Method for quickly adjusting negative difference by using weight of steel billet entering furnace

By calculating the difference between the weight of the steel billet entering the furnace and the actual length, and adjusting the diameter of the bar to adjust its length, the problem in the existing technology that it is difficult for the adjuster to quickly and accurately adjust the negative difference is solved, and the rapid and precise adjustment of the negative difference is achieved. The rolling efficiency and yield rate are improved.

CN118808329AActive Publication Date: 2024-10-22LINGYUAN IRON & STEEL CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411023974.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-10-22
Estimated Expiration
2044-07-29

AI Technical Summary

Technical Problem

In the existing technology, the adjuster cannot quickly and accurately adjust the negative difference of the bar, which affects the rolling efficiency and yield rate, and too many adjustments at one time can easily cause scrap.

Method used

By calculating the difference between the weight of the billet entering the furnace and the actual length, adjusting the diameter of the bar to adjust its length, using the formula L0=∣G1-G0∣×T÷X to calculate the theoretical length difference, and based on the actual length difference and the theoretical The difference in length difference adjusts the diameter of the rod. If the difference is too large, the diameter is increased. If the difference is too small, the diameter is reduced to achieve rapid adjustment of negative differences.

Benefits of technology

It achieves rapid and precise adjustment of the bar negative difference, ensuring that the comprehensive negative difference during the rolling process is within the standard range, improving the yield rate, and is simple to operate, without the need for additional equipment, and can be easily operated by workers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118808329A_ABST
    Figure CN118808329A_ABST
Patent Text Reader

Abstract

The invention discloses a method for quickly adjusting a negative difference by using the weight of a steel billet in a furnace, which is used for double-length rolling cutting of a bar and comprises the following steps of: adjusting a shearing head and a shearing tail according to the reference weight to ensure that the double-length lengths of all sections on a cooling bed are consistent, acquiring the weight of the blank, calculating a theoretical length difference value based on the weight of the blank, and acquiring the actual length of the tail section after rolling cutting. According to the method, the actual length difference value of the actual tail section length and the multiple length is calculated, and the diameter of the bar is adjusted according to the difference value of the actual length difference value and the theoretical length difference value. The method comprises the following steps of: calculating and adjusting the actual length difference value of a product which is actually produced, comparing the length to confirm the negative difference value, and adjusting the length of the bar by adjusting the diameter of the bar, so that the bar with the fixed length meets the production requirement and is close to the maximum negative difference value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of steel negative differential rolling, and more specifically, relates to a method for quickly adjusting the negative differential by utilizing the weight of a steel billet entering a furnace. Background Art

[0002] Bars (rebars) have their own international standards, that is, theoretical weights, according to different specifications and models, but the actual steel produced is often lighter than this weight. This difference is the negative difference. The negative difference is an important technical and economic indicator of a steel rolling mill and an effective way to reduce costs, increase efficiency and improve the yield rate. Because the adjuster cannot immediately adjust the negative difference to the right position during the slot change trial rolling in each shift, the rolling of the comprehensive negative difference is affected, which affects the yield rate; but too much adjustment at one time can easily cause the negative difference to exceed the national standard quality requirements and produce scrap. Quickly and accurately adjusting the negative difference is a difficult problem for bar and wire rolling adjusters, so they have been committed to how to quickly adjust the negative difference so that the negative difference rolling can be completed in one step.

[0003] Therefore, a method is needed to quickly and accurately adjust the bar deviation. Summary of the invention

[0004] The purpose of the present invention is to provide a method for quickly adjusting the negative difference by utilizing the weight of the steel billet entering the furnace in view of the deficiencies in the prior art, so as to solve the problem that the existing adjustment process cannot immediately adjust the negative difference to the right position, thus affecting the rolling of the comprehensive negative difference.

[0005] In order to achieve the above object, the present invention provides a method for quickly adjusting the negative difference by using the weight of the billet entering the furnace, which is used for bar multiple-length rolling and cutting, comprising:

[0006] Adjust the shear head and tail according to the reference weight to make the lengths of each section of the upper cooling bed consistent;

[0007] Obtain the weight of the blank, and calculate the theoretical length difference based on the weight of the blank;

[0008] Obtain the actual tail section length after rolling and cutting, and calculate the actual length difference between the actual tail section length and the multiple length;

[0009] Adjust the rod diameter according to the difference between the actual length difference and the theoretical length difference;

[0010] The calculation formula of the theoretical tail section length difference is: L0 = |G1-G0| × T÷X;

[0011] Among them: L0 is the theoretical length difference; L1 is the actual tail length; L2 is the multiple length; G0 is the reference weight; G1 is the blank weight; T is the length compensation value; X is the cutting number.

[0012] Optionally, adjusting the rod diameter according to the length difference includes:

[0013] Adjust the rolling mill so that the inner diameter of each rolling pass of the rolling mill increases or decreases synchronously.

[0014] Optionally, if L0 < L1-L2, reduce the rod diameter;

[0015] If L0>L2-L1, increase the rod diameter.

[0016] Optionally, when the bar is threaded steel, the threads are adjusted in proportion.

[0017] Optionally, the multiple length is set to 96.5m.

[0018] Optionally, when the rod is Φ16 and the negative difference is 3.9%, G0=2196kg; T=1.58kg / m; X=3.

[0019] Optionally, when the rod is Φ18 and the negative difference is 3.9%, G0=2216kg; T=2kg / m; X=2.

[0020] Optionally, when the rod is Φ20 and the negative difference is 3.9%, G0=2212kg; T=2.47kg / m; X=2.

[0021] Optionally, when the rod is Φ22 and the negative difference is 2.9%, G0=2210kg; T=2.98kg / m; X=2.

[0022] Optionally, when the rod is Φ25 and the negative difference is 2.9%, G0=2200kg; T=3.85kg / m; X=1.

[0023] The present invention provides a method for quickly adjusting the negative difference by using the weight of the billet entering the furnace, and the beneficial effects thereof are:

[0024] 1. The method of quickly adjusting the negative difference by using the weight of the billet entering the furnace can calculate the theoretical length difference of the tail section of the bar according to the standard or product requirements, and then calculate and adjust it with the actual length difference of the actually produced product. The size of the negative difference can be confirmed by comparing the lengths, and then the length of the bar can be adjusted by adjusting the diameter of the bar, so that the fixed-length bar meets the production requirements and is close to the maximum negative difference.

[0025] 2. This method of quickly adjusting the negative difference by using the weight of the billet entering the furnace is simple to use and has obvious effects. It does not require additional equipment and can be easily operated by frontline workers.

[0026] Other features and advantages of the present invention will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] The above and other objects, features and advantages of the present invention will become more apparent through a more detailed description of exemplary embodiments of the present invention in conjunction with the accompanying drawings, wherein like reference numerals generally represent like components throughout the exemplary embodiments of the present invention.

[0028] Figure 1 A schematic flow chart of a method for quickly adjusting a negative difference using the weight of a billet entering a furnace according to an embodiment of the present invention is shown. DETAILED DESCRIPTION

[0029] The preferred embodiments of the present invention will be described in more detail below. Although the preferred embodiments of the present invention are described below, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided to make the present invention more thorough and complete, and to fully convey the scope of the present invention to those skilled in the art.

[0030] like Figure 1 As shown, a method for quickly adjusting the negative difference by using the weight of the billet entering the furnace is used for bar multiple-length rolling and cutting, comprising:

[0031] Adjust the shear head and tail according to the reference weight to make the lengths of each section of the upper cooling bed consistent;

[0032] Obtain the weight of the blank, and calculate the theoretical length difference based on the weight of the blank;

[0033] Obtain the actual tail section length after rolling and cutting, and calculate the actual length difference between the actual tail section length and the multiple length;

[0034] Adjust the rod diameter according to the difference between the actual length difference and the theoretical length difference;

[0035] The calculation formula of the theoretical tail section length difference is: L0 = |G1-G0| × T÷X;

[0036] Among them: L0 is the theoretical length difference; L1 is the actual tail length; L2 is the multiple length; G0 is the reference weight; G1 is the blank weight; T is the length compensation value; X is the cutting number.

[0037] Specifically, the length and weight of the shear head and tail are set according to experience, so that the length of each section of the cooling bed is consistent. This weight can be used as a reference value. Then the theoretical length difference of the tail section of the bar is calculated according to the standard or product requirements, and then the actual length difference of the actual product is calculated and adjusted. The size of the negative difference is confirmed by comparing the lengths, and then the length of the bar can be adjusted by adjusting the diameter of the bar.

[0038] Furthermore, a blank of a certain weight can be adjusted in length by changing the cross section, thereby changing the weight at a fixed length of multiple lengths.

[0039] Furthermore, when implementing on site, it is also necessary to make difference compensation according to the steel type, composition, oxidation and burning loss, etc., and a 0.2% compensation margin can be reserved to adapt to fluctuation compensation. For example, for a Φ16 bar, the negative difference is set to 3.7%.

[0040] In this embodiment, adjusting the rod diameter according to the length difference includes:

[0041] Adjust the rolling mill so that the inner diameter of each rolling pass of the rolling mill increases or decreases synchronously.

[0042] Specifically, different processes have different cutting quantities, and the inner diameters of each roller are adjusted synchronously.

[0043] In this embodiment, if L0 < L1-L2, the rod diameter is reduced;

[0044] If L0>L2-L1, increase the rod diameter.

[0045] Specifically, if L0<L1-L2, the weight of a fixed length of a multiple is too large, and the negative difference is acceptable with a margin, so you can try to reduce the diameter of the bar;

[0046] If L0<L1-L2, the weight of the fixed length of a multiple is too large, and the negative difference exceeds the tolerance, so the diameter of the bar should be increased.

[0047] Furthermore, according to experience, the diameter R is inversely proportional to the actual tail section length L1, and the diameter R is inversely proportional to the negative difference. The smaller R is, the larger the negative difference is.

[0048] In this embodiment, when the bar material is threaded steel, the threads are adjusted in proportion.

[0049] Specifically, threads are arranged on the surface of the threaded steel bar, and the thread parameters are adjusted in association with the rod diameter.

[0050] In this embodiment, the multiple length setting length is 96.5m.

[0051] Specifically, the calibration length is set according to the bar parameters.

[0052] In this embodiment, when the rod is Φ16 and the negative difference is 3.9%, G0=2196kg; T=1.58kg / m; X=3.

[0053] In this embodiment, when the rod is Φ18 and the negative difference is 3.9%, G0=2216kg; T=2kg / m; X=2.

[0054] In this embodiment, when the rod is Φ20 and the negative difference is 3.9%, G0=2212kg; T=2.47kg / m; X=2.

[0055] In this embodiment, when the rod is Φ22 and the negative difference is 2.9%, G0=2210kg; T=2.98kg / m; X=2.

[0056] In this embodiment, when the rod is Φ25 and the negative difference is 2.9%, G0=2200kg; T=3.85kg / m; X=1.

[0057] Example

[0058] Different rods are equipped with different production and processing technologies, as shown in the table:

[0059]

[0060] Take the bar Φ18, the negative difference is 3.9%, G0=2216kg; T=2kg / m; X=2 as an example:

[0061] The billet weight was measured to be 2212kg before loading, and the 1# and 2# shear heads and tails were adjusted to the best state. The shear lengths were 60mm and 280mm respectively; the multiple was adjusted to 96.5m, and when the negative difference was rolled to 3.9%, L0 was 4m;

[0062] After rolling, the actual tail section length is 94.5m, 2m shorter than 96.5m, and the billet weight is 4KG less than the benchmark value.

[0063] Because the actual tail section length is 2m longer than the calculated one, the negative difference is higher than 3.9% at this time. The rolling mill should be adjusted to increase the inner diameter and increase the diameter of the bar.

[0064] According to empirical data, the negative difference of 0.05mm material retraction and release is about 0.1% for adjustment.

[0065] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.

Claims

1. A method for rapidly adjusting the negative difference by using the weight of the billet entering the furnace, which is used for multiple-length rolling and cutting of bars, characterized in that: include: Adjust the shear head and tail according to the reference weight to make the lengths of each section of the upper cooling bed consistent; Obtain the weight of the blank, and calculate the theoretical length difference based on the weight of the blank; Obtain the actual tail section length after rolling and cutting, and calculate the actual length difference between the actual tail section length and the multiple length; Adjust the rod diameter according to the difference between the actual length difference and the theoretical length difference; The calculation formula of the theoretical tail section length difference is: L0 = |G1-G0| × T÷X; Where: L0 is the theoretical length difference; L1 is the actual tail length; L2 is the multiple length; G0 is the reference weight; G1 is the blank weight; T is the length compensation value; X is the cutting number.

2. The method for quickly adjusting the negative difference by using the weight of the billet entering the furnace according to claim 1 is characterized in that: The adjusting the rod diameter according to the length difference comprises: Adjust the rolling mill so that the inner diameter of each rolling pass of the rolling mill increases or decreases synchronously.

3. The method for quickly adjusting the negative difference by using the weight of the billet entering the furnace according to claim 1, characterized in that: If L0<L1-L2, reduce the rod diameter; If L0>L2-L1, increase the rod diameter.

4. The method for quickly adjusting the negative difference by using the weight of the billet entering the furnace according to claim 1, characterized in that: When the bar is threaded steel, the threads are adjusted proportionally.

5. The method for quickly adjusting the negative difference by using the weight of the billet entering the furnace according to claim 1, characterized in that: The multiple length setting is 96.5m.

6. The method for quickly adjusting the negative difference by using the weight of the billet entering the furnace according to claim 5, characterized in that: When the rod is Φ16 and the negative difference is 3.9%, G0=2196kg; T=1.58kg / m; X=3.

7. The method for quickly adjusting the negative difference by using the weight of the billet entering the furnace according to claim 5, characterized in that: When the rod is Φ18 and the negative difference is 3.9%, G0=2216kg; T=2kg / m; X=2.

8. The method for quickly adjusting the negative difference by using the weight of the billet entering the furnace according to claim 5, characterized in that: When the rod is Φ20 and the negative difference is 3.9%, G0=2212kg; T=2.47kg / m; X=2.

9. The method for quickly adjusting the negative difference by using the weight of the billet entering the furnace according to claim 5, characterized in that: For the rod Φ22 and the negative difference is 2.9%, G0=2210kg; T=2.98kg / m; X=2.

10. The method for automatically adding a covering agent to a ladle according to claim 5, characterized in that: When the bar is Φ25 and the negative difference is 2.9%, G0=2200kg; T=3.85kg / m; X=1.

Citation Information

Patent Citations

  • Method for controlling negative deviation of steel bar with rib

    CN101168171A

  • Negative deviation monitoring system and negative deviation detection calculation method for ribbed steel bars

    CN104858242A

  • Method for simply and conveniently controlling negative tolerance of hot-rolled ribbed steel bar finished product

    CN115365293A

  • Method for rolling fixed-weight blank and fixed-length material in square billet hot-delivery direct-rolling process

    CN118143057A

  • Negative allowance detection and control system for rolling bar material