Ruthenium-lanthanum-tantalum composite catalyst, preparation method thereof and application of ruthenium-lanthanum-tantalum composite catalyst in depolymerization of polyvinyl chloride
During the depolymerization process of polyvinyl chloride, the ruthenium-lanthanum-tantalum composite catalyst effectively utilizes the C and Cl resources in PVC to generate ethylene, benzene and Cl2, solving the problems of insufficient utilization of chlorine resources and HCl corrosion in the existing technology, and achieving high efficiency. , environmentally friendly PVC regeneration cycle.
Patent Information
- Application Number
- CN202410822487.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-24
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-06-24
AI Technical Summary
Existing methods for depolymerizing polyvinyl chloride cannot effectively utilize the high content of chlorine resources in PVC, and easily generate HCl gas that corrodes equipment and low value-added tar coke.
Using a ruthenium-lanthanum-tantalum composite catalyst, lanthanum salts and tantalum salts are mixed with alcohol and ammonia water, calcined to obtain a La2O3-Ta2O5 carrier, and immersed in a RuCl3 solution for heat treatment to prepare Ru O2/La2O3-Ta2O5 ruthenium lanthanum tantalum composite catalyst is used to catalyze the depolymerization of polyvinyl chloride to generate ethylene, benzene and Cl2, avoid the formation of tar coke, and use perfluorodecalin as a solvent.
Efficient utilization of C and Cl resources in PVC is achieved. The generated ethylene and Cl2 can be reused in the PVC synthesis process, avoiding the generation of HCl and tar coke, improving the stability and selectivity of the catalyst, and ensuring environmental protection and safe reaction conditions.
Smart Images

Figure CN118807740A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of high-value conversion and utilization of waste plastics, and in particular to a ruthenium lanthanum tantalum composite catalyst and a preparation method thereof and application thereof in depolymerization of polyvinyl chloride. Background Art
[0002] Polyvinyl chloride (PVC) is a polymer material made of vinyl chloride. Due to its good chemical resistance, durability and processability, it is used as a thermoplastic polymer in building materials, medical devices, daily necessities and the automotive industry. It has become an indispensable material in modern industry and daily life. At the same time, the amount of waste PVC generated each year is increasing day by day, which not only causes huge environmental pollution, but also leads to a waste of resources. Therefore, converting waste PVC into high-value products is one of the major challenges facing modern society.
[0003] Usually, PVC is made of ethylene and Cl2 as raw materials through addition reaction to generate 1,2-dichloroethane, then remove HCl to get 1-vinyl chloride monomer, and then polymerize. The Cl content in PVC molecules is 56.8wt%, so how to make good use of the Cl resources in the PVC molecular structure is a very important content in the recycling of PVC.
[0004] According to the degree of retention of the molecular structure of PVC, the current recycling process is mainly divided into two categories: mechanical recycling and chemical recycling. Mechanical recycling refers to the mechanical crushing, screening and grinding of waste PVC, and then reprocessing it into PVC products. However, the mechanical properties of this type of material will be significantly reduced, so the use scenarios are very limited. Chemical recycling mainly includes methods such as gasification, cracking and catalytic depolymerization, that is, breaking the chemical bonds in PVC at high temperature to obtain small molecular gas, liquid and solid products. For example, PVC will undergo dechlorination reaction at 200-300°C to obtain small molecular hydrocarbons, HCl and carbon solids, and CC bonds will further break between 350-500°C to generate aliphatic or aromatic hydrocarbons and coke. The catalytic depolymerization method currently developed is mainly to increase the yield of small carbon molecules in the product. For example, Ni / Al2O3 and Ru / Al2O3 catalysts can be used to hydrogenate PVC into methane, ethane and other products. However, these technologies still inevitably generate low value-added products such as tar coke, and pay little attention to the conversion of Cl resources, which account for 56.8wt% of PVC. Most of them only convert it into HCl gas or form metal chloride solids. HCl not only corrodes recycling equipment, but also may cause chemical burns to workers' skin and eyes. This makes it impossible to effectively utilize the Cl resources with the highest content in PVC, which has become one of the difficulties in PVC recycling and conversion.
[0005] Therefore, how to disclose a catalyst that can catalyze the depolymerization of polyvinyl chloride without producing low-value-added products such as tar coke and HCl gas that corrodes equipment during the depolymerization process is an urgent problem to be solved by those skilled in the art. Summary of the invention
[0006] The object of the present invention is to provide a ruthenium lanthanum tantalum composite catalyst and a preparation method thereof and application in depolymerization of polyvinyl chloride, so as to solve the problems that the existing methods for depolymerization of polyvinyl chloride cannot effectively utilize Cl resources, the product HCl is easy to corrode the recovery equipment, and the products such as tar coke with low added value are easy to be produced.
[0007] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0008] The present invention provides a method for preparing a ruthenium lanthanum tantalum composite catalyst, comprising the following steps:
[0009] 1) mixing lanthanum salt, tantalum salt, alcohol and ammonia water, reacting to obtain a precipitate, and calcining the precipitate to obtain a La2O3-Ta2O5 carrier;
[0010] 2) The La2O3-Ta2O5 carrier is impregnated in a RuCl3 solution, and after the impregnation is completed, a heat treatment is performed to obtain a RuO2 / La2O3-Ta2O5 ruthenium lanthanum tantalum composite catalyst.
[0011] Preferably, in step 1), the molar ratio of the total molar amount of lanthanum in the lanthanum salt and tantalum in the tantalum salt to the ammonia in the ammonia water is 1:1-2;
[0012] The molar ratio of lanthanum in the lanthanum salt to tantalum in the tantalum salt is 0.02-0.2:0.01-0.2.
[0013] Preferably, the concentration of the ammonia water in step 1) is 0.1 to 1.0 mol / L;
[0014] The molar volume ratio of the lanthanum salt to ethanol is 0.02-0.2 mol:1L;
[0015] The lanthanum salt includes one or more of lanthanum nitrate, lanthanum chloride, lanthanum sulfate and lanthanum acetate;
[0016] The tantalum salt includes one or more of tantalum ethoxide, tantalum chloride and tantalum fluoride;
[0017] The alcohol includes one or more of methanol, ethanol, propanol and isopropanol.
[0018] Preferably, the reaction temperature in step 1) is 30 to 90° C., and the reaction time is 2 to 12 hours;
[0019] The calcination temperature is 300-600° C., and the calcination time is 2-6 hours.
[0020] Preferably, the concentration of the RuCl3 solution in step 2) is 0.02-0.2 mol / L;
[0021] The immersion time is 2 to 12 hours.
[0022] Preferably, the heat treatment temperature in step 2) is 250-500° C., and the heat treatment time is 2-6 hours.
[0023] The present invention also provides a ruthenium lanthanum tantalum composite catalyst prepared by the above preparation method, wherein the mass fraction of ruthenium element in the ruthenium lanthanum tantalum composite catalyst is 0.5-5%.
[0024] The present invention also provides an application of the above-mentioned ruthenium lanthanum tantalum composite catalyst in catalytic depolymerization of polyvinyl chloride, and the application method is as follows:
[0025] Polyvinyl chloride, ruthenium lanthanum tantalum composite catalyst and organic solvent are mixed and reacted to obtain ethylene, benzene and chlorine;
[0026] The organic solvent is perfluorodecalin.
[0027] Preferably, the mass ratio of the polyvinyl chloride to the ruthenium lanthanum tantalum composite catalyst is 1:0.1-1;
[0028] The concentration of polyvinyl chloride in the mixed system of polyvinyl chloride, ruthenium lanthanum tantalum composite catalyst and organic solvent is 1-10 g / L.
[0029] Preferably, the reaction temperature is 250-350°C and the reaction time is 1-12h;
[0030] The initial gas pressure of the reaction is 0.5-2 MPa.
[0031] The present invention has at least the following beneficial effects:
[0032] 1. The ruthenium lanthanum tantalum composite catalyst provided by the present invention fully utilizes the two resources of C and Cl in PVC during the process of oxidative depolymerization of polyvinyl chloride, converts them into ethylene, benzene and Cl2 products, avoids the generation of low value-added tar coke, and the obtained ethylene and Cl2 products can be reused in the synthesis process of PVC, realizing the closed-loop cycle of PVC plastic synthesis-depolymerization-resynthesis; the present invention adopts perfluorodecalin as a solvent, which has excellent O2 solubility ability, is non-toxic and harmless, environmentally friendly, has good stability, and does not undergo structural changes under reaction conditions, which can not only realize the efficient breaking of CC and C-Cl bonds in PVC molecules, but also prevent small molecular carbon-containing compounds such as ethylene and benzene from being excessively oxidized into substances such as CO2.
[0033] 2. The La2O3-Ta2O5 carrier in the ruthenium lanthanum tantalum composite catalyst provided by the present invention has both suitable acid centers and O vacancies, and can provide suitable coordinated unsaturated Nb centers and oxygen vacancies, which is beneficial to the directional adsorption and activation of PVC functional groups in the depolymerization reaction of the plastic, thereby improving the selectivity of the target product. The RuO2 active center can cause Cl rearrangement to obtain Cl2 products with high selectivity. The catalyst has good structural stability and is resistant to Cl poisoning. The catalyst will not be over-chlorinated or deactivated by poisoning during the reaction. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 This is the XRD pattern of the ruthenium lanthanum tantalum composite catalyst prepared in Example 1. DETAILED DESCRIPTION
[0035] The present invention provides a method for preparing a ruthenium lanthanum tantalum composite catalyst, comprising the following steps:
[0036] 1) mixing lanthanum salt, tantalum salt, alcohol and ammonia water, reacting to obtain a precipitate, and calcining the precipitate to obtain a La2O3-Ta2O5 carrier;
[0037] 2) The La2O3-Ta2O5 carrier is impregnated in a RuCl3 solution, and after the impregnation is completed, a heat treatment is performed to obtain a RuO2 / La2O3-Ta2O5 ruthenium lanthanum tantalum composite catalyst.
[0038] In the present invention, the mixing method of step 1) is preferably to first mix the lanthanum salt, tantalum salt and ethanol evenly and then add ammonia water for precipitation.
[0039] In the present invention, the molar ratio of the total molar amount of lanthanum in the lanthanum salt and tantalum in the tantalum salt to the ammonia in the ammonia water in step 1) is 1:1-2, preferably 1:1.2-1.8, more preferably 1:1.4-1.6, and more preferably 1:1.5.
[0040] In the present invention, the molar ratio of lanthanum in the lanthanum salt to tantalum in the tantalum salt is 0.02-0.2:0.01-0.2, preferably 0.05-0.18:0.03-0.15, more preferably 0.07-0.15:0.05-0.12, and more preferably 0.10-0.12:0.07-0.10.
[0041] In the present invention, the concentration of the ammonia water in step 1) is 0.1 to 1.0 mol / L, preferably 0.2 to 0.8 mol / L, more preferably 0.4 to 0.6 mol / L, and more preferably 0.5 mol / L.
[0042] In the present invention, the molar volume ratio of the lanthanum salt to ethanol is 0.02-0.2 mol:1L, preferably 0.05-0.18 mol:1L, more preferably 0.07-0.15 mol:1L, and more preferably 0.10-0.12 mol:1L.
[0043] In the present invention, the lanthanum salt includes one or more of lanthanum nitrate, lanthanum chloride, lanthanum sulfate and lanthanum acetate.
[0044] In the present invention, the tantalum salt includes one or more of tantalum ethoxide, tantalum chloride and tantalum fluoride.
[0045] In the present invention, the alcohol includes one or more of methanol, ethanol, propanol and isopropanol.
[0046] In the present invention, the reaction temperature in step 1) is 30-90°C, preferably 40-80°C, more preferably 50-70°C, and more preferably 55-60°C; the reaction time is 2-12h, preferably 4-10h, and more preferably 6-8h.
[0047] In the present invention, the calcination temperature is 300-600°C, preferably 350-550°C, more preferably 400-500°C, and more preferably 450°C; the calcination time is 2-6h, preferably 2.5-5.5h, more preferably 3-5h, and more preferably 3.5-4.5h.
[0048] In the present invention, the concentration of the RuCl3 solution in step 2) is 0.02 to 0.2 mol / L, preferably 0.05 to 0.18 mol / L, more preferably 0.07 to 0.15 mol / L, and more preferably 0.10 to 0.12 mol / L.
[0049] In the present invention, the immersion time is 2 to 12 hours, preferably 4 to 10 hours, and more preferably 6 to 8 hours.
[0050] In the present invention, the temperature of the heat treatment in step 2) is 250-500°C, preferably 300-450°C, and more preferably 350-400°C; the time of the heat treatment is 2-6h, preferably 3-5h, more preferably 3.5-4.5h, and more preferably 4h.
[0051] The present invention also provides a ruthenium lanthanum tantalum composite catalyst prepared by the above preparation method, wherein the mass fraction of ruthenium element in the ruthenium lanthanum tantalum composite catalyst is 0.5-5%, preferably 1.0-4.5%, further preferably 1.5-4.0%, more preferably 2-3.5%, and even more preferably 2.5-3.0%.
[0052] The present invention also provides an application of the above-mentioned ruthenium lanthanum tantalum composite catalyst in catalytic depolymerization of polyvinyl chloride, and the application method is as follows:
[0053] Polyvinyl chloride, ruthenium lanthanum tantalum composite catalyst and organic solvent are mixed and reacted to obtain ethylene, benzene and chlorine;
[0054] The organic solvent is perfluorodecalin.
[0055] In the present invention, the mass ratio of the polyvinyl chloride to the ruthenium lanthanum tantalum composite catalyst is 1:0.1-1, preferably 1:0.2-0.8, more preferably 1:0.4-0.6, and more preferably 1:0.5.
[0056] In the present invention, the concentration of polyvinyl chloride in the mixed system of polyvinyl chloride, ruthenium lanthanum tantalum composite catalyst and organic solvent is 1-10 g / L, preferably 2-8 g / L, more preferably 4-6 g / L, and more preferably 5 g / L.
[0057] In the present invention, the reaction temperature is 250-350°C, preferably 270-330°C, more preferably 290-310°C, and more preferably 300°C; the reaction time is 1-12h, preferably 2-10h, more preferably 4-8h, and more preferably 5-6h.
[0058] In the present invention, the reaction atmosphere is preferably air atmosphere or a mixed atmosphere of oxygen and inert gas, and the volume fraction of oxygen is preferably 1 to 30%, more preferably 5 to 18%, and even more preferably 10 to 15%.
[0059] In the present invention, the inert gas includes one or more of helium, argon, neon and nitrogen.
[0060] In the present invention, the initial gas pressure of the reaction is 0.5-2 MPa.
[0061] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0062] Example 1
[0063] (1) Dissolve lanthanum nitrate and tantalum ethoxide in ethanol, add 14 mol / L ammonia water in a constant temperature water bath at 40°C for precipitation, and the concentration of lanthanum nitrate, tantalum ethoxide and NH3 in the mixed system is 0.03 mol / L, 0.3 mol / L and 0.4 mol / L. After precipitation for 4 hours, filter and separate the precipitate from the reaction system, wash the precipitate with distilled water for 3 times, dry the precipitate at 120°C for 6 hours, and then calcine at 400°C for 2 hours to obtain the La2O3-Ta2O5 carrier.
[0064] (2) The La2O3-Ta2O5 carrier prepared in step (1) was immersed in a RuCl3 solution with a concentration of 0.1 mol / L for 4 h, and the precipitate was separated by filtration. The precipitate was dried at 120°C for 6 h, and then calcined at 300°C for 3 h to obtain a ruthenium lanthanum tantalum composite catalyst with a Ru content of 1 wt%.
[0065] (3) 0.2 g of waste PVC plastic, 0.06 g of the ruthenium lanthanum tantalum composite catalyst prepared in step (2), and 100 mL of perfluorodecalin are placed in a 300 mL sealed high-pressure reactor; an O2 / N2 mixed gas (the volume fraction of O2 is 10%) with a pressure of 0.5 MPa is introduced into the reactor at room temperature, and the reaction is stirred at a temperature of 300°C and a rate of 500 r / min for 4 h, and the gaseous products collected are ethylene and Cl2, and the liquid products are filtered to obtain benzene.
[0066] The ruthenium-lanthanum-tantalum composite catalyst prepared in this example was subjected to an X-ray diffraction experiment. The XRD pattern is shown in FIG. Figure 1 As shown in the figure, it can be seen that the diffraction angles (2theta) of 23.0°, 28.5°, and 36.9° are the crystal plane diffraction peaks of hexagonal Ta2O5 (003), (200), and (203); the crystal plane diffraction peaks of triclinic Ta2O5 (011), (103), (105), (0012), and (0011) are at 23.5°, 24.5°, 26.6°, 30.0°, and 36.7°, and the crystal plane diffraction peaks of hexagonal La2O3 (101), (102), and (112) are at 30.0°, 46.1, and 55.4. This indicates that the Ta2O5-La2O3 provided by the present invention is a composite crystal structure, and the RuO2 content is low and is in a highly dispersed state in the catalyst, with only weak and broad diffraction peaks at 28.0° and 35.1°.
[0067] Example 2
[0068] (1) Dissolve lanthanum nitrate and tantalum ethoxide in ethanol, add 14 mol / L ammonia water in a constant temperature water bath at 60°C for precipitation, and the concentration of lanthanum nitrate, tantalum ethoxide and NH3 in the mixed system is 0.08 mol / L, 0.16 mol / L and 0.36 mol / L. After precipitation for 6 hours, filter the reaction system to separate the precipitate, wash the precipitate with distilled water for 3 times, dry the precipitate at 100°C for 5 hours, and then calcine at 500°C for 2.5 hours to obtain the La2O3-Ta2O5 carrier.
[0069] (2) The La2O3-Ta2O5 carrier prepared in step (1) was immersed in a RuCl3 solution with a concentration of 0.1 mol / L for 7 h, and the precipitate was separated by filtration. The precipitate was dried at 100°C for 5 h, and then calcined at 350°C for 4 h to obtain a ruthenium lanthanum tantalum composite catalyst with a Ru content of 2 wt%.
[0070] (3) 0.4 g of waste PVC plastic, 0.24 g of the ruthenium lanthanum tantalum composite catalyst prepared in step (2), and 100 mL of perfluorodecalin are placed in a 300 mL sealed high-pressure reactor; an O2 / N2 mixed gas (the volume fraction of O2 is 5%) with a pressure of 1 MPa is introduced into the reactor at room temperature, and the reaction is stirred at a temperature of 260°C and a rate of 500 r / min for 6 h, and the gaseous products collected are ethylene and Cl2, and the liquid products are filtered to obtain benzene.
[0071] Example 3
[0072] (1) Dissolve lanthanum nitrate and tantalum ethoxide in ethanol, add 14 mol / L ammonia water in a constant temperature water bath at 70°C for precipitation, and the concentration of lanthanum nitrate, tantalum ethoxide and NH3 in the mixed system is 0.12 mol / L, 0.06 mol / L and 0.32 mol / L. After precipitation for 8 hours, filter the reaction system to separate the precipitate, wash the precipitate with distilled water for 3 times, dry the precipitate at 110°C for 4 hours, and then calcine at 450°C for 3.5 hours to obtain the La2O3-Ta2O5 carrier.
[0073] (2) The La2O3-Ta2O5 carrier prepared in step (1) was immersed in a RuCl3 solution with a concentration of 0.1 mol / L for 3 h, and the precipitate was separated by filtration. The precipitate was dried at 110°C for 4 h, and then calcined at 250°C for 3.5 h to obtain a ruthenium lanthanum tantalum composite catalyst with a Ru content of 0.5 wt%.
[0074] (3) 0.6 g of waste PVC plastic, 0.12 g of the ruthenium lanthanum tantalum composite catalyst prepared in step (2), and 100 mL of perfluorodecalin are placed in a 300 mL sealed high-pressure reactor; an O2 / N2 mixed gas (the volume fraction of O2 is 15%) at a pressure of 1.5 MPa is introduced into the reactor at room temperature, and the reaction is stirred at a temperature of 280°C and a rate of 500 r / min for 8 h, and the gaseous products collected are ethylene and Cl2, and the liquid products are filtered to obtain benzene.
[0075] Example 4
[0076] (1) Dissolve lanthanum nitrate and tantalum ethoxide in ethanol, add 14 mol / L ammonia water in a constant temperature water bath at 50°C for precipitation, and the concentration of lanthanum nitrate, tantalum ethoxide and NH3 in the mixed system is 0.18 mol / L, 0.04 mol / L and 0.35 mol / L. After precipitation for 5 hours, filter and separate the precipitate from the reaction system, wash the precipitate with distilled water for 3 times, dry the precipitate at 120°C for 8 hours, and then calcine at 600°C for 4 hours to obtain the La2O3-Ta2O5 carrier.
[0077] (2) The La2O3-Ta2O5 carrier prepared in step (1) was immersed in a RuCl3 solution with a concentration of 0.1 mol / L for 6 h, and the precipitate was separated by filtration. The precipitate was dried at 120°C for 8 h, and then calcined at 400°C for 2.5 h to obtain a ruthenium lanthanum tantalum composite catalyst with a Ru content of 1.5 wt%.
[0078] (3) 0.1 g of waste PVC plastic, 0.04 g of the ruthenium lanthanum tantalum composite catalyst prepared in step (2), and 100 mL of perfluorodecalin are placed in a 300 mL sealed high-pressure reactor; an O2 / N2 mixed gas (the volume fraction of O2 is 8%) at a pressure of 2 MPa is introduced into the reactor at room temperature, and the reaction is stirred at a temperature of 320°C and a rate of 500 r / min for 5 h, and the gaseous products collected are ethylene and Cl2, and the liquid products are filtered to obtain benzene.
[0079] Example 5
[0080] (1) Dissolve lanthanum nitrate and tantalum ethoxide in ethanol, add 14 mol / L ammonia water in a constant temperature water bath at 80°C for precipitation, and the concentration of lanthanum nitrate, tantalum ethoxide and NH3 in the mixed system is 0.15 mol / L, 0.3 mol / L and 0.9 mol / L. After precipitation for 12 hours, filter the reaction system to separate the precipitate, wash the precipitate with distilled water for 3 times, dry the precipitate at 140°C for 10 hours, and then calcine at 550°C for 2 hours to obtain the La2O3-Ta2O5 carrier.
[0081] (2) The La2O3-Ta2O5 carrier prepared in step (1) was immersed in a RuCl3 solution with a concentration of 0.1 mol / L for 9 h, and the precipitate was separated by filtration. The precipitate was dried at 140°C for 10 h, and then calcined at 450°C for 2 h to obtain a ruthenium lanthanum tantalum composite catalyst with a Ru content of 2.5 wt%.
[0082] (3) 0.3 g of waste PVC plastic, 0.24 g of the ruthenium lanthanum tantalum composite catalyst prepared in step (2), and 100 mL of perfluorodecalin are placed in a 300 mL sealed high-pressure reactor; an O2 / N2 mixed gas (the volume fraction of O2 is 12%) with a pressure of 0.8 MPa is introduced into the reactor at room temperature, and the reaction is stirred at a temperature of 350°C and a rate of 500 r / min for 7 h, and the gaseous products collected are ethylene and Cl2, and the liquid products are filtered to obtain benzene.
[0083] Example 6
[0084] (1) Dissolve lanthanum nitrate and tantalum ethoxide in ethanol, add 14 mol / L ammonia water in a constant temperature water bath at 90°C for precipitation, and the concentration of lanthanum nitrate, tantalum ethoxide and NH3 in the mixed system is 0.02 mol / L, 0.02 mol / L and 0.05 mol / L. After precipitation for 10 hours, filter and separate the precipitate from the reaction system, wash the precipitate with distilled water for 3 times, dry the precipitate at 150°C for 12 hours, and then calcine at 350°C for 6 hours to obtain the La2O3-Ta2O5 carrier.
[0085] (2) The La2O3-Ta2O5 carrier prepared in step (1) was immersed in a RuCl3 solution with a concentration of 0.1 mol / L for 11 h, and the precipitate was separated by filtration. The precipitate was dried at 150°C for 12 h, and then calcined at 500°C for 5 h to obtain a ruthenium lanthanum tantalum composite catalyst with a Ru content of 4 wt%.
[0086] (3) 1 g of waste PVC plastic, 1 g of the ruthenium lanthanum tantalum composite catalyst prepared in step (2), and 100 mL of perfluorodecalin are placed in a 300 mL sealed high-pressure reactor; an O2 / N2 mixed gas (the volume fraction of O2 is 20%) at a pressure of 1.2 MPa is introduced into the reactor at room temperature, and the reaction is stirred at a temperature of 250°C and a rate of 500 r / min for 2 h, and the gaseous products collected are ethylene and Cl2, and the liquid products are filtered to obtain benzene.
[0087] Example 7
[0088] (1) Dissolve lanthanum nitrate and tantalum ethoxide in ethanol, add 14 mol / L ammonia water in a constant temperature water bath at 75°C for precipitation, and the concentration of lanthanum nitrate, tantalum ethoxide and NH3 in the mixed system is 0.16 mol / L, 0.18 mol / L and 0.5 mol / L. After precipitation for 9 hours, filter and separate the precipitate from the reaction system, wash the precipitate with distilled water for 3 times, dry the precipitate at 105°C for 2 hours, and then calcine at 300°C for 5.5 hours to obtain the La2O3-Ta2O5 carrier.
[0089] (2) The La2O3-Ta2O5 carrier prepared in step (1) was immersed in a RuCl3 solution with a concentration of 0.1 mol / L for 12 h, and the precipitate was separated by filtration. The precipitate was dried at 105°C for 2 h, and then calcined at 400°C for 5.5 h to obtain a ruthenium lanthanum tantalum composite catalyst with a Ru content of 5 wt%.
[0090] (3) 0.8 g of waste PVC plastic, 0.4 g of the ruthenium lanthanum tantalum composite catalyst prepared in step (2), and 100 mL of perfluorodecalin are placed in a 300 mL sealed high-pressure reactor; an O2 / N2 mixed gas (the volume fraction of O2 is 1%) at a pressure of 1.6 MPa is introduced into the reactor at room temperature, and the reaction is stirred at a temperature of 340°C and a rate of 500 r / min for 10 h, and the gaseous products collected are ethylene and Cl2, and the liquid products are filtered to obtain benzene.
[0091] Example 8
[0092] (1) Dissolve lanthanum nitrate and tantalum ethoxide in ethanol, add 14 mol / L ammonia water in a constant temperature water bath at 65°C for precipitation, and the concentration of lanthanum nitrate, tantalum ethoxide and NH3 in the mixed system is 0.2 mol / L, 0.02 mol / L and 0.3 mol / L. After precipitation for 7 hours, filter and separate the precipitate from the reaction system, wash the precipitate with distilled water for 3 times, dry the precipitate at 115°C for 7 hours, and then calcine at 400°C for 5 hours to obtain the La2O3-Ta2O5 carrier.
[0093] (2) The La2O3-Ta2O5 carrier prepared in step (1) was immersed in a RuCl3 solution with a concentration of 0.1 mol / L for 10 h, and the precipitate was separated by filtration. The precipitate was dried at 115°C for 7 h, and then calcined at 350°C for 6 h to obtain a ruthenium lanthanum tantalum composite catalyst with a Ru content of 4.5 wt%.
[0094] (3) 0.9 g of waste PVC plastic, 0.63 g of the ruthenium lanthanum tantalum composite catalyst prepared in step (2), and 100 mL of perfluorodecalin are placed in a 300 mL sealed high-pressure reactor; an O2 / N2 mixed gas (the volume fraction of O2 is 12%) with a pressure of 0.1 MPa is introduced into the reactor at room temperature, and the reaction is stirred at a temperature of 310°C and a rate of 500 r / min for 12 h, and the gaseous products collected are ethylene and Cl2, and the liquid products are filtered to obtain benzene.
[0095] Example 9
[0096] (1) Dissolve lanthanum nitrate and tantalum ethoxide in ethanol, add 14 mol / L ammonia water in a constant temperature water bath at 55°C for precipitation, and the concentration of lanthanum nitrate, tantalum ethoxide and NH3 in the mixed system is 0.06 mol / L, 0.01 mol / L and 0.12 mol / L. After precipitation for 2 hours, filter the reaction system to separate the precipitate, wash the precipitate with distilled water for 3 times, dry the precipitate at 135°C for 11 hours, and then calcine at 450°C for 2.5 hours to obtain the La2O3-Ta2O5 carrier.
[0097] (2) The La2O3-Ta2O5 carrier prepared in step (1) was immersed in a RuCl3 solution with a concentration of 0.1 mol / L for 11 h, and the precipitate was separated by filtration. The precipitate was dried at 135°C for 11 h, and then calcined at 300°C for 3.5 h to obtain a ruthenium lanthanum tantalum composite catalyst with a Ru content of 3.5 wt%.
[0098] (3) 0.4 g of waste PVC plastic, 0.4 g of the ruthenium lanthanum tantalum composite catalyst prepared in step (2), and 100 mL of perfluorodecalin are placed in a 300 mL sealed high-pressure reactor; an O2 / N2 mixed gas (the volume fraction of O2 is 6%) at a pressure of 1.7 MPa is introduced into the reactor at room temperature, and the reaction is stirred at a temperature of 330°C and a rate of 500 r / min for 3 h, and the gaseous products collected are ethylene and Cl2, and the liquid products are filtered to obtain benzene.
[0099] Example 10
[0100] (1) Dissolve lanthanum nitrate and tantalum ethoxide in ethanol, add 14 mol / L ammonia water in a constant temperature water bath at 50°C for precipitation, and the concentration of lanthanum nitrate, tantalum ethoxide and NH3 in the mixed system is 0.1 mol / L, 0.15 mol / L and 0.45 mol / L. After precipitation for 3 hours, filter the reaction system to separate the precipitate, wash the precipitate with distilled water for 3 times, dry the precipitate at 145°C for 9 hours, and then calcine at 500°C for 4 hours to obtain the La2O3-Ta2O5 carrier.
[0101] (2) The La2O3-Ta2O5 carrier prepared in step (1) was immersed in a RuCl3 solution with a concentration of 0.1 mol / L for 8 h, and the precipitate was separated by filtration. The precipitate was dried at 145°C for 9 h, and then calcined at 450°C for 4 h to obtain a ruthenium lanthanum tantalum composite catalyst with a Ru content of 3 wt%.
[0102] (3) 0.5 g of waste PVC plastic, 0.45 g of the ruthenium lanthanum tantalum composite catalyst prepared in step (2), and 100 mL of perfluorodecalin are placed in a 300 mL sealed high-pressure reactor; an O2 / N2 mixed gas (the volume fraction of O2 is 18%) with a pressure of 0.3 MPa is introduced into the reactor at room temperature, and the reaction is stirred at a temperature of 290°C and a rate of 500 r / min for 9 hours, and the gaseous products collected are ethylene and Cl2, and the liquid products are filtered to obtain benzene.
[0103] Comparative Example 1
[0104] (1) Dissolve lanthanum nitrate in ethanol, add 14 mol / L ammonia water in a constant temperature water bath at 40°C for precipitation, and the concentration of lanthanum nitrate in the mixed system is 0.03 mol / L and the concentration of NH3 is 0.4 mol / L. After reacting for 4 hours, filter the product with filter paper, wash it with distilled water three times, dry it at 120°C for 6 hours, and then calcine it at 400°C for 2 hours to obtain La2O3 carrier;
[0105] (2) The La2O3 carrier prepared in step (1) was impregnated in a RuCl3 solution with a concentration of 0.1 mol / L for 4 h. After the impregnation, the carrier was dried at 120°C for 6 h and calcined at 300°C for 3 h to obtain a RuO2 / La2O3 catalyst with a Ru content of 1 wt%.
[0106] (3) 0.2 g of PVC and 0.06 g of RuO2 / La2O3 catalyst were dispersed in 100 mL of perfluorodecalin, and then placed in a 300 mL autoclave, into which a 0.5 MPa O2 / N2 mixed gas (the volume fraction of O2 was 10%) was introduced, and the temperature was raised to 300° C. and reacted for 4 h. After the reaction was completed, the gas product was collected, and the liquid was filtered to obtain the liquid product.
[0107] Comparative Example 2
[0108] (1) Tantalum ethoxide was dissolved in ethanol, and 14 mol / L ammonia water was added to a constant temperature water bath at 40°C for precipitation. The concentration of tantalum ethoxide in the mixed system was 0.3 mol / L and the concentration of NH3 was 0.4 mol / L. After reacting for 4 hours, the product was filtered with filter paper, washed with distilled water for 3 times, dried at 120°C for 6 hours, and then calcined at 400°C for 2 hours to obtain a Ta2O5 carrier.
[0109] (2) The Ta2O5 carrier prepared in step (1) was impregnated in a RuCl3 solution with a concentration of 0.1 mol / L for 4 h. After the impregnation, it was dried at 120°C for 6 h and calcined at 300°C for 3 h to obtain a RuO2 / Ta2O5 catalyst with a Ru content of 1 wt%.
[0110] (3) 0.2 g of PVC and 0.06 g of RuO2 / Ta2O5 catalyst were dispersed in 100 mL of perfluorodecalin, and then placed in a 300 mL autoclave, into which a 0.5 MPa O2 / N2 mixed gas (the volume fraction of O2 was 10%) was injected, and the temperature was raised to 300° C. and reacted for 4 h. After the reaction was completed, the gas product was collected and the liquid was filtered to obtain the liquid product.
[0111] The gas and liquid products obtained by depolymerizing PVC in Examples 1 to 10 and Comparative Examples 1 to 2 were qualitatively and quantitatively analyzed, and the analysis method was as follows:
[0112] First, the obtained gas product is passed into 100 mL of KI solution with a concentration of 0.5 mol / L to absorb the Cl2 in the gas, and then the Cl2 and ethylene are quantitatively analyzed by potentiometric titration and gas chromatography respectively.
[0113] The potentiometric titration method (reference Maximilian Moser, Cecilia Mondelli, Amol P.Amrute, Atsushi Tazawa, Detre Teschner, Manfred E.Schuster, Achim Klein-Hoffman, Núria López, Timm Schmidt, Javier Pérez-Ramírez, HCl Oxidation on IrO2-Based Catalysts: From Fundamentals to Scale-Up, ACS Catalysis, 2013, 3, 2813-2822) was carried out on a Swiss Mettler Toledo G20s automatic titrator, using a 0.1 mol / L Na2S2O3 standard solution to titrate I2. The volume V (unit mL) of the Na2S2O3 standard solution used was recorded, and the amount of Cl2 generated (mmol / g) was analyzed. Where m(PVC) is the mass of PVC added to the reaction (in g).
[0114] The ethylene product was quantitatively analyzed by the external standard method on a gas chromatograph model 8890 from Agilent, USA. The injection port temperature was 200°C, the column oven was kept at 60°C for 5 min, then heated to 150°C at a rate of 10°C / min and kept for 5 min. The chromatographic column used was a Gas-CarbonPLOT capillary column (the column length was 60m, the diameter was 0.32mm, and the film thickness was 1.5μm). The chromatographic column carrier gas was He gas, the column flow rate was 0.5mL / min, the detector was a FID detector, and the detector temperature was 200°C. The amount of ethylene product generated (mmol / g) was Wherein n (ethylene) and m (PVC) are the amount of ethylene (mmol) analyzed by gas chromatography and the mass of PVC added to the reaction (g), respectively.
[0115] The liquid product after the reaction was filtered, and then the benzene content was quantitatively analyzed by external standard method on Agilent Model 8890 gas chromatograph. The injection port temperature was 250°C, the column oven was kept at 100°C for 5 minutes, and then heated to 220°C at a rate of 10°C / min and kept for 10 minutes. The chromatographic column used was HP-5 capillary column (chromatographic column length 60m, diameter 0.32mm, film thickness 0.25μm), the chromatographic column carrier gas was He gas, the column flow rate was 0.5mL / min, the detector was FID detector, and the detector temperature was 250°C. The amount of benzene product generated (mmol / g) is Wherein n (benzene) and m (PVC) are the amount of ethylene (mmol) analyzed by gas chromatography and the mass of PVC added to the reaction (g), respectively.
[0116] The results are shown in Table 1.
[0117] Table 1 Results of yields of products in Examples 1 to 10 and Comparative Examples 1 to 2
[0118]
[0119] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a ruthenium lanthanum tantalum composite catalyst, characterized in that: The following steps are involved: 1) mixing lanthanum salt, tantalum salt, alcohol and ammonia water, reacting to obtain a precipitate, and calcining the precipitate to obtain a La2O3-Ta2O5 carrier; 2) The La2O3-Ta2O5 carrier is impregnated in a RuCl3 solution, and after the impregnation is completed, a heat treatment is performed to obtain a RuO2 / La2O3-Ta2O5 ruthenium lanthanum tantalum composite catalyst.
2. The method for preparing a ruthenium lanthanum tantalum composite catalyst according to claim 1, characterized in that: In the step 1), the molar ratio of the total molar amount of lanthanum in the lanthanum salt and tantalum in the tantalum salt to the ammonia in the ammonia water is 1:1-2; The molar ratio of lanthanum in the lanthanum salt to tantalum in the tantalum salt is 0.02-0.2:0.01-0.
2.
3. The method for preparing a ruthenium lanthanum tantalum composite catalyst according to claim 2, characterized in that: The concentration of ammonia water in step 1) is 0.1-1.0 mol / L; The molar volume ratio of the lanthanum salt to ethanol is 0.02-0.2 mol:1L; The lanthanum salt includes one or more of lanthanum nitrate, lanthanum chloride, lanthanum sulfate and lanthanum acetate; The tantalum salt includes one or more of tantalum ethoxide, tantalum chloride and tantalum fluoride. The alcohol includes one or more of methanol, ethanol, propanol and isopropanol.
4. The method for preparing a ruthenium lanthanum tantalum composite catalyst according to claim 3, characterized in that: The reaction temperature in step 1) is 30-90°C and the reaction time is 2-12h; The calcination temperature is 300-600° C., and the calcination time is 2-6 hours.
5. The method for preparing a ruthenium-lanthanum-tantalum composite catalyst according to any one of claims 1 to 4, characterized in that: The concentration of the RuCl3 solution in step 2) is 0.02-0.2 mol / L; The immersion time is 2 to 12 hours.
6. The method for preparing a ruthenium-lanthanum-tantalum composite catalyst according to claim 5, characterized in that: The heat treatment temperature in step 2) is 250-500° C., and the heat treatment time is 2-6 hours.
7. The ruthenium lanthanum tantalum composite catalyst prepared by the preparation method of a ruthenium lanthanum tantalum composite catalyst according to any one of claims 1 to 6, characterized in that: The mass fraction of ruthenium element in the ruthenium-lanthanum-tantalum composite catalyst is 0.5-5%.
8. Use of the ruthenium lanthanum tantalum composite catalyst according to claim 7 in catalytic depolymerization of polyvinyl chloride, characterized in that: The application method is as follows: Polyvinyl chloride, ruthenium lanthanum tantalum composite catalyst and organic solvent are mixed and reacted to obtain ethylene, benzene and chlorine; The organic solvent is perfluorodecalin.
9. Use of the ruthenium lanthanum tantalum composite catalyst in catalytic depolymerization of polyvinyl chloride according to claim 8, characterized in that: The mass ratio of the polyvinyl chloride to the ruthenium lanthanum tantalum composite catalyst is 1:0.1-1; The concentration of polyvinyl chloride in the mixed system of polyvinyl chloride, ruthenium lanthanum tantalum composite catalyst and organic solvent is 1-10 g / L.
10. Use of the ruthenium lanthanum tantalum composite catalyst according to claim 8 or 9 in catalytic depolymerization of polyvinyl chloride, characterized in that: The reaction temperature is 250-350°C and the reaction time is 1-12h; The initial gas pressure of the reaction is 0.5-2 MPa.
Citation Information
Patent Citations
Preparation method of SLATON catalyst for catalyzing visual light to decompose water to prepare oxygen
CN104190463A
Ru / SnO2 catalyst for catalytic combustion of vinyl chloride and preparation method and application of Ru / SnO2 catalyst
CN107233882A
Ruthenium catalyst for synthesis ammonia and preparation method thereof
CN110102295A
Method for catalytically converting oxygen-containing waste plastic into benzoic acid monomer
CN117402054A
Cited By
Modified catalyst for resisting chloride ion poisoning and preparation method thereof
CN120827865A