Aerogel and preparation method thereof

By using ultra-high temperature aging and supercritical drying technology in airgel materials, the efficiency and cost problems of high-temperature aging of airgel materials have been solved, performance improvement and production efficiency optimization have been achieved, and a material with excellent mechanics and insulation has been achieved. Aerogel products with thermal and hydrophobic properties.

CN118807627APending Publication Date: 2024-10-22IBIH ADVANCED MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411128895.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-10-22

Smart Images

  • Figure BDA0004997255660000071
    Figure BDA0004997255660000071
  • Figure BDA0004997255660000081
    Figure BDA0004997255660000081
  • Figure BDA0004997255660000091
    Figure BDA0004997255660000091
Patent Text Reader

Abstract

The invention relates to the technical field of aerogel, and discloses aerogel and a preparation method thereof. The method comprises the following steps: (1) aging wet gel in the presence of a solvent I to obtain aged wet gel; (2) carrying out supercritical drying on the aged wet gel to obtain aerogel; wherein the aging conditions are as follows: the temperature is 65-300 DEG C, and the pressure is 3-12 MPa; the supercritical drying conditions are as follows: the temperature is 32-300 DEG C, and the pressure is 4-12 MPa; the aging temperature is 5-10 DEG C lower than the temperature of the supercritical point of the solvent I, and the aging pressure is 1-7 MPa lower than the pressure of the supercritical point of the solvent I. According to the method provided by the invention, aging and drying are carried out in an ultra-high temperature form, heat in heating is fully utilized, the energy consumption is reduced, the process period is shortened, the production cost is reduced, and the performance of the aerogel material is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of aerogels, and in particular to an aerogel and a preparation method thereof. Background Art

[0002] Aerogel materials were invented in 1931, and have a history of nearly 100 years. Although researchers and companies have conducted a lot of research on their aging and have obtained many rules, they are mainly focused on the boiling point temperature that cannot exceed the aging temperature, and have not conducted in-depth exploration and research on high-temperature aging. In addition, during the preparation of aerogel materials, they need to go through the processes of sol-gel, aging, modification, and drying. The aging process is relatively long, which directly affects the production cycle of the entire material, reduces production efficiency, and increases production costs.

[0003] CN108046274A discloses a method for preparing SiO2 aerogel, wherein the SiO2 wet gel prepared by the sol-gel method is dried by a supercritical drying method to obtain SiO2 aerogel, characterized in that the supercritical drying comprises: gradually increasing the pressure in an inert atmosphere and within a pressure range of 2-7MPa for gradient segmented drying, and then increasing the pressure to 11-12MPa for constant pressure drying, and the drying temperature is 270-280°C. The use of this preparation method can alleviate the technical problems of the existing preparation method that easily lead to shrinkage cracking of the aerogel skeleton and pore collapse, thereby achieving the purpose of increasing the porosity and preventing the aerogel from cracking. However, the operation process of this preparation method is relatively complicated, and it is necessary to gradually increase the temperature by a gradient; and this method needs to be aged at a temperature of 40-60°C for 20-24h before drying, and the production cycle is long and the production cost is high.

[0004] Therefore, the present invention provides an ultra-high temperature aging method for aging aerogels to shorten the process cycle and reduce production costs. Summary of the invention

[0005] The purpose of the present invention is to overcome the problems of low aerogel production efficiency and high production cost in the prior art.

[0006] In order to achieve the above object, the first aspect of the present invention provides a method for preparing an aerogel, the method comprising:

[0007] (1) aging the wet gel in the presence of solvent I to obtain an aged wet gel;

[0008] (2) subjecting the aged wet gel to supercritical drying to obtain an aerogel;

[0009] Wherein, the aging conditions include: temperature of 65-300°C and pressure of 3-12MPa;

[0010] The supercritical drying conditions include: temperature of 32-300°C and pressure of 4-12MPa;

[0011] The aging temperature is 5-10° C. lower than the temperature of the supercritical point of solvent I, and the aging pressure is 1-7 MPa lower than the pressure of the supercritical point of solvent I.

[0012] The second aspect of the present invention provides an aerogel prepared by the method described in the first aspect.

[0013] The method provided by the present invention performs aging and drying in the form of ultra-high temperature, fully utilizes the heat during heating, reduces energy consumption, shortens the process cycle, reduces production costs, and improves the performance of aerogel materials. DETAILED DESCRIPTION

[0014] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0015] As mentioned above, the first aspect of the present invention provides a method for preparing an aerogel, the method comprising:

[0016] (1) aging the wet gel in the presence of solvent I to obtain an aged wet gel;

[0017] (2) subjecting the aged wet gel to supercritical drying to obtain an aerogel;

[0018] Wherein, the aging conditions include: temperature of 65-300°C and pressure of 3-12MPa;

[0019] The supercritical drying conditions include: temperature of 32-300°C and pressure of 4-12MPa;

[0020] The aging temperature is 5-10° C. lower than the temperature of the supercritical point of solvent I, and the aging pressure is 1-7 MPa lower than the pressure of the supercritical point of solvent I.

[0021] Preferably, the supercritical drying conditions include: a temperature of 230-300° C. and a pressure of 5-10 MPa. The inventors found that under the preferred conditions, the aerogel obtained has lower thermal conductivity, lower density and higher mechanical properties.

[0022] It should be noted that the present invention has no special requirements for the amount of the solvent I, as long as it can completely immerse the wet gel during the aging process. For example, the amount of the solvent I is 1-5 mL relative to 1 g of the wet gel.

[0023] Preferably, the aging conditions include: a temperature of 100-300° C. and a pressure of 2-5 MPa.

[0024] Preferably, the temperature of the supercritical drying is between the temperature of the supercritical point of solvent I and 300°C; the pressure of the supercritical drying is ≥ the pressure of the supercritical point of solvent I. The inventors found that in this preferred case, the aerogel obtained has better thermal insulation performance and low density performance.

[0025] Preferably, the supercritical drying step comprises: subjecting the aged wet gel to a first supercritical drying to obtain gel I; and then subjecting the gel I to a second supercritical drying to obtain aerogel.

[0026] Preferably, the temperature of the second supercritical drying is 5-10° C. higher than that of the first supercritical drying. The inventors found that in this preferred case, the aerogel can be made more transparent, less prone to yellowing, less organic matter, and lower thermal conductivity and density.

[0027] Preferably, the aging time is 10-300 min; and the first supercritical drying time is 1-3 h.

[0028] In the present invention, after the temperature is raised, the second supercritical drying is performed by reducing the pressure at a certain rate to first reduce the pressure to the supercritical point of the solvent and then reduce the pressure to 0 MPa. Preferably, the second supercritical drying is performed by reducing the pressure at a first pressure reduction rate to the supercritical point of the solvent and then reducing the pressure at a second pressure reduction rate until the pressure drops to 0 MPa; the first pressure reduction rate and the second pressure reduction rate are each independently 2-4 MPa / min.

[0029] Preferably, the method further comprises: reducing the temperature of the product after the second supercritical drying to below 80° C. to obtain an aerogel.

[0030] Preferably, the solvent I is selected from at least one of anhydrous methanol, anhydrous ethanol, n-hexane, isopropanol, acetone, cyclohexane, n-pentane, propane and ethane.

[0031] Preferably, the wet gel is prepared by a sol-gel method.

[0032] Preferably, the wet gel is selected from at least one of silicon-based wet gel, aluminum oxide wet gel, zirconium oxide wet gel, yttrium oxide wet gel, and polyimide wet gel.

[0033] Preferably, the wet gel is a silicon-based wet gel. The inventors found that in this preferred case, the aerogel obtained has better thermal insulation and low density performance.

[0034] According to a preferred embodiment, the steps of preparing the silicon-based wet gel by the solvent-gel method include:

[0035] A precursor solution containing a silicon source, a solvent II and water is reacted with a catalyst to obtain a silicon-based wet gel.

[0036] According to a preferred specific embodiment, the method further comprises: before carrying out the reaction, first mixing the silicon source, the solvent II and the water to obtain a precursor solution.

[0037] The present invention has no special requirements for the first mixing method, as long as the silicon source, solvent II and water can be mixed evenly. Exemplarily, the first mixing conditions include: temperature of 25-30°C, time of 10-60min, and rotation speed of 100-500rpm.

[0038] Preferably, the silicon source is selected from at least one of methyl orthosilicate, ethyl orthosilicate, methyltrimethoxysilane, methyltriethoxysilane, dimethyldimethoxysilane and dimethyldiethoxysilane.

[0039] Preferably, the solvent II is selected from at least one of methanol, ethanol, n-hexane, isopropanol and hexamethyldisiloxane.

[0040] Preferably, the catalyst is an acidic catalyst and / or a basic catalyst.

[0041] Preferably, the acidic catalyst is selected from at least one of hydrochloric acid, hydrofluoric acid and ammonium fluoride.

[0042] Preferably, the alkaline catalyst is selected from at least one of aqueous ammonia, sodium hydroxide and sodium bicarbonate.

[0043] Preferably, in the precursor solution, the molar ratio of the silicon source, the solvent II and the water is 1:25-70:2-6.

[0044] Preferably, the reaction operation comprises the following steps: using an acidic catalyst to adjust the pH value of the precursor solution to 2-3 and then reacting, and then adding an alkaline catalyst to adjust the pH value to 7-8 to obtain a silicon-based wet gel; or

[0045] The pH value of the precursor solution is adjusted to 7-8 by using an alkaline catalyst and then reacted to obtain a silicon-based wet gel.

[0046] Preferably, the reaction conditions include: temperature of 25-50°C and time of 20-180 min.

[0047] As mentioned above, the second aspect of the present invention provides an aerogel prepared by the method described in the first aspect.

[0048] Preferably, the thermal conductivity of the aerogel is 0.015-0.021w / (m·k) and the density is 0.05-0.20g / cm 3 , elastic modulus is 0.1-15MPa, and hydrophobic angle is 120-150°.

[0049] Compared with the prior art, the present invention has the following advantages:

[0050] 1. The present invention uses ultra-high temperature aging to age the wet gel, which can improve the mechanical properties (elastic modulus), thermal insulation properties, hydrophobic properties and low-density properties of the aerogel, and obtain an aerogel product with better performance.

[0051] 2. The present invention utilizes the heat and time in the supercritical drying heating process to age the wet gel, which not only saves the heat energy waste in the process, but also shortens the entire process cycle and further reduces the cost.

[0052] 3. In a high-temperature solvent environment, the wet gel skeleton structure itself can be dehydrated. At the same time, because it is in an alcohol pressure environment, the skeleton will not collapse, which effectively protects the integrity of its skeleton structure, thereby ensuring the excellent performance of the product.

[0053] 4. In a high-temperature solvent environment, the solvent used breaks the bonds and condenses the bonds with the hydroxyl groups on the surface of the wet gel, dehydrating to generate hydrophobic groups, thereby forming a self-hydrophobic product. No modification process is required, which not only saves material costs but also shortens the process cycle and improves production efficiency.

[0054] The present invention will be described in detail below through preparation examples and test examples. In the following preparation examples and test examples, unless otherwise specified, all raw materials used are commercially available.

[0055] Silicon source: Methyl orthosilicate, purchased from Zhangjiagang Xinya Chemical Co., Ltd.

[0056] Hydrochloric acid: hydrochloric acid with a concentration of 37 wt%.

[0057] Preparation Example 1

[0058] The method for preparing a silicon-based wet gel comprises the following steps:

[0059] S1: 1 mol of methyl orthosilicate, 4 mol of deionized water, and 25 mol of ethanol are first mixed to obtain a precursor solution;

[0060] The first mixing conditions were: temperature 30°C, time 30 min, and rotation speed 300 rpm;

[0061] S2: adding hydrochloric acid to the precursor solution to adjust the pH value to 2, reacting at 30° C. for 60 min, and then adding a 3 wt % sodium bicarbonate solution to adjust the pH value to 7 to obtain a silicon-based wet gel.

[0062] Preparation Example 2

[0063] The method for preparing alumina wet gel comprises the following steps:

[0064] S1: 1 mol of aluminum chloride hexahydrate, 6 mol of ethanol, and 38 mol of an aqueous solution are first mixed to obtain a precursor solution;

[0065] The first mixing condition: temperature is 30°C, time is 30 min, and speed is 300 rpm;

[0066] S2: 5.5 mol of propylene oxide was added dropwise to the precursor solution and reacted at 30° C. for 60 min to obtain wet alumina gel.

[0067] Example 1

[0068] This example is used to illustrate that the aerogel of the present invention is prepared according to the raw material formula and process parameters in Table 1 and the following method.

[0069] The method for preparing aerogel comprises the following steps:

[0070] (1) placing the wet gel in a supercritical drying device for aging in the presence of solvent I to obtain an aged wet gel;

[0071] (2) subjecting the aged wet gel to a first supercritical drying to obtain gel I;

[0072] (3) subjecting the gel I to a second supercritical drying (i.e., when the temperature reaches the second supercritical drying temperature, firstly reducing the pressure at a first pressure reduction rate to the supercritical point of the solvent, and then reducing the pressure at a second pressure reduction rate until the pressure drops to 0 MPa), cooling to room temperature, and obtaining an aerogel.

[0073] Unless otherwise specified, the remaining embodiments are carried out using the same process as that of Embodiment 1, except that the aerogel raw material formulas and process parameters used are different, see Table 1 for details.

[0074] Table 1

[0075]

[0076]

[0077] Comparative Example 1

[0078] This comparative example 1 is carried out in a similar manner to that of Example 1, except that in step (1) of this example, the aging temperature is 225° C. and the pressure is 7 MPa, and the other conditions are the same as those of Example 1; and aerogel DA1 is obtained.

[0079] Comparative Example 2

[0080] This comparative example 1 is carried out in a similar manner to that of Example 1, except that in step (1) of this example, the aging temperature is 245° C. and the pressure is 5 MPa, and the remaining conditions are the same as those of Example 1; and aerogel DA2 is obtained.

[0081] Test Case

[0082] The performance of the aerogel prepared in the above example was tested, and the specific test method is as follows:

[0083] Thermal conductivity is tested according to GB / T10294 standard;

[0084] Density test: Micromeritics Geopyc 1360 density analyzer was used to test the density. The average value of the three tests was the sample density.

[0085] The elastic modulus was tested as follows: a universal testing machine (model Zwick Z010) was used to perform a uniaxial compression test on the whole cylinder, the compression rate was set to 1 mm / min until the displacement remained unchanged, and then the pressure was released at a decompression rate of 0.2 mm / min to obtain the stress-strain curve of the sample, where the slope of the curve of the elastic deformation part was the elastic modulus of the sample, and the average value of the test was obtained three times as the elastic modulus of the sample;

[0086] Hydrophobic angle test: The test was carried out using a hydrophobic contact angle tester (Beijing Harke Testing Instrument Factory, model HARKE-SPCAX1), and the water contact angle was calculated by measuring the angle formed by a water drop on the surface of the material.

[0087] The specific test results are shown in Table 2.

[0088] Table 2

[0089]

[0090] It can be seen from the above results that the aerogel prepared by the method provided by the present invention has excellent heat insulation, low density and hydrophobic effects.

[0091] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A method for preparing aerogel, characterized in that: The method includes: (1) aging the wet gel in the presence of solvent I to obtain an aged wet gel; (2) subjecting the aged wet gel to supercritical drying to obtain an aerogel; Wherein, the aging conditions include: temperature of 65-300°C and pressure of 3-12MPa; The supercritical drying conditions include: temperature of 32-300°C and pressure of 4-12MPa; The aging temperature is 5-10° C. lower than the temperature of the supercritical point of solvent I, and the aging pressure is 1-7 MPa lower than the pressure of the supercritical point of solvent I.

2. The method according to claim 1, characterized in that The aging conditions include: a temperature of 100-300° C. and a pressure of 2-5 MPa; and / or The temperature of the supercritical drying is between the temperature of the supercritical point of the solvent I and 300° C.; the pressure of the supercritical drying is ≥ the pressure of the supercritical point of the solvent I.

3. The method according to claim 1 or 2, characterized in that: The supercritical drying step comprises: subjecting the aged wet gel to a first supercritical drying to obtain gel I; and subjecting the gel I to a second supercritical drying to obtain aerogel; The temperature of the second supercritical drying is 5-10° C. higher than the temperature of the first supercritical drying.

4. The method according to claim 3, characterized in that The aging time is 10-300 min; the first supercritical drying time is 1-3 h; and / or The second supercritical drying is performed by reducing the pressure at a first pressure reduction rate to the supercritical point of the solvent, and then reducing the pressure at a second pressure reduction rate until the pressure drops to 0 MPa; the first pressure reduction rate and the second pressure reduction rate are each independently 2-4 MPa / min; and / or The solvent I is selected from at least one of anhydrous methanol, anhydrous ethanol, n-hexane, isopropanol, acetone, cyclohexane, n-pentane, propane and ethane.

5. The method according to any one of claims 1 to 4, characterized in that: The wet gel is prepared by a sol-gel method; and / or The wet gel is selected from at least one of silicon-based wet gel, aluminum oxide wet gel, zirconium oxide wet gel, yttrium oxide wet gel, and polyimide wet gel.

6. The method according to any one of claims 1 to 4, characterized in that: The wet gel is a silicon-based wet gel, and the steps of preparing the silicon-based wet gel by a solvent-gel method include: A precursor solution containing a silicon source, a solvent II and water is reacted with a catalyst to obtain a silicon-based wet gel.

7. The method according to claim 6, characterized in that The catalyst is an acidic catalyst and / or a basic catalyst; Preferably, the acidic catalyst is selected from at least one of hydrochloric acid, hydrofluoric acid and ammonium fluoride; Preferably, the alkaline catalyst is selected from at least one of aqueous ammonia, sodium hydroxide and sodium bicarbonate.

8. The method according to claim 6 or 7, characterized in that: The silicon source is selected from at least one of methyl orthosilicate, ethyl orthosilicate, methyltrimethoxysilane, methyltriethoxysilane, dimethyldimethoxysilane and dimethyldiethoxysilane; and / or In the precursor solution, the molar ratio of the silicon source, the solvent II and the water is 1:25-70:2-6.

9. The method according to any one of claims 6 to 8, characterized in that: The reaction conditions include: temperature of 25-50° C. and time of 20-180 min.

10. Aerogel prepared by the method according to any one of claims 1 to 9.