the formation of the cavity 14 is preferably performed as follows: Figure 3A (d) and Figure 3B As shown in (e), the Si substrate 10c is etched away until the cavity 14 reaches the SiO2 layer 10d ( Figure 3A (d)), the SiO2 layer 10d is etched away from the cavity 14 separately ( Figure 3B (e) in the figure). The etching of the Si substrate 10c can be either dry etching or wet etching as described above. In this scheme, since the etching can be accurately stopped at the SiO2 layer 10d, it is possible to avoid adverse conditions caused by excessive Si etching (for example, relaxation of the self-supporting film caused by the substrate 10 being too thin). The subsequent etching and removal of the SiO2 layer 10d exposed in the cavity 14 is preferably performed using hydrofluoric acid. As a result, in the cavity 14, the Si layer 10e is exposed as a self-supporting film.
[0059] (4) Removal of mask layer
[0060] like Figure 1B As shown in (e) in the figure, the mask layer 12 covering the first surface 10a is etched away. Thus, a substrate 10 having a cavity 14 (i.e., a cavity substrate 15) is obtained. The etching removal of the mask layer 12 can be performed by wet etching using an etching solution such as hydrofluoric acid as described above. Thus, a cavity substrate 15 having a cavity 14 is obtained. The mask layer 12 covering the peripheral area P of the second surface 10b can be left. That is, in the subsequent film forming process, an EUV transparent film 16 can be formed on the mask layer 12 covering the peripheral area P of the second surface 10b. Thus, the mask removal process can be omitted.
[0061] However, as a variation, the mask layer 12 covering the peripheral region P of the second surface 10b may also be etched away. Figure 1C (e') and Figure 2B As shown in (e) in FIG. 1 , the mask layer 12 covering the first surface 10a and the mask layer 12 covering the peripheral region P of the second surface 10b can both be etched away. By also etching away the mask layer 12 covering the peripheral region P of the second surface 10b, since the mask layer 12 is completely absent, it is possible to avoid the mask layer 12 remaining in an eaves shape.
[0062] When using the SOI substrate 10', similarly, Figure 3B As shown in (f) in FIG. 1 , the mask layer 12 covering the first surface 10 a may be removed by etching in the same manner as described above.
[0063] (5) Formation of EUV Transmitting Film
[0064] like Figure 1B As shown in (f) in FIG. 1 , an EUV transparent film 16 is formed on the surface of the substrate 10 on the cavity 14 side and on the surface of the mask layer 12 covering the second surface 10b. Alternatively, Figure 1C (f') and Figure 2B In the variation shown in (f) of FIG. 1 , the EUV transparent film 16 is formed on the surface of the substrate 10 on the side of the cavity 14. That is, in the conventional method, the EUV transparent film 16 is formed on the flat surface on the opposite side to the surface on which the cavity 14 is formed, but in the present invention, the film is formed from the non-flat surface on the side of the substrate 10 on which the cavity 14 is formed (when the mask layer 12 is present on the surface, from the mask layer 12). The advantages brought about by this will be described in the following process.
[0065] The EUV permeable film 16 preferably has a main layer composed of at least one metal selected from the group consisting of Ni, Al, Be, Cr and Ga. These metals have the following advantages: when the substrate 10 such as a Si substrate is etched away with XeF2 gas to make the EUV permeable film 16 self-standing, it is not easily corroded by XeF2 gas. This can be proved by the fact that, compared with the boiling point of XeF2 of 114°C, the boiling points of the fluorides of Ni, Al, Be, Cr and Ga are extremely high, reaching 1750°C (NiF2), 1260°C (AlF3), 1169°C (BeF2), 1100°C (CrF2), and 950°C (GaF3). This is because: a high boiling point means a low vapor pressure, and for this reason, it is not easily etched by XeF2 gas. From the perspective of being an EUV permeable film, a particularly preferred main layer is composed of Be (metal beryllium). Be has a higher EUV transmittance than Si and C, and therefore exhibits a practically high EUV transmittance (e.g., 93% or more). In addition, from the viewpoint of protecting the main layer, the EUV transparent film 16 preferably further includes a protective layer covering at least one side (preferably both sides) of the main layer. When the main layer is composed of Be, preferred examples of materials constituting the protective layer include beryllium nitride, beryllium oxide, and beryllium fluoride.
[0066] The formation of the EUV transparent film 16 can be performed by any film forming method. As examples of preferred film forming methods, sputtering or CVD (chemical vapor deposition) can be cited. As described above, in the present invention, the film is formed from the non-flat surface of the substrate 10 on the side where the cavity 14 is formed. However, even if it is a film forming method with poor tortuosity such as sputtering, since the thickness of the substrate 10 such as a Si substrate is generally less than 1 mm, there will not be a large difference in film thickness when the film is formed on the inner surface of the cavity 14 compared to when the film is formed on a flat surface.
[0067] For example, in the case of making a three-layer structure of beryllium nitride / beryllium / beryllium nitride, it is preferred that: the beryllium film as the main layer is made by sputtering using a pure Be target, and the beryllium nitride film as the protective layer is made by reactive sputtering. The reactive sputtering can be performed as follows: For example, in sputtering using a pure Be target, nitrogen is introduced into the chamber, whereby beryllium and nitrogen react to generate beryllium nitride. As described later, the beryllium nitride film may have a gradient composition layer (a layer composed of a nitrogen concentration gradient region described later) in which the nitrogen concentration decreases toward the beryllium film. An example of the preferred sequence at this time is as follows. First, in addition to introducing Ar, which is usually used as an atmosphere gas, nitrogen is also introduced, and Be sputtering is performed at the same time, thereby forming a beryllium nitride film. After forming a beryllium nitride film of a specified thickness, Be sputtering is performed while reducing the amount of nitrogen, thereby forming a gradient composition layer. After the gradient composition layer is formed, the subsequent introduction of nitrogen is stopped, and a beryllium layer is formed with a specified thickness. Thereafter, a gradient composition layer was formed again while increasing the amount of nitrogen gas introduced, and a beryllium nitride film was formed again as the outermost layer by reactive sputtering.
[0068] In addition, as another method, the preparation of beryllium nitride can also be carried out as follows: after forming the beryllium film, irradiate nitrogen plasma to cause beryllium to undergo a nitridation reaction to generate beryllium nitride. In short, the synthesis method of beryllium nitride is not limited to these methods. It should be noted that the beryllium target for forming the beryllium nitride film and the beryllium target for forming the beryllium film preferably use separate targets, but the same target can also be used in the formation of the beryllium nitride film and the formation of the beryllium film. It should be noted that the beryllium nitride film and the beryllium film can be formed in a sputtering device with one chamber as in the embodiment described later, or a sputtering device with two chambers can be used to form the beryllium nitride film and the beryllium film in each chamber respectively.
[0069] When using the SOI substrate 10', similarly, Figure 3B As shown in (g) in FIG. 1 , the EUV transmitting film 16 may be formed on the surface of the SOI substrate 10 ′ on the cavity 14 side and the surface of the mask layer 12 covering the second surface 10 b in the same manner as described above.
[0070] (6) Self-supporting EUV-transmitting film
[0071] like Figure 1B (g) Figure 1C (g') and Figure 2B As shown in (g) in FIG. 1 , the substrate 10 is etched away from the first surface 10a until the EUV transparent film 16 is exposed on the side opposite to the cavity 14, so that the EUV transparent film 16 in the cavity region C is formed into a self-standing film. In this way, the etching of the substrate 10 (for example, a Si substrate) for forming the EUV transparent film 16 into a self-standing film is different from the conventional process of etching the substrate 10 from the inner surface of the cavity 14, and is performed from the flat surface of the substrate 10 on the side opposite to the cavity 14. This brings the following advantages.
[0072] First, the EUV transparent film 16 has resistance to the etchant (or has a protective film with resistance to the etchant), and therefore functions as a protective film on the surface of the cavity 14 of the substrate 10 such as the Si substrate, and prevents the substrate 10 on the inner surface of the cavity 14 from being side-etched. This can prevent the mask layer 12 from remaining in an eaves shape. That is, as described above, in the conventional process, side etching occurs on the side of the cavity 14, resulting in the existence of Figure 4B (g) and Figure 4C The problem is that the mask layer 112 shown in the figure remains in the shape of an eave extending toward the cavity 114. In this state, the inner edge portion 112a of the eave with weak strength is damaged to generate particles (dust), and the particles are easily attached to the EUV transparent film 116. If particles are attached to the EUV transparent film 116, the EUV light is blocked by the particles during exposure, resulting in poor exposure in which the mask pattern cannot be accurately transferred. In contrast, in the method of the present invention, the cavity 14 and the mask layer 12 are covered with the EUV transparent film 16, so side etching does not occur, and as a result, the mask layer 12 can be prevented from remaining in the shape of an eave. It should be noted that it is also possible to consider removing the mask layer 12 after etching the substrate 10, but this will generate time and cost for the removal, and since the EUV transparent film 16 has been completed as a self-supporting film, it is equivalent to adding a process with a high risk of damage to the self-supporting film. The method of the present invention does not require the addition of such a process.
[0073] Second, the etching of the substrate 10 is performed on a flat surface without the cavity 14. Therefore, compared with etching performed on the surface of the substrate 10 on the cavity 14 side, etching unevenness caused by the difference in shape between the flat portion and the non-flat portion (corner, etc.) is less likely to occur, and uniform etching can be performed. That is, in the etching performed from the inner surface of the cavity 14 in the conventional process, etching unevenness due to position occurs due to uneven diffusion of the etchant, but in the method of the present invention, the EUV transparent film 16 is made into a self-standing film by etching the flat surface, so etching unevenness is less likely to occur. Therefore, according to the method of the present invention, a high-quality EUV transparent film 16 or a protective member 18 can be manufactured.
[0074] As described above, according to the method of the present invention, a high-quality EUV transparent film or protective member can be manufactured by an efficient method that avoids the mask layer 12 from remaining in an eave shape extending toward the cavity 14 and is less likely to generate particles.
[0075] The etching of the substrate 10 for forming the EUV transmitting film 16 into a self-standing film is preferably performed by etching that does not corrode the EUV transmitting film 16. For example, when etching a Si substrate, it is preferable to perform etching using XeF2 gas.
[0076] When using the SOI substrate 10', similarly, Figure 3AAs shown in (h) in FIG. 1 , regarding the self-supporting film formation of the EUV transparent film 16, the SOI substrate 10' (specifically, the Si layer 10e) is etched away from the first surface 10a in the same manner as described above until the EUV transparent film 16 is exposed on the side opposite to the cavity 14. As a result of the self-supporting film formation of the EUV transparent film 16 in the cavity region C, the self-supporting film portion of the EUV transparent film 16 and the SiO2 layer 10d are exposed on the same plane on the side opposite to the cavity 14. In this scheme, since the SiO2 layer 10d exists under the Si layer 10e, even if the etching time management in the XeF2 etching for removing the Si layer 10e is not strictly performed, the etching can be stopped at the SiO2 layer 10d.
[0077] As a result of etching away the substrate 10 or the SOI substrate 10', the EUV transparent film 16 in the cavity region C becomes a self-standing film. On the other hand, in the peripheral region P excluding the cavity region, three layers of the substrate 10, the mask layer 12, and the EUV transparent film 16 remain ( Figure 1B (g)), the substrate 10 and the EUV transparent film 16 are two layers ( Figure 1C (g') and Figure 2B (g)), or the four layers of SiO2 layer 10d, Si substrate 10c, mask layer 12 and EUV transparent film 16 ( Figure 3B In (h)), a frame 17 for supporting the self-supporting film is formed. Thus, a protection member 18 having the EUV transmitting film 16 (protective membrane) and the frame 17 is obtained.
[0078] Protective parts
[0079] As described above, the manufacturing method of the present invention can manufacture an EUV transparent film and a protection member including the EUV transparent film.
[0080] like Figure 1B As shown in (g) of FIG. 1 , a protective member 18 of one embodiment of the present invention comprises: a substrate 10, a mask layer 12, and an EUV transparent film 16. The substrate 10 has a first surface 10a and a second surface 10b, and has a cavity 14 in the center. The mask layer 12 covers the second surface 10b of the substrate 10. The EUV transparent film 16 continuously covers the surface of the mask layer 12 and the inner surface of the cavity 14 of the substrate 10, and is exposed as a self-supporting film constituting the bottom surface of the cavity 14 at the same height as the first surface 10a.
[0081] like Figure 1C (g') and Figure 2BAs shown in (g) of FIG. 1 , another embodiment of the protective member 18' of the present invention includes a substrate 10 and an EUV transparent film 16. The substrate 10 has a first surface 10a and a second surface 10b, and has a cavity 14 in the center. The EUV transparent film 16 continuously covers the second surface 10b of the substrate 10 and the inner surface of the cavity 14, and is exposed as a self-supporting film constituting the bottom surface of the cavity 14 at the same height as the first surface 10a.
[0082] In either scenario, Figure 3B As shown in (h) of FIG. 1 , the substrate 10 is composed of two layers, namely, a Si substrate 10c and a SiO 2 layer 10d. This is a typical layer structure of a protective member 18" manufactured using an SOI substrate 10'.
[0083] As described above, the protective member 18, 18' or 18" has the EUV transparent film 16 (protective film) and the frame 17. The frame 17 is composed of three layers ( Figure 1B (g)), the substrate 10 and the EUV transparent film 16 are two layers ( Figure 1C (g') and Figure 2B (g))), or the SiO2 layer 10d, Si substrate 10c, mask layer 12 (can be omitted) and EUV transparent film 16 these three layers or four layers ( Figure 1C The (h)) structure in .
[0084] Optimal solution for EUV permeable membrane
[0085] As described above, the EUV transparent film of the preferred embodiment comprises: a main layer, and a protective layer covering at least one side (preferably both sides) of the main layer. In this embodiment, the main layer is preferably composed of metal beryllium, and on the other hand, the protective layer is preferably composed of beryllium nitride. By combining the main layer composed of metal beryllium and the protective layer composed of beryllium nitride in this way, an EUV transparent film having both a practically high EUV transmittance (for example, 93% or more) and durability in a low-pressure hydrogen atmosphere environment can be provided.
[0086] The main layer of this scheme is preferably composed of metal beryllium. However, the main layer does not need to be composed entirely of metal beryllium. Preferably, more than 99% by weight, more preferably more than 99.5% by weight, and further preferably more than 99.8% by weight of the main layer is composed of metal beryllium. It can ensure the basic functions of a protective film (anti-particle adhesion function, etc.) and contribute to the realization of a high practical EUV transmittance. From this point of view, the thickness of the main layer is preferably 10 to 70 nm, more preferably 15 to 50 nm, and further preferably 20 to 35 nm.
[0087] The protective layer of this scheme is a layer used to protect the metal beryllium layer, that is, the main layer. Therefore, the protective layer only needs to cover at least one side of the main layer, but it is preferred that both sides of the main layer be covered with the protective layer. The protective layer is preferably composed of beryllium nitride. However, the main layer does not need to be completely composed of beryllium nitride, and more than 99% by weight, preferably more than 99.5% by weight, and more preferably more than 99.8% by weight of the main layer can be composed of beryllium nitride. The EUV transmittance of beryllium nitride is high, so if compared with the same thickness, the EUV transmittance is higher than that of a beryllium film formed with a Ru layer. According to theoretical calculations, the transmittance when a Ru film with a thickness of 3nm is formed on both sides of a beryllium film with a thickness of 30nm is 85.8%, while the transmittance when a beryllium nitride with a thickness of 3nm is formed on both sides of a beryllium film with a thickness of 30nm is 91.1%. The transmittance when a beryllium nitride layer with a thickness of 2nm and a gradient composition layer with a thickness of 1nm (a layer composed of a nitrogen concentration gradient region described later) is formed on both sides of a beryllium film with a thickness of 30nm exceeds 91.1%. By forming a dense beryllium nitride layer on both sides of the beryllium layer, it is possible to inhibit it from reacting with the XeF2 gas used for etching the Si substrate described later. In addition, since beryllium is a very reactive material, it is easily oxidized to form beryllium oxide, but oxidation can be inhibited by the formation of beryllium nitride. As described above, the advantage of using a beryllium nitride layer as a protective layer is that the EUV transmittance is increased, the beryllium film (main layer) in the etching process is protected, and oxidation is prevented.
[0088] The thickness of the protective layer of this embodiment is preferably 5nm or less, and more preferably 3nm or less. If a protective layer with a thickness of 3nm is formed on both sides of the main layer, the EUV transmittance of the 3nm thick beryllium nitride film is as high as 95%, which is significantly higher than the 90% of the Ru film. There is no special lower limit on the thickness of the protective layer. If it is too thin, it is difficult to cover the entire surface of the main layer, or the crystallinity of beryllium nitride is poor, and it is difficult to obtain the physical properties of beryllium nitride. Therefore, it is typically greater than 1nm. It should be noted that in this specification, the term "beryllium nitride" means: not only a stoichiometric composition such as Be3N2 is allowed, but also a stoichiometric composition such as Be3N 2-x (wherein 0<x<2) is a general composition of such non-stoichiometric compositions.
[0089] The protective layer preferably has a nitrogen concentration gradient region in which the nitrogen concentration decreases as it approaches the main layer. That is, the composition of the beryllium nitride constituting the protective layer as described above may include a stoichiometric composition such as Be3N2 to Be3N 2-x(wherein 0<x<2) is a non-stoichiometric composition. In this case, the beryllium nitride constituting the protective layer preferably has a gradient composition that approaches a beryllium-rich composition as it approaches the main layer. Accordingly, the adhesion between the protective layer (i.e., the beryllium nitride layer) and the main layer (i.e., the metal beryllium layer) can be improved, and the stress caused by the thermal expansion difference between the two layers can be alleviated. That is, the adhesion between the two layers can be improved to suppress peeling, or the two layers can be made less likely to peel off by absorbing EUV light and becoming a thermal expansion mitigation layer between the two layers at high temperatures. The thickness of the nitrogen concentration gradient region is preferably smaller than the thickness of the protective layer. That is, the entire region without the thickness of the protective layer is the nitrogen concentration gradient region. For example, preferably only a portion of the thickness of the protective layer, such as a region preferably 10 to 70% of the thickness of the protective layer, and more preferably a region 15 to 50% of the thickness of the protective layer is the nitrogen concentration gradient region.
[0090] The EUV permeable film 16 of the present embodiment can have a practically high EUV transmittance, which is preferably 91% or more, more preferably 92% or more, and further preferably 93% or more. The higher the EUV transmittance, the better, so the upper limit is not particularly limited, but the EUV transmittance of the EUV permeable film 16 of the present embodiment can be typically 99% or less, more typically 98% or less, and further typically 95% or less.
[0091] Example
[0092] The present invention is further specifically described through the following examples.
[0093] Example 1
[0094] according to Figure 1A and Figure 1B A composite self-supporting film (EUV transmitting film) having a three-layer structure of beryllium nitride / beryllium / beryllium nitride was produced in the order shown below.
[0095] (1) Preparation of cavity substrate
[0096] As the substrate 10, a Si wafer ( Figure 1A On both sides of the Si wafer, a SiO2 layer with a thickness of 1 μm is formed by thermal oxidation as a mask layer 12 ( Figure 1A (b) in the figure). A resist is applied to both sides of a Si wafer having a SiO2 layer formed thereon, and exposure and development are performed in such a manner that a hole of 110 mm × 140 mm in the resist is formed on one side as a cavity area C, thereby forming a resist mask for SiO2 etching (not shown). One side of the substrate is wet-etched with hydrofluoric acid, thereby etching away the exposed portion of the SiO2 film in the cavity area C to expose the Si wafer, and then the resist mask is removed with an ashing device ( Figure 1AThen, the Si wafer is dry-etched (anisotropically etched) along the thickness direction by reactive ion etching from the exposed portion of the cavity region C to form a cavity 14 ( Figure 1A (d) in the figure). At this time, the etching time is calculated in advance based on the etching rate so that the thickness of the Si wafer remaining as the bottom of the cavity 14 is about 10 μm, and etching is performed at this etching time. The SiO2 layer on the side opposite to the cavity 14 is removed and cleaned with hydrofluoric acid to prepare a cavity substrate 15 ( Figure 1B (e) in the figure.
[0097] (2) Formation of composite membrane
[0098] On the cavity 14 forming surface of the cavity substrate 15 obtained in (1) above, a composite film of a three-layer structure of beryllium nitride / beryllium / beryllium nitride is formed in the entire region including the cavity region C (inner surface of the cavity 14) and the peripheral region P (SiO2 layer) as follows ( Figure 1B (f) in the figure). First, the cavity substrate 15 is fixed to the sputtering device and a pure Be target is installed. The chamber is evacuated and adjusted to an internal pressure of 0.5 Pa and a flow ratio of argon gas to nitrogen gas of 1:1, and reactive sputtering is performed, and the reactive sputtering is terminated when the beryllium nitride stacking time is 2nm. Next, nitrogen gas is not introduced, and only argon gas is used for sputtering, and the sputtering is terminated when the beryllium nitride stacking time is 25nm. After that, nitrogen gas is introduced again in the same way as the initial step, and reactive sputtering is performed at the same time, and the reactive sputtering is terminated when the beryllium nitride stacking time is 2nm. Thus, a composite film of beryllium nitride 2nm / beryllium 25nm / beryllium nitride 2nm is formed as an EUV transparent film 16.
[0099] (3) Self-supporting membrane
[0100] The cavity substrate 15 with EUV permeable film 16 obtained in (2) is fixed in the chamber of the XeF2 etcher in a manner that the surface on the opposite side of the cavity 14 (i.e., the exposed surface of the Si substrate 10) is etched with XeF2, and the chamber is fully evacuated. At this time, if there is residual moisture in the chamber, it reacts with the XeF2 gas to produce hydrofluoric acid, causing corrosion or unexpected etching of the etcher, so it is fully evacuated. As needed, the chamber is repeatedly evacuated and nitrogen is introduced to reduce residual moisture. After fully evacuating, the valve between the XeF2 raw material bottle and the preparatory chamber is opened. As a result, XeF2 sublimates, and XeF2 gas is also accumulated in the preparatory chamber. After XeF2 gas is fully accumulated in the preparatory chamber, the valve between the preparatory chamber and the chamber is opened, and XeF2 gas is introduced into the chamber. XeF2 gas reacts with Si to generate SiF4 and Xe. The boiling point of SiF4 is -95°C, so the generated SiF4 evaporates quickly, and a reaction occurs between the newly exposed Si substrate and F. Si etching continues, and after the XeF2 in the chamber is reduced, the chamber is evacuated, and XeF2 gas is introduced into the chamber again for etching. In this way, evacuation, XeF2 gas introduction, and etching are repeated, and etching is continued until the Si substrate 10 corresponding to the portion to be self-supporting disappears. After the unnecessary portion of the Si substrate disappears, the etching is terminated. Thus, a composite self-supporting film having an EUV transparent film 16 and a protective member 18 (frame 17 supporting the composite self-supporting film) is obtained. Figure 1B (g) in FIG. 1 ). The EUV transmittance of the obtained composite self-supporting film having a three-layer structure of beryllium nitride / beryllium / beryllium nitride was measured and found to be 92.8%.
[0101] Example 2
[0102] according to Figure 2A and Figure 2B A composite self-supporting film (EUV transmitting film) having a three-layer structure of beryllium nitride / beryllium / beryllium nitride was produced in the order shown below.
[0103] (1) Preparation of cavity substrate
[0104] As the substrate 10, a Si wafer ( Figure 2A On both sides of the Si wafer, a SiO2 layer with a thickness of 1 μm is formed by thermal oxidation as a mask layer 12 ( Figure 2A(b) in the figure). A resist is applied to both sides of a Si wafer having a SiO2 layer formed thereon, and exposure and development are performed in such a manner that a hole of 110 mm × 140 mm in the resist is formed on one side as a cavity area C, thereby forming a resist mask for SiO2 etching (not shown). One side of the substrate is wet-etched with hydrofluoric acid, thereby etching away the exposed portion of the SiO2 film in the cavity area C to expose the Si wafer, and then the resist mask is removed with an ashing device ( Figure 2A Then, the Si wafer is wet-etched (anisotropically etched) along the thickness direction using TMAH solution from the exposed portion of the cavity region C to form a cavity 14 ( Figure 2A (d) in the figure). At this time, the etching time is calculated in advance based on the etching rate so that the thickness of the Si wafer remaining as the bottom of the cavity 14 is about 10 μm, and etching is performed at this etching time. At this time, etching based on the TMAH solution is anisotropic etching, which is mainly performed upward in the figure, but etching is also performed in the lateral direction. Therefore, Figure 2A As shown in (d) in FIG. 1 , the mask layer 12 forms an eaves structure. Then, the mask layers 12 on both sides of the substrate are removed and cleaned using hydrofluoric acid to prepare a cavity substrate 15' ( Figure 2B (e) in the figure.
[0105] (2) Formation of composite membrane
[0106] On the cavity 14 forming surface of the cavity substrate 15' obtained in (1) above, a composite film having a three-layer structure of beryllium nitride / beryllium / beryllium nitride is formed as an EUV transmission film 16 in the same manner as in Example 1, including the cavity region C (inner surface of the cavity 14) and the peripheral region P. Figure 2B (f) in the figure.
[0107] (3) Self-supporting membrane
[0108] The cavity substrate 15' with the EUV transparent film 16 obtained in (2) above is fixed in the chamber of a XeF2 etcher in such a manner that the surface opposite to the cavity 14 (i.e., the exposed surface of the Si substrate 10) is etched with XeF2, and XeF2 etching is performed in the same manner as in Example 1. Thus, the Si substrate 10 at the bottom of the cavity 14 is etched away to obtain a composite self-supporting film having the EUV transparent film 16 and a protective member 18' (frame 17) supporting the composite self-supporting film. Figure 2B (g) in Example 2). At this time, unlike Example 1, in Example 2, the mask layer 12 is removed, so that the eaves structure caused by the mask layer 12 is not formed, so the mask layer 12 is not damaged to generate particles. The EUV transmittance of the composite self-supporting film having the three-layer structure of beryllium nitride / beryllium / beryllium nitride was measured and the result was 93.1%.
[0109] Example 3
[0110] according to Figure 3A and Figure 3B A composite self-supporting film (EUV transmitting film) having a three-layer structure of beryllium nitride / beryllium / beryllium nitride was produced in the order shown below.
[0111] (1) Preparation of cavity substrate
[0112] As the substrate 10', an SOI substrate ( Figure 3A On both sides of the SOI substrate 10', a SiO2 layer with a thickness of 1 μm is formed by thermal oxidation as a mask layer 12 ( Figure 3A (b) in the figure). A resist is applied to both sides of an SOI substrate 10' on which a SiO2 layer is formed, and exposure and development are performed in such a manner that a hole of 110 mm x 140 mm in the resist can be formed on one side as a cavity area C, thereby forming a resist mask for SiO2 etching (not shown). One side of the substrate is wet-etched with hydrofluoric acid, thereby etching away the exposed portion of the SiO2 film in the cavity area C, exposing the SOI substrate 10', and then the resist mask is removed using an ashing device ( Figure 3A Then, the Si substrate 10c is dry-etched (anisotropically etched) along the thickness direction by reactive ion etching from the exposed portion of the cavity region C until the SiO2 layer 10d is exposed, thereby forming a cavity 14 ( Figure 3A The exposed SiO2 layer 10d is removed by etching with hydrofluoric acid to expose the Si layer 10e ( Figure 3B (e) in the figure). Then, the mask layer 12 (SiO2 layer) on the side opposite to the cavity 14 is removed by etching with hydrofluoric acid to prepare a cavity substrate 15 for forming an EUV transparent film. Figure 3B (f) in the figure.
[0113] (2) Formation of composite membrane
[0114] On the cavity 14 forming surface of the cavity substrate 15" obtained in (1) above, a composite film of a three-layer structure of beryllium nitride / beryllium / beryllium nitride is formed as an EUV transmission film 16 in the same manner as in Example 1, including the cavity region C (inner surface of the cavity 14) and the peripheral region P (SiO2 layer). Figure 3B (g) in the figure.
[0115] (3) Self-supporting membrane
[0116] The cavity substrate 15" with the EUV transparent film 16 obtained in the above (2) is fixed in the chamber of the XeF2 etcher in such a manner that the surface opposite to the cavity 14 (i.e., the exposed surface of the Si layer 10e) is etched with XeF2, and XeF2 etching is performed in the same manner as in Example 1. As a result, the Si layer 10e at the bottom of the cavity 14 is etched away to obtain a composite self-supporting film having the EUV transparent film 16 and a protective member 18" of a frame 17 supporting the composite self-supporting film. Figure 3B (h) in Example 1). At this time, unlike Example 1, in Example 2, there is a SiO2 layer 10d under the Si layer 10e, so even if the etching time management in the XeF2 etching for removing the Si layer 10e is not strictly performed, the etching can be stopped at the SiO2 layer 10d. This is advantageous in terms of preventing over-etching. The EUV transmittance of the obtained composite self-supporting film of the three-layer structure of beryllium nitride / beryllium / beryllium nitride was measured and the result was 93.3%.
[0117] Results and Investigation
[0118] In Examples 1 to 3, the mask layer (SiO2 layer in Examples 1 to 3) used to form the cavity on the substrate and the inner surface of the cavity are covered with a composite film of beryllium nitride / beryllium / beryllium nitride, so the inner surface of the cavity is not etched during XeF2 etching. That is, side etching does not occur. In Examples 1 to 3, the Si thickness at the bottom of the cavity is 10 μm, so if the existing method is used, side etching of about 10 μm will also occur, and the mask layer will become an eaves structure extending toward the cavity. When the mask layer is an eaves structure, since the mask layer is composed of SiO2 with a thickness of only 1 μm, it has low strength and is easily damaged. In addition, if it is damaged, particles (dust) will be generated and attached to the self-supporting film. In the case where the self-supporting film is used as a protective film, if particles are attached to the self-supporting film, the EUV light will be blocked by the particles during exposure, and the mask pattern cannot be accurately transferred, resulting in poor exposure. In this regard, since the eaves structure is not formed in the self-supporting film produced in the present invention, there is no problem that the eaves structure is damaged and adheres to the self-supporting film.
Claims
1. A method for manufacturing an EUV transparent film, in, Including the following processes: preparing a substrate having a first surface and a second surface; Covering the entire area of the first surface and the peripheral area of the second surface except the cavity area located in the center with a mask layer; Partially etching away the substrate exposed in the cavity region to form a cavity; Etching away the mask layer covering the first surface; forming an EUV transparent film on a surface of the substrate on the cavity side and a surface of the mask layer covering the second surface; as well as The substrate is etched away from the first surface until the EUV transmitting film is exposed on the side opposite to the cavity, so that the EUV transmitting film in the cavity region is formed into a self-standing film.
2. A method for manufacturing an EUV transparent film, in, Including the following processes: preparing a substrate having a first surface and a second surface; Covering the entire area of the first surface and the peripheral area of the second surface except the cavity area located in the center with a mask layer; Partially etching away the substrate exposed in the cavity region to form a cavity; Etching away the mask layer covering the first surface and the mask layer covering the peripheral area of the second surface; forming an EUV transparent film on a surface of the substrate on the cavity side; as well as The substrate is etched away from the first surface until the EUV transmitting film is exposed on the side opposite to the cavity, so that the EUV transmitting film in the cavity region is formed into a self-standing film.
3. The method for producing an EUV transparent film according to claim 1 or 2, in, The EUV transmitting film includes a main layer composed of metal beryllium.
4. The method for producing an EUV transparent film according to claim 3, in, The EUV transmitting film includes a protective layer covering at least one surface of the main layer.
5. The method for producing an EUV transparent film according to any one of claims 1 to 4, in, The substrate is a Si substrate.
6. The method for producing an EUV transparent film according to any one of claims 1 to 4, in, The substrate is an SOI substrate, and the SOI substrate comprises a Si substrate, a Si layer, and a SiO 2 The first surface is a surface of the Si layer, and the second surface is a surface of the Si substrate.
7. The method for producing an EUV transparent film according to claim 6, in, The cavity is formed by etching the Si substrate until the cavity reaches the SiO 2 After the SiO 2 The layer is removed from the cavity by etching. As a result, the self-supporting film portion of the EUV transparent film and the SiO 2 The layer is exposed on the same plane on the opposite side of the cavity.
8. A protective member, in, have: a substrate having a first surface and a second surface and having a cavity in the center; a mask layer, wherein the mask layer covers the second surface of the substrate; as well as An EUV transparent film continuously covers the surface of the mask layer and the inner surface of the cavity of the substrate and is exposed as a self-supporting film constituting a bottom surface of the cavity at the same height as the first surface.
9. A protective member, in, have: a substrate having a first surface and a second surface and having a cavity in the center; and An EUV transparent film continuously covers the second surface of the substrate and the inner surface of the cavity and is exposed as a self-supporting film constituting a bottom surface of the cavity at the same height as the first surface.
10. The protection member according to claim 8, which is manufactured by the method according to any one of claims 1 to 7.
11. The protection member according to claim 9, which is manufactured by the method according to any one of claims 2 to 7.