Nitrogen and sulfur doped activated aluminum oxide and preparation method thereof

By introducing nitrogen and sulfur heteroatoms into alumina to change its pore structure and surface pH, it solves the limitations of the existing alumina catalyst's pore structure and surface pH, significantly improves the adsorption performance, and is suitable for ethylene oxychlorination reactions.

CN118807802AActive Publication Date: 2024-10-22CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202310402620.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-14
Publication Date
2024-10-22
Estimated Expiration
2043-04-14

AI Technical Summary

Technical Problem

Existing alumina catalysts have limitations in pore structure and surface pH, and methods for introducing various heteroatoms have not been reported, limiting their application prospects.

Method used

By introducing nitrogen and sulfur heteroatoms into alumina at the same time, using the reaction of amide sulfonic acid polymers and sodium metaaluminate, nitrogen and sulfur doped activated alumina is prepared, changing its pore structure and surface pH, and using in-situ polymerization -The decomposition method uniformly introduces heteroatoms and increases the mesopore volume.

Benefits of technology

It significantly increases the specific surface area and mesopore volume of alumina, enhances its adsorption performance, and is suitable for the preparation of catalysts for ethylene oxychlorination reactions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004182641780000121
    Figure BDA0004182641780000121
Patent Text Reader

Abstract

The invention provides nitrogen and sulfur doped aluminum oxide and a preparation method thereof. By introducing an in-situ polymerization decomposition method, nitrogen and sulfur heteroatoms are introduced into the aluminum oxide, so that the pore structure and the adsorption characteristic of the aluminum oxide are improved, and the activated aluminum oxide with more excellent performance is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of catalysts, and in particular relates to nitrogen-sulfur doped activated alumina and a preparation method thereof. Background Art

[0002] Activated alumina is a porous, highly dispersed inorganic material with a high specific surface area pore structure composed of micropores, mesopores or macropores. It has the adsorption properties, surface activity, thermal stability and other characteristics required for catalysis, and can be processed into different shapes as needed. It is suitable as a catalyst carrier to produce various catalysts.

[0003] The introduction of heteroatoms into alumina will bring new properties to alumina, such as changes in pore structure, changes in the number and strength of acidic sites, and changes in the influence of loaded metals on the electronic state of metals. Therefore, alumina with the introduction of heteroatoms exhibits special properties. For example, J Energ Chem, 2022 (70) 332-339 reported that the catalytic activity of sulfur-doped alumina was significantly improved. At present, there are relatively few studies on the introduction of heteroatoms into alumina, and there are no reports on the method of introducing multiple heteroatoms at one time. The introduction of multiple heteroatoms can change the pore structure and surface pH of alumina, and has good application prospects. Summary of the invention

[0004] The present invention provides a nitrogen-sulfur doped activated alumina, which simultaneously introduces multiple heteroatoms during the reaction process. The introduction of multiple heteroatoms can change the pore structure and surface pH of the alumina, and has good application prospects.

[0005] One of the purposes of the present invention is to provide a nitrogen-sulfur doped activated alumina, comprising: an alumina carrier and a nitrogen-sulfur component. The nitrogen-sulfur component may exist in the form of aluminum nitrate or aluminum nitrite, aluminum sulfate or aluminum sulfite, a small amount of organic components containing nitrogen, sulfur and carbon, or may be nitrogen oxides or sulfur oxides gradually oxidized at high temperatures (e.g., above 450°C).

[0006] According to the present invention, in the nitrogen-sulfur doped activated alumina, the nitrogen content is 0.08-0.90wt%, and the sulfur content is 0.2-2wt%; for example, the nitrogen content can be any value among 0.08, 0.09, 0.10, 0.20, 0.30, 0.40, 0.50, 0.60, 0.70, 0.80, 0.90wt% or any range between two values, and the sulfur content can be any value among 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0wt% or any range between two values;

[0007] The specific surface area of ​​the nitrogen-sulfur doped activated alumina is 100 to 600 m 2 / g, for example, 100, 150, 200, 250, 300, 350, 400, 450, 500, 550, 600 m 2 / g or any value or range between any two values; preferably, the specific surface area of ​​the nitrogen-sulfur doped activated alumina is 150-500m 2 / g;

[0008] The pore volume of the nitrogen-sulfur doped activated alumina is 0.2-1.2 ml / g, for example, it can be any value among 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2 ml / g or a range between any two values; preferably, the pore volume of the nitrogen-sulfur doped activated alumina is 0.3-1.0 ml / g.

[0009] According to the present invention, nitrogen and sulfur are introduced into the nitrogen-sulfur doped activated alumina at one time, which can change the pore structure and surface pH of the alumina. The nitrogen-sulfur doped activated alumina is prepared from an aluminum source and an amide sulfonic acid polymer.

[0010] The second object of the present invention is to provide a method for preparing the nitrogen-sulfur doped activated alumina, comprising: calcining the alumina-loaded amide sulfonic acid polymer to obtain the nitrogen-sulfur doped activated alumina. Preferably, the preparation method comprises the following steps:

[0011] (1) adding a basic compound to a solution of an amide sulfonic acid monomer compound to neutralize the solution, and then introducing a protective gas to remove oxygen;

[0012] (2) adding an acidic compound to a sodium aluminate solution for neutralization reaction, aging, and filtering;

[0013] (3) adding the solid obtained by filtration in step (2) to the deoxygenated amide sulfonic acid monomer compound solution in step (1), then adding an auxiliary agent and an initiator, and heating for polymerization reaction;

[0014] (4) kneading, drying and calcining the product obtained after the polymerization reaction in step (3) to obtain the nitrogen-sulfur doped activated alumina.

[0015] According to an embodiment of the present invention, in the method for preparing nitrogen-sulfur doped activated alumina, in step (1):

[0016] The amide sulfonic acid monomer compound is 2-acrylamide-2-methylpropane sulfonic acid (AMPS);

[0017] The concentration of the amide sulfonic acid monomer compound solution is 3 to 15 wt %, for example, it can be any value of 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15 wt % or a range between any two values; preferably, the concentration of the amide sulfonic acid monomer compound solution is 5 to 12 wt %;

[0018] The alkaline compound is selected from inorganic alkaline compounds, and inorganic alkaline compounds commonly used in the art can be selected. For example, the alkaline compound is preferably at least one selected from sodium hydroxide, sodium carbonate, potassium hydroxide, and ammonia water; the alkaline compound can be added in the form of a commonly used solution, and the concentration of the solution can be prepared according to actual operation, as long as the neutralization of the amide sulfonic acid monomer compound solution can be achieved;

[0019] The pH of the neutralized solution is 6 to 10, for example, it can be any value among 6, 6.5, 7, 7.5, 8, 8.5, 9, 9.5, 10 or a range between any two values.

[0020] According to an embodiment of the present invention, in the method for preparing nitrogen-sulfur doped activated alumina, in step (2):

[0021] The concentration of the sodium aluminate solution is 3 to 35 wt%, for example, any value among 3, 5, 10, 15, 20, 25, 30, 35 wt% or a range between any two values; preferably, the concentration of the sodium aluminate solution is 5 to 30 wt%;

[0022] The acidic compound is selected from at least one of an inorganic acid and CO2, wherein the inorganic acid can be an inorganic acid commonly used in the art, for example, the inorganic acid is selected from at least one of hydrochloric acid, sulfuric acid, and nitric acid; the inorganic acid can be added in the form of a commonly used solution, and the concentration of the solution can be prepared according to actual operation, as long as the neutralization reaction of sodium aluminate can be achieved, the CO2 can be directly introduced into the solution, and a mixture of CO2 and nitrogen can also be introduced into the solution;

[0023] The mass ratio of the sodium aluminate to the amide sulfonic acid monomer compound is (13-130):1, which can be any value among 13:1, 15:1, 20:1, 25:1, 30:1, 40:1, 50:1, 60:1, 70:1, 80:1, 90:1, 100:1, 110:1, 120:1, 130:1, or a range between any two values;

[0024] The conditions of the neutralization reaction are: reacting under a protective gas atmosphere, and the reaction end point pH is 7 to 9, for example, it can be any value among 7, 7.5, 8, 8.5, 9 or a range between any two values;

[0025] The aging condition is aging at 20-50°C for 2-24h. For example, it can be aging at 20°C, 25°C, 30°C, 35°C, 40°C, 45°C or 50°C for 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h, 10h, 11h, 12h, 13h, 14h, 15h, 16h, 17h, 18h, 19h, 20h, 21h, 22h, 23h or 24h.

[0026] According to an embodiment of the present invention, in the method for preparing nitrogen-sulfur doped activated alumina, in step (3):

[0027] The auxiliary agent is selected from at least one of disodium ethylenediaminetetraacetate and citric acid;

[0028] Based on the mass of the amide sulfonic acid monomer compound being 100wt%, the amount of the auxiliary agent used is no more than 0.25wt%;

[0029] The initiator is selected from an oxidation-reduction initiation system, preferably a persulfate-sulfite oxidation-reduction initiation system; in the initiator, the oxidant is selected from persulfate, preferably at least one of potassium persulfate and sodium persulfate; the reducing agent is selected from sulfite, preferably at least one of sodium bisulfite and potassium sulfite; based on the mass of the amide sulfonic acid monomer compound as 100wt%, the amount of the oxidant is 0.01-0.1wt%, and the amount of the reducing agent is 0.005-0.05wt%. t%, for example, the amount of the oxidant can be any value in 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.1wt% or any range between two values, and the amount of the reducing agent can be any value in 0.005, 0.006, 0.007, 0.008, 0.009, 0.01, 0.02, 0.03, 0.04, 0.05wt% or any range between two values;

[0030] The polymerization reaction conditions are: polymerization temperature of 30-60°C, polymerization time of 2-10h, for example, aging at 30°C, 35°C, 40°C, 45°C, 50°C, 55°C or 60°C for 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h or 10h.

[0031] According to an embodiment of the present invention, in the method for preparing nitrogen-sulfur doped activated alumina, in step (4):

[0032] The kneading can be carried out in a kneading manner commonly used in the art. Preferably, the kneading time is 10 to 60 minutes, for example, any value among 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60 minutes or a range between any two values;

[0033] The drying may be carried out using commonly used drying equipment and drying conditions in the art. Preferably, the drying temperature is 120-200° C., for example, any value among 120, 130, 140, 150, 160, 170, 180, 190, 200° C. or a range between any two values.

[0034] The calcination can be carried out using calcination equipment and calcination conditions commonly used in the art. Preferably, the calcination conditions are: carried out in a protective gas atmosphere, the calcination temperature is 350-550° C., and the calcination time is 2-10 hours; the protective gas can be nitrogen or other inert gases, the calcination temperature can be any value among 350, 375, 400, 425, 450, 475, 500, 525, 550° C. or a range between any two values, and the calcination time can be any value among 2, 3, 4, 5, 6, 7, 8, 9, 10 hours or a range between any two values.

[0035] According to a specific embodiment of the present invention, the nitrogen-sulfur doped activated alumina can be prepared according to the following steps:

[0036] Step 1, using an amide sulfonic acid monomer compound as a raw material, preparing an aqueous solution, adding an alkaline compound to neutralize it, and passing an inert gas to deoxygenate for 20-60 minutes;

[0037] Step 2: prepare a sodium aluminate solution, which can be prepared directly using commercial sodium aluminate or by reacting sodium hydroxide and aluminum oxide;

[0038] Step 3, adding an acidic compound, such as CO2 or various inorganic acids, to the sodium aluminate solution to carry out a neutralization reaction, and aging for a period of time;

[0039] Step 4, filtering and washing the aged solid-liquid mixture, adding the solution in step 1 to the filter cake, stirring, adding an auxiliary agent and an initiator, and allowing the amide sulfonic acid monomer compound to undergo polymerization reaction at a certain temperature for a period of time;

[0040] Step 5: knead the mixture in step 4, dry and calcine to obtain nitrogen-sulfur doped activated alumina.

[0041] The nitrogen-sulfur doped activated alumina provided by the present invention can be used to prepare an ethylene oxychlorination reaction catalyst and is applied in an ethylene oxychlorination reaction.

[0042] The present invention disperses an alumina carrier in a solution of an amide sulfonic acid monomer compound, and after adding an initiator, the amide sulfonic acid monomer compound undergoes an in-situ polymerization reaction on the carrier surface to form a high molecular compound, which can improve the mesoporous structure of the alumina, increase the mesopore volume, and increase the binding force between the nitrogen and sulfur components and the carrier; at the same time, the auxiliary agent component added during the reaction can complex with heavy metal ions that are unfavorable to the polymerization reaction, thereby shielding the influence of the heavy metal ions.

[0043] The present invention polymerizes sulfur-nitrogen-containing monomers and introduces them into the alumina synthesis process, using an in-situ polymerization-decomposition method, which not only uniformly introduces nitrogen and sulfur atoms into the alumina, but also changes the pore structure of the alumina, increases the specific surface area, and significantly increases the mesopore volume, thereby improving the adsorption performance. DETAILED DESCRIPTION

[0044] The present invention is described in detail below in conjunction with specific embodiments. It is necessary to point out that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by those skilled in the art based on the contents of the present invention still fall within the scope of protection of the present invention.

[0045] The test instruments and test conditions used in the examples are as follows:

[0046] The test method for the adsorption amount of basic fuchsin is as follows: 50 ml of basic fuchsin solution with an initial concentration of 200 mg / L is mixed with 20 g of the aluminum oxide sample to be tested, stirred at 600 rpm, and after adsorption for 60 minutes, the mixture is filtered under reduced pressure, and the filtrate is measured using an ultraviolet spectrophotometer. The adsorption amount of basic fuchsin by aluminum oxide is obtained by calculation.

[0047] The specific surface area and mesopore volume were measured using a surface area analyzer using the BET principle and helium as the adsorption gas.

[0048] Sulfur and nitrogen contents were determined using a sulfur and nitrogen analyzer.

[0049] The raw materials used in the examples and comparative examples, unless otherwise specified, are disclosed in the prior art, for example, they can be directly purchased or prepared according to the preparation methods disclosed in the prior art.

[0050] Example 1

[0051] (1) Add 12 g of 2-acrylamido-2-methylpropanesulfonic acid (AMPS) and 88 g of deionized water into a flask, adjust the pH value to 9 with 0.8 mol / L sodium hydroxide solution, and introduce nitrogen to deoxygenate for 30 min;

[0052] (2) 160 g of sodium aluminate was dissolved in 2000 g of deionized water to prepare a solution, and a mixed gas containing carbon dioxide and nitrogen in a ratio (volume ratio) of 1:1 was introduced at 30° C. for neutralization reaction, and the end point pH value was 8. After the neutralization reaction, the solution was aged for 5 h;

[0053] (3) After filtering the solid-liquid mixture and washing with deionized water, the AMPS sodium salt solution obtained in step (1) was added, and then 0.01 g of disodium ethylenediaminetetraacetate as an auxiliary agent, 0.004 g of potassium persulfate as an initiator, and 0.003 g of sodium bisulfite were added, and the polymerization reaction was carried out at 40° C. for 4 hours;

[0054] (4) The product obtained after the polymerization reaction in step (3) was kneaded for 30 minutes, dried at 120° C. for 10 hours, and calcined at 400° C. for 5 hours in a nitrogen atmosphere to obtain nitrogen-sulfur doped activated alumina.

[0055] After analysis, the sulfur content in the nitrogen-sulfur doped activated alumina sample obtained in Example 1 was 1.81 wt %, and the nitrogen content was 0.80 wt %.

[0056] Example 2

[0057] The operation steps and methods are the same as those in Example 1, the amount of AMPS used is 6g AMPS, 54g deionized water, and the initiators used in the polymerization process are 0.002g potassium persulfate and 0.002g sodium bisulfite. The specific operation is:

[0058] (1) Add 6 g of 2-acrylamido-2-methylpropanesulfonic acid (AMPS) and 54 g of deionized water into a flask, adjust the pH value to 9 with 0.8 mol / L sodium hydroxide solution, and introduce nitrogen for deoxygenation for 30 min;

[0059] (2) 160 g of sodium aluminate was dissolved in 2000 g of deionized water to prepare a solution, and a mixed gas containing carbon dioxide and nitrogen in a ratio (volume ratio) of 1:1 was introduced at 30° C. for neutralization reaction, and the end point pH value was 8. After the neutralization reaction, the solution was aged for 5 h;

[0060] (3) After filtering the solid-liquid mixture and washing with deionized water, the AMPS sodium salt solution obtained in step (1) was added, and then 0.01 g of disodium ethylenediaminetetraacetate as an auxiliary agent, 0.002 g of potassium persulfate as an initiator, and 0.002 g of sodium bisulfite were added, and the polymerization reaction was carried out at 40° C. for 4 h;

[0061] (4) The product obtained after the polymerization reaction in step (3) was kneaded for 30 minutes, dried at 120° C. for 10 hours, and calcined at 400° C. for 5 hours in a nitrogen atmosphere to obtain nitrogen-sulfur doped activated alumina.

[0062] After analysis, the sulfur content in the nitrogen-sulfur doped activated alumina sample obtained in Example 2 was 0.90wt%, and the nitrogen content was 0.39wt%.

[0063] Example 3

[0064] The operation steps and methods are the same as those in Example 1, and the neutralization reaction is carried out with a mixture of carbon dioxide and nitrogen in a ratio of 1:1, and the end point pH value is 7. The specific operation is:

[0065] (1) Add 12 g of 2-acrylamido-2-methylpropanesulfonic acid (AMPS) and 88 g of deionized water into a flask, adjust the pH value to 9 with 0.8 mol / L sodium hydroxide solution, and introduce nitrogen for deoxygenation for 30 min;

[0066] (2) 160 g of sodium aluminate was dissolved in 2000 g of deionized water to prepare a solution, and a mixed gas containing carbon dioxide and nitrogen in a ratio (volume ratio) of 1:1 was introduced at 30° C. for neutralization reaction, and the end point pH value was 7. After the neutralization reaction, the solution was aged for 5 h;

[0067] (3) After filtering the solid-liquid mixture and washing with deionized water, the AMPS sodium salt solution obtained in step (1) was added, and then 0.01 g of disodium ethylenediaminetetraacetate as an auxiliary agent, 0.004 g of potassium persulfate as an initiator, and 0.003 g of sodium bisulfite were added, and the polymerization reaction was carried out at 40° C. for 4 hours;

[0068] (4) The product obtained after the polymerization reaction in step (3) was kneaded for 30 minutes, dried at 120° C. for 10 hours, and calcined at 400° C. for 5 hours in a nitrogen atmosphere to obtain nitrogen-sulfur doped activated alumina.

[0069] After analysis, the sulfur content in the nitrogen-sulfur doped activated alumina sample obtained in Example 3 was 1.85wt%, and the nitrogen content was 0.83wt%.

[0070] Example 4

[0071] The operation steps and methods are the same as those in Example 1, and the sodium aluminate solution is neutralized with dilute sulfuric acid, and the end point pH value is controlled to be 7. The specific operation is:

[0072] (1) Add 12 g of 2-acrylamido-2-methylpropanesulfonic acid (AMPS) and 88 g of deionized water into a flask, adjust the pH value to 9 with 0.8 mol / L sodium hydroxide solution, and introduce nitrogen for deoxygenation for 30 min;

[0073] (2) 160 g of sodium aluminate was dissolved in 2000 g of deionized water to prepare a solution, and 0.4 mol / L dilute sulfuric acid was added at 30° C. for neutralization reaction. The end point pH value was 7. After the neutralization reaction, the solution was aged for 5 h;

[0074] (3) After filtering the solid-liquid mixture and washing with deionized water, the AMPS sodium salt solution obtained in step (1) was added, and then 0.01 g of disodium ethylenediaminetetraacetate as an auxiliary agent, 0.004 g of potassium persulfate as an initiator, and 0.003 g of sodium bisulfite were added, and the polymerization reaction was carried out at 40° C. for 4 hours;

[0075] (4) The product obtained after the polymerization reaction in step (3) was kneaded for 30 minutes, dried at 120° C. for 10 hours, and calcined at 400° C. for 5 hours in a nitrogen atmosphere to obtain nitrogen-sulfur doped activated alumina.

[0076] After analysis, the sulfur content in the nitrogen-sulfur doped activated alumina sample obtained in Example 4 was 1.85wt%, and the nitrogen content was 0.84wt%.

[0077] Example 5

[0078] The operation steps and methods are the same as those in Example 1, and the polymerization reaction is carried out at 40°C for 8 hours. The specific operation is:

[0079] (1) Add 12 g of 2-acrylamido-2-methylpropanesulfonic acid (AMPS) and 88 g of deionized water into a flask, adjust the pH value to 9 with 0.8 mol / L sodium hydroxide solution, and introduce nitrogen for deoxygenation for 30 min;

[0080] (2) 160 g of sodium aluminate was dissolved in 2000 g of deionized water to prepare a solution, and a mixed gas containing carbon dioxide and nitrogen in a ratio (volume ratio) of 1:1 was introduced at 30° C. for neutralization reaction, and the end point pH value was 8. After the neutralization reaction, the solution was aged for 5 h;

[0081] (3) After filtering the solid-liquid mixture and washing with deionized water, the AMPS sodium salt solution obtained in step (1) was added, and then 0.01 g of disodium ethylenediaminetetraacetate as an auxiliary agent, 0.004 g of potassium persulfate as an initiator, and 0.003 g of sodium bisulfite were added, and the polymerization reaction was carried out at 40° C. for 8 h;

[0082] (4) The product obtained after the polymerization reaction in step (3) was kneaded for 30 minutes, dried at 120° C. for 10 hours, and calcined at 400° C. for 5 hours in a nitrogen atmosphere to obtain nitrogen-sulfur doped activated alumina.

[0083] After analysis, the sulfur content in the nitrogen-sulfur doped activated alumina sample obtained in Example 5 was 1.79wt%, and the nitrogen content was 0.75wt%.

[0084] Example 6

[0085] The operation steps and methods are the same as those in Example 1, the calcination temperature is 500°C, and the calcination time is 5 hours. The specific operations are:

[0086] (1) Add 12 g of 2-acrylamido-2-methylpropanesulfonic acid (AMPS) and 88 g of deionized water into a flask, adjust the pH value to 9 with 0.8 mol / L sodium hydroxide solution, and introduce nitrogen for deoxygenation for 30 min;

[0087] (2) 160 g of sodium aluminate was dissolved in 2000 g of deionized water to prepare a solution, and a mixed gas containing carbon dioxide and nitrogen in a ratio (volume ratio) of 1:1 was introduced at 30° C. for neutralization reaction, and the end point pH value was 8. After the neutralization reaction, the solution was aged for 5 h;

[0088] (3) After filtering the solid-liquid mixture and washing with deionized water, the AMPS sodium salt solution obtained in step (1) was added, and then 0.01 g of disodium ethylenediaminetetraacetate as an auxiliary agent, 0.004 g of potassium persulfate as an initiator, and 0.003 g of sodium bisulfite were added, and the polymerization reaction was carried out at 40° C. for 4 hours;

[0089] (4) The product obtained after the polymerization reaction in step (3) was kneaded for 30 minutes, dried at 120° C. for 10 hours, and calcined at 500° C. for 5 hours in a nitrogen atmosphere to obtain nitrogen-sulfur doped activated alumina.

[0090] After analysis, the sulfur content in the nitrogen-sulfur doped activated alumina sample obtained in Example 6 was 1.37wt%, and the nitrogen content was 0.63wt%.

[0091] Example 7

[0092] The operation steps and methods are the same as those in Example 1, the amount of AMPS used is 1.25g AMPS, 12g deionized water, and the initiators potassium persulfate 0.001g and sodium bisulfite 0.001g are used in the polymerization process. The specific operation is:

[0093] (1) Add 1.25 g of 2-acrylamido-2-methylpropanesulfonic acid (AMPS) and 12 g of deionized water into a flask, adjust the pH value to 9 with 0.8 mol / L sodium hydroxide solution, and introduce nitrogen for deoxygenation for 30 min;

[0094] (2) 160 g of sodium aluminate was dissolved in 2000 g of deionized water to prepare a solution, and a mixed gas containing carbon dioxide and nitrogen in a ratio (volume ratio) of 1:1 was introduced at 30° C. for neutralization reaction, and the end point pH value was 8. After the neutralization reaction, the solution was aged for 5 h;

[0095] (3) After filtering the solid-liquid mixture and washing with deionized water, the AMPS sodium salt solution obtained in step (1) was added, and then 0.01 g of disodium ethylenediaminetetraacetate as an auxiliary agent, 0.001 g of potassium persulfate as an initiator, and 0.001 g of sodium bisulfite were added, and the polymerization reaction was carried out at 40° C. for 4 hours;

[0096] (4) The product obtained after the polymerization reaction in step (3) was kneaded for 30 minutes, dried at 120° C. for 10 hours, and calcined at 400° C. for 5 hours in a nitrogen atmosphere to obtain nitrogen-sulfur doped activated alumina.

[0097] After analysis, the sulfur content in the nitrogen-sulfur doped activated alumina sample obtained in Example 7 was 0.20wt%, and the nitrogen content was 0.08wt%.

[0098] Example 8

[0099] The operation steps and methods are the same as those in Example 1, except that the auxiliary agent is replaced with 0.025 g of citric acid. The specific operation is:

[0100] (1) Add 12 g of 2-acrylamido-2-methylpropanesulfonic acid (AMPS) and 88 g of deionized water into a flask, adjust the pH value to 9 with 0.8 mol / L sodium hydroxide solution, and introduce nitrogen for deoxygenation for 30 min;

[0101] (2) 160 g of sodium aluminate was dissolved in 2000 g of deionized water to prepare a solution, and a mixed gas containing carbon dioxide and nitrogen in a ratio (volume ratio) of 1:1 was introduced at 30° C. for neutralization reaction, and the end point pH value was 8. After the neutralization reaction, the solution was aged for 5 h;

[0102] (3) After filtering the solid-liquid mixture and washing with deionized water, the AMPS sodium salt solution obtained in step (1) was added, and then 0.025 g of citric acid as an auxiliary agent, 0.004 g of potassium persulfate as an initiator, and 0.003 g of sodium bisulfite were added, and the polymerization reaction was carried out at 40° C. for 4 h;

[0103] (4) The product obtained after the polymerization reaction in step (3) was kneaded for 30 minutes, dried at 120° C. for 10 hours, and calcined at 400° C. for 5 hours in a nitrogen atmosphere to obtain nitrogen-sulfur doped activated alumina.

[0104] After analysis, the sulfur content in the nitrogen-sulfur doped activated alumina sample obtained in Example 8 was 1.78wt%, and the nitrogen content was 0.79wt%.

[0105] Comparative Example 1

[0106] Dissolve 160g of sodium aluminate solution in 2000g of deionized water to prepare a solution, and introduce a mixed gas containing carbon dioxide and nitrogen in a ratio (volume ratio) of 1:1 at 30°C for neutralization reaction, with an end point pH value of 8. After neutralization reaction, age for 5h; filter and wash the solid-liquid mixture. Finally, dry at 120°C for 10h, and calcine at 400°C for 5h in a nitrogen atmosphere to obtain activated alumina.

[0107] Comparative Example 2

[0108] Dissolve 160g of sodium aluminate solution in 2000g of deionized water to prepare a solution. First, add 12g of AMPS, and introduce a mixed gas containing carbon dioxide and nitrogen in a ratio (volume ratio) of 1:1 at 30°C for neutralization reaction. The end point pH value is 8. After the neutralization reaction, age for 5h; filter and wash the solid-liquid mixture. Finally, dry at 120°C for 10h, and calcine at 400°C for 5h in a nitrogen atmosphere to obtain activated alumina.

[0109] Table 1. Test results of different samples

[0110]

[0111] Judging from the reaction evaluation results, by doping nitrogen and sulfur, the alumina material increases the specific surface area and significantly increases the mesopore volume, and the adsorption performance is significantly improved.

Claims

1. A nitrogen-sulfur doped activated alumina comprising: An alumina carrier and a nitrogen-containing sulfur component supported on the alumina carrier.

2. The nitrogen-sulfur doped activated alumina according to claim 1, characterized in that: The nitrogen-sulfur doped activated alumina has a nitrogen content of 0.08-0.90 wt% and a sulfur content of 0.2-2 wt%; and / or, The specific surface area of ​​the nitrogen-sulfur doped activated alumina is 100 to 600 m 2 / g, preferably 150 to 500 m 2 / g; and / or, The pore volume of the nitrogen-sulfur doped activated alumina is 0.2-1.2 ml / g, preferably 0.3-1.0 ml / g.

3. The nitrogen-sulfur doped activated alumina according to claim 1 or 2, characterized in that: The nitrogen-sulfur doped active alumina is prepared from an aluminum source and an amide sulfonic acid polymer.

4. A method for preparing the nitrogen-sulfur doped activated alumina according to any one of claims 1 to 3, comprising: The nitrogen-sulfur doped activated alumina is obtained by calcining the alumina loaded with amide sulfonic acid polymer.

5. The preparation method according to claim 4, characterized in that: The preparation method comprises the following steps: (1) adding a basic compound to a solution of an amide sulfonic acid monomer compound to neutralize the solution, and then introducing a protective gas to remove oxygen; (2) adding an acidic compound to a sodium aluminate solution for neutralization reaction, aging, and filtering; (3) adding the solid obtained by filtration in step (2) to the deoxygenated amide sulfonic acid monomer compound solution in step (1), then adding an auxiliary agent and an initiator, and heating for polymerization reaction; (4) kneading, drying and calcining the product obtained after the polymerization reaction in step (3) to obtain the nitrogen-sulfur doped activated alumina.

6. The preparation method according to claim 5, characterized in that: In the step (1): The amide sulfonic acid monomer compound is 2-acrylamide-2-methylpropane sulfonic acid; and / or, The concentration of the amide sulfonic acid monomer compound solution is 3 to 15 wt %, preferably 5 to 12 wt %; and / or, The alkaline compound is selected from inorganic alkaline compounds, preferably at least one selected from sodium hydroxide, sodium carbonate, potassium hydroxide, and ammonia water; and / or, The pH of the neutralized solution is 6-10.

7. The preparation method according to claim 5, characterized in that: In the step (2): The concentration of the sodium aluminate solution is 3 to 35 wt%, preferably 5 to 30 wt%; and / or, The acidic compound is selected from at least one of an inorganic acid and CO2, preferably, the inorganic acid is selected from at least one of hydrochloric acid, sulfuric acid and nitric acid; and / or, The mass ratio of the sodium aluminate to the amide sulfonic acid monomer compound is (13-130):1; and / or, The conditions of the neutralization reaction are: reacting under a protective gas atmosphere, and the pH at the reaction end point is 7 to 9; and / or, The aging condition is aging at 20-50° C. for 2-24 hours.

8. The preparation method according to claim 5, characterized in that: In the step (3): The auxiliary agent is selected from at least one of disodium ethylenediaminetetraacetate and citric acid; and / or, Based on 100 wt% of the mass of the amide sulfonic acid monomer compound, the amount of the auxiliary agent does not exceed 0.25 wt%; and / or, The initiator is selected from an oxidation-reduction initiation system; and / or, The conditions of the polymerization reaction are: polymerization temperature is 30-60° C., and polymerization time is 2-10 hours.

9. The preparation method according to claim 8, characterized in that: In the initiator: The oxidant is a persulfate, preferably at least one selected from potassium persulfate and sodium persulfate; and / or, The reducing agent is a sulfite, preferably at least one selected from sodium bisulfite and potassium sulfite; and / or, Based on 100 wt% of the mass of the amide sulfonic acid monomer compound, the amount of the oxidant is 0.01-0.1 wt%, and the amount of the reducing agent is 0.005-0.05 wt%.

10. The preparation method according to claim 5, characterized in that: In the step (4): The kneading time is 10 to 60 minutes; and / or, The drying temperature is 120 to 200°C; and / or, The calcination conditions are: carried out in a protective gas atmosphere, the calcination temperature is 350-550° C., and the calcination time is 2-10 hours.

Citation Information

Patent Citations

  • Hydrotreating catalyst intermediate, hydrotreating catalyst, and preparation methods of hydrotreating catalyst intermediate and hydrotreating catalyst

    CN106946807A

  • Hydrogenation treatment catalyst and preparation method thereof

    CN109772387A

  • Hydrogenation treatment catalyst as well as preparation method and application thereof

    CN109772400A

  • Hydrotreating catalyst, preparation method and applications thereof

    CN110090654A

  • Process for preparing active alumina by sodium metaaluminate-carbon dioxide method

    CN1254684A