Manganese-based thermocatalyst material, preparation method and application thereof, manganese-based thermocatalyst coating and cooking utensil

The manganese-based thermal catalyst material with a nano-polycrystalline structure effectively degrades oil fume grease under low temperature conditions, solving the problems of low thermal energy utilization and serious oil fume pollution in the existing technology, and achieving self-cleaning and environmental protection effects during the cooking process.

CN118807731APending Publication Date: 2024-10-22FOSHAN SHUNDE MIDEA ELECTRICAL HEATING APPLIANCES MFG CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202310404704.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-14
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

Existing thermocatalytic materials are difficult to effectively degrade oil fumes and grease in low-temperature cooking environments, resulting in additional heating time and energy consumption during the cooking process, reducing thermal energy utilization, and oil fume pollution seriously affects the environment and health.

Method used

It adopts manganese-based thermal catalyst materials with nano-polycrystalline structure, including tetravalent manganese and trivalent manganese. By adjusting the pH value and roasting temperature, a catalyst with a high specific surface area is formed. The coating covers the surface of the cooking utensils and utilizes the heat generated during the cooking process. Carry out catalytic oxidative degradation.

Benefits of technology

It can effectively degrade oil fume and grease under low temperature conditions of 100℃-300℃, reduce environmental pollution and health risks, improve the cleanliness of cooking utensils, reduce energy consumption, and avoid oil accumulation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118807731A_ABST
    Figure CN118807731A_ABST
Patent Text Reader

Abstract

The invention discloses a manganese-based thermocatalyst material, a preparation method and application thereof, a manganese-based thermocatalyst coating and a cooking utensil, and belongs to the field of metal catalysts. The manganese-based thermal catalyst material is of a nano polycrystalline structure and comprises a manganese element and an oxygen element, and the manganese element comprises tetravalent manganese and trivalent manganese. The manganese-based thermal catalyst material has thermal catalytic performance and large specific surface area, a large number of catalytic active sites can be exposed, in the cooking process, oil fume grease pollutants make contact with the catalytic active sites of the manganese-based thermal catalyst material, heat generated by cooking serves as a catalytic heat source, and the catalytic activity of the oil fume grease pollutants is improved. Oil fume grease pollutant molecules are subjected to catalytic oxidation reaction under the action of oxygen in air and finally degraded into carbon dioxide and water. According to the cooking utensil, the purpose of timely degrading oil fume grease in the cooking process at the low temperature of 100-300 DEG C is achieved, environmental pollution can be reduced, damage to health of people is reduced, accumulation of oil stains is reduced, and the cooking utensil becomes easy to clean.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of metal catalysts, and in particular to a manganese-based thermal catalyst material and a preparation method and application thereof, and a manganese-based thermal catalytic coating and a cooking utensil. Background Art

[0002] With the rapid growth of the national economy, the tertiary industry has also risen. While obtaining significant economic benefits, it has also brought severe environmental and social problems. The catering industry is one of the key components of my country's tertiary industry. The oil fume it produces has become one of the outstanding contributors to atmospheric VOCs pollutants. Studies have shown that the content of formaldehyde in motor vehicle exhaust is equivalent to that in catering oil fume, but the total content of carbonyl compounds in oil fume is about 5 times the total content in exhaust. If the oil fume is released into the atmosphere without purification, it will not only cause air pollution and lead to phenomena such as photochemical smog, but also seriously damage people's health. The strong irritating odor often causes symptoms such as coughing and tears. It enters the body's circulatory system through the respiratory system, which is very likely to cause nasal and laryngeal inflammation and respiratory diseases. Polycyclic aromatic hydrocarbons and heterocyclic amine compounds are cancer-inducing substances. In addition, oil fume condensate is a flammable oily mixture. After direct discharge, it will adhere to the outer wall of the building to form large oil stains, which not only hinders the appearance, but also buries fire hazards. As the management of cooking fume emission becomes more standardized and strict, the harm of restaurant cooking fume pollution has become the focus of people's attention. Therefore, choosing a low-cost, simple equipment, and efficient purification method is an important part of reducing cooking fume pollution.

[0003] At present, the use of thermal catalytic materials to degrade oil and grease has been applied, but the thermal catalytic temperature of thermal catalytic materials in the prior art is usually around 300°C. For some cooking utensils with a larger cooking temperature range, such as air fryers, the cooking temperature can be controlled within a range of below 200°C. At this time, it is necessary to add a self-cleaning function. After cooking is completed, the temperature must be further heated to above 200°C or even above 300°C to complete the cleaning. This relatively increases the heating time and heating energy consumption, and reduces the thermal energy utilization rate during the cooking process. Summary of the invention

[0004] The main purpose of the present invention is to provide a manganese-based thermal catalyst material and its preparation method, application and manganese-based thermal catalytic coating, cooking utensils, which can oxidatively degrade oil stains during the cooking process, thereby solving the technical problem that a large amount of volatile oil smoke is easily generated during the cooking process, which not only pollutes the environment but also affects people's health.

[0005] To achieve the above object, the present invention provides a manganese-based thermal catalyst material. The manganese-based thermal catalyst material is a nano-polycrystalline structure, including manganese elements and oxygen elements, and the manganese elements include tetravalent manganese and trivalent manganese.

[0006] In some embodiments of the present application, the catalytic temperature of the manganese-based thermal catalyst material is 100° C.-300° C. Specifically, the catalytic temperature is the temperature value at which the thermal catalytic functional coating material begins to undergo a catalytic oxidation reaction.

[0007] In some embodiments of the present application, the atomic percentage of tetravalent manganese and trivalent manganese is (1-2):1.

[0008] In some embodiments of the present application, the manganese-based thermal catalyst material contains 5%-70% of the manganese element calculated by mass percentage.

[0009] In some embodiments of the present application, the specific surface area of ​​the manganese-based thermal catalyst material is in the range of 30-250 m 2 / g; and / or, the pore volume range of the manganese-based thermal catalyst material is 0.5-1.0cm 3 / g; and / or, the average pore size range of the manganese-based thermal catalyst material is 10-20nm.

[0010] In some embodiments of the present application, the nano-polycrystalline structure is composed of a single crystal particle, and the average particle size of the single crystal particle is 1nm-500nm.

[0011] In some embodiments of the present application, the manganese-based thermal catalyst material is spherical with a diameter ranging from 10 nm to 10 μm;

[0012] and / or, the manganese-based thermal catalyst material is in the shape of a rod, with a length ranging from 10 nm to 10 μm and a diameter ranging from 10 nm to 1 μm;

[0013] And / or, the manganese-based thermal catalyst material is in the form of a sheet with a width ranging from 10 nm to 10 μm and a thickness ranging from 2 nm to 1 μm.

[0014] In addition, to achieve the above object, the present invention also provides a method for preparing the manganese-based thermal catalyst material as described above, comprising the following steps:

[0015] Mixing a reaction solution A containing manganese ions and a reaction solution B containing transition metal ions to form a mixed solution C;

[0016] The pH of the mixed solution C is adjusted to cause a coprecipitation reaction to obtain a precipitate D;

[0017] The precipitate D is calcined to obtain the manganese-based thermal catalyst material.

[0018] In some embodiments of the present application, the manganese ions include divalent manganese ions provided by a manganese salt; and / or, the transition metal ions are provided by a transition metal salt.

[0019] In some embodiments of the present application, the manganese salt includes at least one of manganese nitrate, manganese sulfate, manganese chloride, and potassium permanganate;

[0020] And / or, the transition metal salt includes at least one of nitrate, sulfate and chloride.

[0021] In some embodiments of the present application, the mass percentage of the manganese salt and the transition metal salt is 1:(1-1.5).

[0022] In some embodiments of the present application, in the step of forming the precipitate D, the precipitate D is formed by adjusting the pH value of the mixed solution C to between 8 and 10.

[0023] In some embodiments of the present application, the calcination temperature is 450° C.-750° C., and the calcination time is 3 h-8 h.

[0024] In some embodiments of the present application, the calcination temperature is 500° C.-650° C., and the calcination time is 5 h-6 h.

[0025] In addition, to achieve the above-mentioned purpose, the present invention also provides a manganese-based thermal catalytic coating, wherein the manganese-based thermal catalytic coating comprises the manganese-based thermal catalyst material of the present invention as described above.

[0026] In addition, to achieve the above-mentioned object, the present invention also provides a cooking utensil, wherein the cooking utensil comprises the manganese-based thermocatalytic coating of the present invention as described above.

[0027] In some embodiments of the present application, the cooking utensil is an electric pressure cooker, a frying machine, an automatic cooking machine, an air fryer or an electric baking pan, etc.

[0028] In some embodiments of the present application, the cooking utensil has a heating module, and the manganese-based thermal catalytic coating is coated on the surface of the heating module and any inner surface in the cooking cavity.

[0029] In some embodiments of the present application, the cooking utensil is an air fryer, and the manganese-based thermal catalytic coating is coated on the surface of the heating module and any inner surface in the cooking cavity.

[0030] In some embodiments of the present application, the heating module of the air fryer is a disc-shaped metal heating tube.

[0031] In addition, to achieve the above-mentioned purpose, the present invention also provides a use of the manganese-based thermal catalyst material as described above in the present invention in degrading cooking fume grease pollutants.

[0032] The beneficial effects that can be achieved by the present invention are:

[0033] The present invention provides a manganese-based thermal catalyst material, which includes manganese elements and oxygen elements. The manganese elements include tetravalent manganese and trivalent manganese, have strong activity, and have good thermal catalytic performance. In addition, the manganese-based thermal catalyst material is a nano-polycrystalline structure with a large specific surface area, can expose a large number of catalytic active sites, and has a good catalytic effect on the oxidative degradation of oil smoke and grease generated by cooking.

[0034] Based on the above advantages, the manganese-based thermal catalyst material of the present invention has good catalytic activity under relatively low temperature conditions of 100°C-300°C, and is applied to cooking utensils. During the cooking process, the oil fume and grease pollutants generated are in direct contact with the catalytic active sites of the manganese-based thermal catalyst material, and the heat generated by cooking is used as the catalytic heat source. The oil fume and grease pollutant molecules undergo catalytic oxidation reactions under the action of oxygen in the air, and are eventually degraded into carbon dioxide and water, thereby achieving the purpose of timely degradation of the oil fume and grease during the cooking process, ensuring that there is no grease deposition and residue in the cavity after cooking, avoiding the pain point of difficult cleaning inside the cavity, and no additional energy consumption is required. It can not only reduce environmental pollution and reduce damage to people's health, but also reduce the accumulation of oil stains, making cooking utensils easy to clean, especially electrical appliances such as air fryers with compact structural design, closed space, and easy cleaning dead corners inside the cooking cavity. It can solve many problems caused by the difficulty of daily hygiene cleaning and reduce the breeding of bacteria and carcinogenic risks on the surface of cooking utensils.

[0035] The raw materials used in the invention are cheap and safe, and the synthesis process is simple and efficient. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.

[0037] Figure 1 This is a diagram illustrating the preparation process of the manganese-based thermal catalyst material according to Example 1 of the present invention.

[0038] Figure 2 is the XRD spectrum of the manganese-based thermal catalyst material prepared in Example 1 of the present invention;

[0039] Figure 3 is a surface microscopic FESEM morphology image of the manganese-based thermal catalyst material prepared in Example 1 of the present invention;

[0040] Figure 4It is a curve diagram of the catalytic degradation conversion rate of toluene of the products prepared in Examples 1 and 2 of the present invention and Comparative Example 1. DETAILED DESCRIPTION

[0041] It should be understood that the specific embodiments described herein are only used to explain the present invention, and are not used to limit the present invention.

[0042] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0043] In the present invention, descriptions such as "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In addition, the technical solutions between the various embodiments can be combined with each other, but they must be based on the ability of ordinary technicians in the field to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such a combination of technical solutions does not exist and is not within the scope of protection required by the present invention.

[0044] The invention provides a manganese-based thermal catalyst material.

[0045] The manganese-based thermal catalyst material of the present invention includes manganese and oxygen, and the manganese includes tetravalent manganese and trivalent manganese. When the manganese-based catalyst material does not show catalytic activity, the manganese element has multiple valence states, among which tetravalent manganese and trivalent manganese are more active, which can give the catalyst better thermal catalytic performance, and can exert better catalytic activity under low temperature conditions of 100°C-300°C. In the daily cooking process, the generated oil smoke and grease can be oxidized and degraded, ensuring that there is no grease deposition and residue in the cavity after cooking, avoiding the user's pain point that the cavity is difficult to clean.

[0046] It can be understood that 100°C-300°C refers to the temperature at which the manganese-based thermal catalyst material of the present invention begins to undergo catalytic reaction, and under the above temperature conditions, the conversion rate of the catalytic oxidation reaction of the reactants can reach 50% or more.

[0047] The manganese-based thermal catalyst material of the present invention is a nano-polycrystalline structure, composed of multiple single crystal particles, has a large specific surface area, can expose more catalytic active sites, has low-temperature thermal catalytic performance, and has catalytic activity under temperature conditions of 100°C-300°C. It can play an excellent catalytic role in the oxidative degradation of oil smoke and grease generated during the daily cooking process, ensuring that there is no grease deposition and residue in the cavity after cooking, avoiding the pain point of cooking scenes where the cavity is difficult to clean.

[0048] The manganese-based thermal catalyst material of the present invention has catalytic activity under the temperature condition of 100°C-300°C. When applied to the field of cooking, the heat generated by the cooking utensils during the cooking process can be used as a catalytic heat source, so that the manganese-based thermal catalyst material shows catalytic activity during the cooking process and directly contacts with the oil fume and oil pollution molecules generated during the cooking process. The pollutant molecules undergo catalytic oxidation reaction under the action of oxygen in the air and are finally degraded into carbon dioxide and water, thereby achieving catalytic oxidation degradation of the oil fume and grease generated during the cooking process, preventing the volatilization of oil fume, pollution to the environment and damage to people's health, and reducing the accumulation of oil pollution. The cooking utensils become easier to clean, especially electrical appliances with compact structural design and closed space such as air fryers. The cooking cavity is very easy to form a cleaning dead corner. The air fryer sprayed with the manganese-based thermal catalyst material of the present invention can catalytically degrade the oil pollution sputtered onto the manganese-based thermal catalyst material during the cooking process, which can solve many problems caused by the difficulty of cleaning in daily hygiene and reduce the growth of bacteria and carcinogenic risks on the surface of cooking utensils.

[0049] The manganese element in the manganese-based thermal catalyst material of the present invention has multiple valence states such as tetravalent and trivalent. Among them, both trivalent manganese and tetravalent manganese have good thermal catalytic activity, and the thermal catalytic activity of tetravalent manganese is better than that of trivalent manganese. By controlling the atomic percentage of tetravalent manganese and trivalent manganese in the manganese-based thermal catalyst material to (1-2):1, better thermal catalytic activity can be obtained, which is beneficial to promoting the catalytic oxidation degradation of oil smoke and grease generated during the cooking process.

[0050] Specifically, the atomic percentage of tetravalent manganese and trivalent manganese in the manganese-based thermal catalyst material can be any ratio within the range of (1-2):1, such as 1:1.1, 1:1.2, 1:1.3, 1:1.4, 1:1.5, 1:1.6, 1:1.7, 1:1.8, 1:1.8, 1:1.9, 1:2.0, etc.

[0051] In some embodiments, the manganese-based thermal catalyst material contains 5%-70% manganese element calculated by mass percentage. Specifically, the manganese element content can be 5%, 10%, 15%, 20%, 25%, 30%, 40%, 50%, 60%, 70%, 35%, 45%, 55%, 65%, 70%, etc., any content value within the range of 5%-70%, which can maximize the thermal catalytic activity of the manganese-based thermal catalyst material and improve the oxidative degradation effect on cooking oil fume and oil stains.

[0052] In some embodiments, the specific surface area of ​​the manganese-based thermal catalyst material of the present invention is in the range of 30-250 m 2 / g; and / or, the pore volume range of the manganese-based thermal catalyst material is 0.5-1.0cm 3 / g; and / or, the average pore size range of the manganese-based thermal catalyst material is 10-20nm.

[0053] For example, the specific surface area of ​​a manganese-based thermal catalyst material can be 30 m 2 / g, 50m 2 / g, 80m 2 / g、100m 2 / g, 130m 2 / g, 150m 2 / g, 180m 2 / g, 200m 2 / g, 210m 2 / g, 220m 2 / g, 250m 2 / g etc. 30-250m 2 / g; the pore volume can be 0.5cm 3 / g, 0.6cm 3 / g, 0.7cm 3 / g, 0.8cm 3 / g, 0.9cm 3 / g, 1.0cm 3 / g etc. 0.5-1.0cm 3 / g range is any value; the average pore size range is any value in the range of 10-20nm such as 10nm, 11nm, 13nm, 15nm, 16nm, 18nm, 19nm, 20nm. The manganese-based thermal catalyst material with the above physical properties can show more catalytic active sites, which is conducive to its catalytic effect on the oxidation and degradation of cooking fume oil.

[0054] In some embodiments, the nano-polycrystalline structure of the manganese-based thermal catalyst material of the present invention is composed of single crystal particles, wherein the average particle size of the single crystal particles is 1nm-500nm, specifically, the average particle size of the single crystal particles can be any value within the range of 1nm-500nm, such as 1nm, 10nm, 50nm, 80nm, 100nm, 150nm, 200nm, 250nm, 300nm, 350nm, 400nm, 450nm, 460nm, 480nm, 500nm, etc. The nano-polycrystalline structure composed of single crystal particles in the above average particle size range can provide a larger specific surface area, and the manganese-based thermal catalyst material can expose more catalytic active sites, and play a better catalytic role in the oxidative degradation of oil smoke and grease generated during the cooking process.

[0055] It can be understood that the above restrictions on the specific surface area, pore volume, average pore size, and average particle size of single crystal particles of manganese-based thermal catalyst materials can meet only one of them or can meet them all at the same time. Meeting them all at the same time is more conducive to the catalytic effect of oxidative degradation of cooking fume and oil pollution under low temperature conditions of 100°C-300°C.

[0056] The present invention does not limit the appearance of the manganese-based thermal catalyst material, which may be in the form of a sphere, a rod, or a sheet.

[0057] Among them, the diameter range of the spherical manganese-based thermal catalyst material is 10nm-10μm, specifically, it can be any value within the range of 10nm-10μm, such as 10nm, 20nm, 30nm, 40nm, 50nm, 80nm, 100nm, 500nm, 700nm, 900nm, 1μm, 2μm, 3μm, 4μm, 5μm, 6μm, 7μm, 8μm, 9μm, 9.5μm, 10μm, etc.

[0058] The length of the rod-shaped manganese-based thermal catalyst material ranges from 10nm to 10μm, and the diameter ranges from 10nm to 1μm. Specifically, the length range can be any value within the range of 10nm to 10μm, such as 10nm, 20nm, 30nm, 40nm, 50nm, 80nm, 100nm, 500nm, 700nm, 900nm, 1μm, 2μm, 3μm, 4μm, 5μm, 6μm, 7μm, 8μm, 9μm, 9.5μm, 10μm, etc.; the diameter can be any value within the range of 10nm to 1μm, such as 10nm, 20nm, 30nm, 40nm, 50nm, 60nm, 70nm, 80nm, 90nm, 1μm, etc.

[0059] The width of the flake manganese-based thermal catalyst material ranges from 10nm to 10μm, and the thickness ranges from 2nm to 1μm. Specifically, the width range can be any value in the range of 10nm to 10μm, such as 10nm, 20nm, 30nm, 40nm, 50nm, 80nm, 100nm, 500nm, 700nm, 900nm, 1μm, 2μm, 3μm, 4μm, 5μm, 6μm, 7μm, 8μm, 9μm, 9.5μm, 10μm, etc.; the thickness range can be any value in the range of 2nm to 1μm, such as 2nm, 3nm, 4nm, 8nm, 10nm, 50nm, 100nm, 300nm, 500nm, 600nm, 800nm, 900nm, 950nm, 1μm, etc.

[0060] The manganese-based thermal catalyst material having the above spherical, and / or rod-shaped, and / or flaky appearance has more crystal faces, can expose more catalytic active sites, and play a better catalytic role in the oxidative degradation of oil smoke and grease generated during the cooking process.

[0061] In addition, the present invention also provides a method for preparing the manganese-based thermal catalyst material as described above, comprising the following steps:

[0062] Step S10, mixing a reaction solution A containing manganese ions and a reaction solution B containing transition metal ions to form a mixed solution C;

[0063] Step S20, adjusting the pH of solution C to cause a coprecipitation reaction to obtain a precipitate D;

[0064] Step S30, calcining the precipitate D to obtain the manganese-based thermal catalyst material.

[0065] In some embodiments of step S10, the manganese ions include divalent manganese ions, which is beneficial to increase the content of tetravalent manganese and trivalent manganese in the manganese-based thermal catalyst material.

[0066] In some embodiments of step S10, the manganese ions are provided by a manganese salt, and the manganese salt can be dissolved in water to obtain a reaction solution A containing manganese ions. Specifically, the manganese salt includes at least one of manganese nitrate, manganese sulfate, manganese chloride, and potassium permanganate, and the above types of manganese salts are conducive to preparing a manganese-based thermal catalyst material with a nano-polycrystalline structure.

[0067] In some embodiments of step S10, the transition metal ions are provided by transition metal salts, and the transition metal salts can be dissolved in water to obtain a reaction solution B containing transition metal ions. Specifically, the transition metal salts include at least one of nitrates, sulfates, and chlorides, and the above transition metal salts are beneficial for helping the reactants to form a nano-polycrystalline structure with better morphology during the calcination process, obtain a larger specific surface area, and expose more catalytic active sites.

[0068] In some embodiments of step S10, the mixing of reaction solution A and reaction solution B may be promoted under stirring conditions, with the stirring speed being 500-1500 rpm.

[0069] In some embodiments of step S20, the pH value of the mixed solution C can be adjusted under stirring conditions to quickly induce a coprecipitation reaction, and the stirring speed is 500-1500 rpm.

[0070] In some embodiments of step S20, after the co-precipitation occurs, the precipitate D can be obtained by suction filtration and washing, and the purity of the precipitate D can be improved.

[0071] In some embodiments of step S30, the calcination temperature of the precipitate D is 450°C-750°C, and the calcination time is 3h-8h. Specifically, the calcination temperature can be any value within the range of 450°C-750°C, such as 450°C, 500°C, 550°C, 600°C, 650°C, 700°C, 750°C, etc.; the calcination time can be any value within the range of 3h-8h, such as 3h, 3.5h, 4h, 4.5h, 5h, 5.5h, 6h, 6.5h, 7h, 7.5h, 8h, etc. Under the above calcination conditions, the reactants in the ionic state can be promoted to form manganese metal oxides, and the proportion of tetravalent manganese and trivalent manganese can be increased. In addition, it is also beneficial for the product to form a morphology with a nano-polycrystalline structure, expose more catalytic active sites, and exert a better catalytic oxidation effect.

[0072] The manganese-based thermal catalyst material obtained after calcination can be in powder form, or in block form or granular form, and then processed into powder form. The powdered manganese-based thermal catalyst material is more conducive to spraying into a uniform manganese-based thermal catalytic coating.

[0073] This step does not limit the roasting equipment. In some embodiments, the roasting equipment can be a furnace.

[0074] The present invention does not limit the relationship between the addition amounts of the above manganese salt and the transition metal salt. In some embodiments, calculated by mass percentage, the mass percentage of the manganese salt and the transition metal salt is 1:(1-1.5). For example, it can be any ratio in the range of 1:(1-1.5), such as 1:1, 1:1.2, 1:1.3, 1:1.4, 1:1.5, etc.

[0075] Under the above addition conditions, it is beneficial to obtain a manganese-based thermal catalyst material with a nano-polycrystalline structure, and the content of manganese element can reach 5%-70%, and the proportion of tetravalent manganese ions and trivalent manganese ions is relatively high, which is beneficial to improve the catalytic effect of the catalyst material in the oxidative degradation reaction of cooking fume and oil pollution, and promote the rapid degradation of fume and oil pollution into carbon dioxide and water.

[0076] In addition, the present invention also provides a manganese-based thermal catalytic coating, which includes the manganese-based thermal catalyst material of the present invention as described above.

[0077] This embodiment does not limit the method of coating the manganese-based thermal catalyst material on the surface of the cooking utensil to form a manganese-based thermal catalytic coating. In some embodiments, the above manganese-based thermal catalyst material is sprayed on the surface of the heating module of the cooking utensil and any inner surface in the cooking cavity to form a thermal catalytic functional coating. The heating module provides a catalytic temperature, so that the catalyst can oxidize and degrade oil smoke and oil during the cooking process and show good catalytic activity.

[0078] In addition, the present invention also provides a cooking utensil having a heating module, which only needs to provide a temperature of 100°C-300°C to enable the manganese-based thermal catalytic coating to exhibit good thermal catalytic activity during the oxidation and degradation of oil smoke and oil pollution.

[0079] The present invention does not limit the types of cooking utensils, including electric pressure cookers, frying machines, automatic cooking machines, air fryers or electric baking pans, etc. The heat generated by the heating module in the above cooking utensils can be used as a catalytic heat source to directly catalyze and oxidize the oil stains splashed onto the surface of the manganese-based thermal catalytic coating. The oil stains are degraded during the cooking process, which can reduce pollution to the environment and the impact on people's health. At the same time, the accumulation of oil stains is avoided, making the cooking utensils easier to clean.

[0080] In some embodiments of the present application, the manganese-based thermal catalyst material contains 10%-40% of the manganese element; and / or, the atomic percentage of tetravalent manganese and trivalent manganese in the manganese-based thermal catalyst material is (1.5-2):1; and / or, the specific surface area of ​​the manganese-based thermal catalyst material is in the range of 200-250m 2 / g; and / or, the pore volume range of the manganese-based thermal catalyst material is 0.5-1.0cm 3 / g; and / or, the average pore size range of the manganese-based thermal catalyst material is 10-20nm, which can meet the catalytic temperature in the range of 100°C-220°C, realize synchronous self-cleaning during the cooking process, and achieve the effect of low-temperature catalytic oil pollution.

[0081] In some embodiments, the cooking appliance is an air fryer, and the manganese-based thermal catalyst material is coated on the surface of the heating module of the air fryer and the inner cavity surface near the heating module to form a manganese-based thermal catalytic coating. Specifically, the heating module can be a disc-shaped metal heating tube, which can make the manganese-based thermal catalytic coating be heated more evenly. The cooking temperature of the disc-shaped metal heating tube is used as the catalytic temperature to directly catalytically oxidize and degrade the oil stains splashed onto the surface of the heating module and the inner cavity surface near the heating module.

[0082] Specifically, when the air fryer is working, it only needs to reach a lower cooking temperature of 100℃-220℃ to stimulate the catalytic activity of the manganese-based thermal catalytic coating. The exposed catalytic active sites in the manganese-based thermal catalytic coating are in direct contact with the oil stains. Under aerobic conditions, the hydrocarbons in the oil stains are promoted to undergo catalytic oxidation reactions with oxygen. During the cooking process, the oil stains formed by volatile oil smoke can be degraded into carbon dioxide and water, which can reduce pollution to the environment and the impact on people's health. At the same time, it avoids the accumulation of oil stains, truly realizing the long-term surface self-cleaning function of the air fryer.

[0083] The manganese-based thermal catalytic coating at least covers the top wall of the receiving chamber of the air fryer in this embodiment. In the air fryer, the food is generally arranged near the bottom of the receiving chamber. Based on the cooking structure of the air fryer, the cooking medium in the receiving chamber, that is, the hot air flow, is driven to circulate rapidly by the operation of the fan. In one embodiment, the fan is located close to the top wall of the receiving chamber, so the negative pressure area formed by the operation of the fan causes the cooking medium carrying oil fume / grease pollutants to contact the top wall position first, thereby causing the top wall to be most prone to accumulation of oil fume / grease pollutants. In this embodiment, a manganese-based thermal catalytic coating is arranged on the top wall of the receiving chamber to catalytically degrade the oil fume / grease pollutants passing near the top wall. The catalytic efficiency is high, which is conducive to keeping the inner wall of the receiving chamber clean.

[0084] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the following specific embodiments are only used to explain the present invention, and are not used to limit the present invention.

[0085] Example 1

[0086] Weigh the raw materials according to the formula in Table 1, Figure 1 The manganese-based thermal catalyst material was prepared according to the preparation process and the preparation conditions in Table 1:

[0087] Step S10: dissolving a manganese salt with deionized water to obtain a reaction solution A containing manganese ions; dissolving a transition metal salt with deionized water to obtain a reaction solution B containing transition metal ions, and adding the reaction solution B to the reaction solution A under stirring at 500-1500 rpm to form a mixed solution C;

[0088] Step S20: Under the stirring condition of 500-1500 rpm, the pH of the mixed solution C is adjusted to cause a coprecipitation reaction, and a precipitate D is obtained through suction filtration and washing.

[0089] Step S30: calcining the precipitate D in a muffle furnace to obtain a manganese-based thermal catalyst material.

[0090] Examples 2 to 7

[0091] According to Examples 2 to 7 in Table 1, refer to the preparation method of Example 1, and the specific preparation conditions are shown in Table 1.

[0092] Comparative Examples 1 to 4

[0093] Raw materials were weighed according to the formula in Table 1, and a manganese-based thermal catalyst material was prepared according to the preparation steps of Example 1 and the preparation conditions in Table 1.

[0094] Table 1 Formula and preparation conditions of manganese-based thermal catalyst materials in Examples and Comparative Examples

[0095]

[0096] Note: “ / ” in Table 1 means no addition.

[0097] Performance Test:

[0098] 1. The manganese-based thermal catalyst material obtained in Example 1 was characterized by XRD diffractometer. The results are shown in Figure 2 .

[0099] like Figure 2 As shown, the manganese-based thermal catalyst material has characteristic diffraction peaks at 37.2°, 43.3°, 56.5°, and 67.1°, and because the diffraction peaks are broadened due to the nano-polycrystalline structure, the half-peak width FWHM is between 0.6° and 3°, indicating that the manganese-based thermal catalyst material of the present invention has a nano-polycrystalline structure.

[0100] 2. The morphology of the manganese-based thermal catalyst material obtained in Example 1 was observed using an electron microscope at 2500 times magnification. Figure 3 .

[0101] like Figure 3 As shown, the manganese-based thermal catalyst has a uniform spherical granular morphology, and the average particle size is approximately below 500 nm.

[0102] 3. The catalytic performance of the products obtained in the examples and comparative examples was tested by toluene oxidation experiment. The results are shown in Table 2. The catalytic performance curves of the products obtained in Example 1, Example 2 and Comparative Example 1 are shown in Table 2. Figure 4 .

[0103] 4. The specific surface area, pore volume and average particle size of the products obtained in the examples and comparative examples were measured, and the results are shown in Table 2. The specific surface area, pore volume and average pore size were measured using the Brunauer-Emmett-Teller (BET) method.

[0104] 5. Determination of the mass percentage of manganese element and Mn in the products obtained in the examples and comparative examples 4+ and Mn 3+The manganese content is in mass percentage and is determined using an energy dispersive X-ray spectrometer (EDS) or inductively coupled plasma spectroscopy (ICP); Mn 4+ / Mn 3+ The ratios were determined using X-ray photoelectron spectroscopy (XPS).

[0105] Table 2 Performance comparison of the products obtained in the embodiments and comparative examples

[0106]

[0107]

[0108] Note: T10, T50 and T90 in the catalytic effect correspond to the temperatures required for the toluene conversion rate to reach 10%, 50% and 90% during the toluene oxidation test respectively;

[0109] Combining Table 2 and Figure 4 It can be seen that the product obtained in the embodiment has a larger specific surface area and has a surface area of ​​0.5-1.0cm 3 / g pore volume and 10-20nm nanometer average particle size, nano polycrystalline structure, high manganese content, Mn 4+ / Mn 3+ The ratio is relatively high, and a large number of catalytic active sites can be exposed. The catalytic reaction can begin at a temperature of 100-300°C. The higher the catalytic temperature, the better the catalytic effect, and T50<300°C. In the daily cooking process, the fumes and grease generated by cooking can be oxidized and degraded, and it has a good catalytic degradation effect. Compared with the thermal catalysts in the prior art whose catalytic temperatures are generally above 200°C, the temperature at which the thermal catalytic functional coating material prepared by the present invention begins to undergo a catalytic reaction can be reduced to below 200°C, and a catalytic reaction can occur under the conditions of 100°C-150°C, and T50<300°C. The catalytic degradation effect on oil pollution is good. In the daily cooking process, for example, in the cooking process of the air fryer, the generated oil pollution can be decomposed to complete self-cleaning, without further processing to increase additional consumption, achieving low-temperature catalysis, completing the purpose of self-cleaning while cooking, ensuring that there is no grease deposition and residue in the cavity after cooking, avoiding the pain point of cooking scenes where the cavity is difficult to clean, and truly realizing the long-term surface self-cleaning function of cooking utensils.

[0110] In Comparative Example 1, no transition metal salt is added, and the obtained product is not a nano-polycrystalline structure, and a good catalytic effect can only be achieved at 340°C.

[0111] In Comparative Example 2, no manganese salt is added, and the obtained product is difficult to achieve a better catalytic effect at 100-300°C.

[0112] The product obtained in Comparative Example 3 is not a nano-polycrystalline structure, has a small specific surface area, cannot expose sufficient catalytic active sites, and cannot achieve a good catalytic effect below 400°C.

[0113] In Comparative Example 4, manganese oxide was used as the manganese source. The product obtained had coarsened grains and could not obtain an ideal nano-microcrystalline catalyst, so the specific surface area was only 20 g / m 2 , it cannot expose enough catalytic active sites and cannot achieve good catalytic effect below 400°C.

[0114] The above are only preferred embodiments of the present invention, and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. A manganese-based thermal catalyst material, characterized in that: The manganese-based thermal catalyst material is a nano-polycrystalline structure, and includes manganese elements and oxygen elements, wherein the manganese elements include tetravalent manganese and trivalent manganese.

2. The manganese-based thermal catalyst material according to claim 1, characterized in that: The catalytic temperature of the manganese-based thermal catalyst material is between 100°C and 300°C.

3. The manganese-based thermal catalyst material according to claim 1, characterized in that: The atomic percentage of the tetravalent manganese and the trivalent manganese is (1-2):

1.

4. The manganese-based thermal catalyst material according to claim 1, characterized in that: Calculated by mass percentage, the manganese-based thermal catalyst material contains 5%-70% of the manganese element.

5. The manganese-based thermal catalyst material according to claim 1, characterized in that: The specific surface area of ​​the manganese-based thermal catalyst material ranges from 30 to 250 m 2 / g; and / or, the pore volume range of the manganese-based thermal catalyst material is 0.5-1.0cm 3 / g; and / or, the average pore size range of the manganese-based thermal catalyst material is 10-20nm.

6. The manganese-based thermal catalyst material according to claim 1, characterized in that: The nano-polycrystalline structure is composed of a single crystal particle, and the average particle size of the single crystal particle is 1nm-500nm.

7. The manganese-based thermal catalyst material according to claim 1, characterized in that: The manganese-based thermal catalyst material is spherical with a diameter ranging from 10nm to 10μm; and / or, the manganese-based thermal catalyst material is in the shape of a rod, with a length ranging from 10 nm to 10 μm and a diameter ranging from 10 nm to 1 μm; And / or, the manganese-based thermal catalyst material is in the form of a sheet with a width ranging from 10 nm to 10 μm and a thickness ranging from 2 nm to 1 μm.

8. A method for preparing a manganese-based thermal catalyst material according to any one of claims 1 to 7, characterized in that: The following steps are involved: Mixing a reaction solution A containing manganese ions and a reaction solution B containing transition metal ions to form a mixed solution C; The pH of the mixed solution C is adjusted to cause a coprecipitation reaction to obtain a precipitate D; The precipitate D is calcined to obtain the manganese-based thermal catalyst material.

9. The method for preparing a manganese-based thermal catalyst material according to claim 8, characterized in that: The manganese ions include divalent manganese ions provided by a manganese salt; and / or the transition metal ions are provided by a transition metal salt.

10. The method for preparing a manganese-based thermal catalyst material according to claim 9, characterized in that: The manganese salt includes at least one of manganese nitrate, manganese sulfate, manganese chloride and potassium permanganate; And / or, the transition metal salt includes at least one of nitrate, sulfate, and chloride; And / or, the mass percentage of the manganese salt and the transition metal salt is 1:(1-1.5).

11. The method for preparing a manganese-based thermal catalyst material according to claim 8, characterized in that: In the step of forming the precipitate D, the precipitate D is formed by adjusting the pH value of the mixed solution C to between 8 and 10.

12. The method for preparing a manganese-based thermal catalyst material according to claim 8, characterized in that: The calcination temperature is 450° C.-750° C., and the calcination time is 3 h-8 h.

13. The method for preparing a manganese-based thermal catalyst material according to claim 12, characterized in that: The calcination temperature is 500° C.-650° C., and the calcination time is 5 h-6 h.

14. A manganese-based thermal catalytic coating, characterized in that: The manganese-based thermal catalytic coating comprises the manganese-based thermal catalyst material according to any one of claims 1 to 7.

15. A cooking utensil, characterized in that: The cooking utensil comprises the manganese-based thermocatalytic coating of claim 14 .

16. The cooking appliance according to claim 15, characterized in that The cooking appliance is any one of an electric pressure cooker, a frying machine, an automatic cooking machine, an air fryer or an electric baking pan.

17. The cooking appliance according to claim 15, characterized in that The cooking utensil has a heating module, and the manganese-based thermal catalytic coating is coated on the surface of the heating module and / or coated on any inner surface in the cooking cavity.

18. The cooking appliance according to claim 17, characterized in that The cooking utensil is an air fryer, and the manganese-based thermal catalytic coating is coated on the surface of a heating module of the air fryer and / or coated on any inner surface in a cooking cavity.

19. The cooking appliance according to claim 18, characterized in that The heating module of the air fryer is a disc-shaped metal heating tube.

20. Use of the manganese-based thermal catalyst material according to any one of claims 1 to 7 in degrading cooking fume grease pollutants.

Citation Information

Patent Citations

  • Ni-Mn composite oxide catalyst for eliminating benzene-series volatile organic substances from air and preparation method thereof

    CN105126863A

  • Method used for treating VOCs exhaust gas at low cost

    CN107583453A

  • Non-noble metal catalyst for catalytic combustion of volatile organic compounds and preparation method

    CN111686754A

  • Manganese copper ore material and application thereof in removing carbon monoxide at room temperature

    CN114669191A

  • Manganese oxide superfine nano-powder containing high-index crystal face oxygen defects as well as preparation method and application of manganese oxide superfine nano-powder

    CN115028203A