Forging method of titanium material

Through the 5-fire forging method and the three-piercing and three-drawing process, gradually heating and performing large deformation reversal upsetting, the problem of insufficient mechanical properties and deformation uniformity of large-size titanium alloy bars has been solved, and efficient mechanical performance improvement and deformation uniformity have been achieved. The number of fires is reduced.

CN118808510APending Publication Date: 2024-10-22JIANGSU YUTI NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410788441.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-19
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

During the forging process of titanium alloys, existing technology is difficult to effectively improve the mechanical properties and deformation uniformity of large-size bars, resulting in low strength and poor plasticity.

Method used

Adopting a 5-fire forging method, each fire uses three piers and three drawing processes to gradually heat and carry out 35-40% large deformation and reversing upsetting, and finally perform shaping, rounding and annealing. The control temperatures are 1148-928℃ and 728℃.

Benefits of technology

Successfully reduced the number of forging fires, significantly improved the mechanical properties of titanium alloy large bars, complied with the GB/T 2965-2007 standard, and reached Class A flaw detection level.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention belongs to the field of titanium material forging, and particularly relates to a titanium material forging method. Forging is carried out by adopting five heating numbers, and a three-upsetting and three-drawing process is selected for each heating number; the forging method comprises the following steps: cogging and heating titanium and titanium alloy at 1148-1152 DEG C, and performing reversing upsetting and drawing by adopting 40% large deformation; after secondary heating at 1048-1052 DEG C, performing reversing upsetting and drawing by adopting 40% large deformation; carrying out third-fire heating at 978-982 DEG C, and then carrying out 35% reversing upsetting and drawing deformation; performing four-fire heating at 948-952 DEG C, and performing 35% reversing upsetting and drawing deformation; performing five-fire heating at 928-932 DEG C, performing 35% conventional deformation, and performing shaping and rounding; and annealing to complete the forging method of the titanium material. According to the method, large bar products are machined for titanium and titanium alloy, the number of forging fire is successfully reduced, and the mechanical performance of forged products is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of titanium material forging, and in particular relates to a titanium material forging method. Background Art

[0002] Forging is a processing method that uses a forging machine to apply pressure to a metal blank to cause it to undergo plastic deformation in order to obtain a forging with certain mechanical properties, shape, and size. It is one of the two major components of forging (forging and stamping).

[0003] Forging can eliminate defects such as loose castings produced during the metal smelting process, optimize the microstructure, and preserve complete metal flow lines. The mechanical properties of forgings are generally better than those of castings of the same material. Forgings are mostly used for important parts of related machinery with high loads and severe working conditions, except for simpler shapes that can be made of rolled plates, profiles or welded parts.

[0004] Titanium and titanium alloys are widely used in aviation, aerospace, shipbuilding, petroleum, chemical industry, weapons, electronics and other industries due to their excellent comprehensive mechanical properties. Forging is one of the important ways to produce titanium alloy parts. Through the forging method, not only can the appropriate forging shape be obtained, but more importantly, the mechanical properties of the alloy can be improved. During the forging process, the size of the deformation, the appropriate forging temperature and forging method are the key factors to control the quality of the forging. Using a large deformation, appropriate forging temperature and forging method can reduce the number of forging fires, improve the mechanical properties of the forging, meet the use requirements, and effectively reduce costs.

[0005] Titanium and titanium alloys have the main characteristics of high melting point, low density and high strength. They are widely used in aircraft engine structures, such as for manufacturing compressor disks, blades and other rotating parts that bear high pressure. Free forging is one of the main processing methods for forging titanium and titanium alloy bars, cakes and rings. As a process of free forging, reversing upsetting is widely used in the free forging process. It is a key process that must be used in the production process of large-size bars. Titanium and titanium alloys have small linear expansion coefficients, high tensile strength and poor metal fluidity. Therefore, if straight upsetting and straight drawing are used in the processing of large-size bad materials, uneven metal deformation, low strength and poor plasticity will be caused. However, the use of reversing upsetting can make the entire bad material cross section obtain a very uniform structure during the forging process, thereby improving the comprehensive performance of the product.

[0006] Compared with straight upsetting and straight drawing, the material deformation after reversing upsetting and drawing is uniform, with less dead zone; there is no large lamellar structure in the low-magnification structure, the microstructure is well equiaxed, and the primary a phase is evenly distributed on the matrix. The comprehensive mechanical properties of the finished bar after reversing upsetting and drawing are significantly improved compared with straight upsetting and straight drawing, with uniform deformation of the blank, fine grains, and improved strength.

[0007] The free forging of titanium and titanium alloys is divided into the following four processes:

[0008] 1. Material preparation: After smelting, titanium and titanium alloys need to be polished from the rough titanium ingots into finished titanium ingots, and the riser end needs to be cut off.

[0009] 2. Heating: Heat the titanium alloy blank to a suitable temperature, generally the β phase temperature (850℃~950℃), so that it can reach a state of plastic deformation. Titanium materials are very sensitive to temperature.

[0010] According to production experience: Generally, it takes 5.5 hours to heat a 3-ton TC4 titanium ingot to the specified temperature. It is divided into four sections: heating up, reaching temperature, keeping warm, and taking out of the furnace. Detailed records need to be made. The "Forging Temperature Record Sheet" includes a temperature rise curve.

[0011] 3. Forging: Put the heated titanium alloy billet into the forging machine for forging. Control the temperature and deformation (30% to 50%), and do not flatten the material with one hammer. First pull it out, then punch it back, three punches and three pulls, to break the defects such as loose casting produced in the metal smelting process.

[0012] 4. Cooling: After forging, the overheated titanium alloy billet is air-cooled to room temperature to increase its strength and toughness. There are other cooling methods: water cooling, air cooling, oil cooling, and furnace cooling. Summary of the invention

[0013] In order to solve the existing technical problems and enhance the performance of titanium alloy, this application provides the following technical solutions:

[0014] The present invention provides a forging method for titanium material, which adopts five firings for forging, and each firing adopts three-piercing and three-drawing processes; the forging method comprises the following steps:

[0015] S1: heating the workpiece at 1148-1152°C and then performing reversing upsetting with a large deformation of 35-40%; the workpiece is titanium or titanium alloy;

[0016] S2: After the reversing upsetting in step S1, the processed material is heated at 1048-1052°C and then reversing upsetting with a large deformation of 35-40%;

[0017] S3: the processed material after the reversing upsetting in step S2 is heated at 978-982°C for three times and then deformed by 32-35% reversing upsetting;

[0018] S4: the processed material after the reversing upsetting in step S3 is heated at 948-952°C and then deformed by 32-35% reversing upsetting;

[0019] S5: the processed material after the reversing upsetting in step S4 is heated at 928-932°C for five times and then deformed by 32-35% conventionally to be shaped and rounded;

[0020] S6: Annealing the processed material after the shaping and rounding in step S5 to complete the forging method of the titanium material.

[0021] Preferably, the temperature of the blank opening heating is 1150°C.

[0022] Preferably, the temperature of the second fire heating is 1050°C.

[0023] Preferably, the temperature of the triple-fire heating is 980°C.

[0024] Preferably, the temperature of the four-fire heating is 950°C.

[0025] Preferably, the temperature of the five-fire heating is 930°C.

[0026] Preferably, the processed material is TC4 titanium alloy material.

[0027] Preferably, the annealing temperature is 728-732°C.

[0028] Specifically, the annealing temperature is 730°C.

[0029] The present invention also provides a titanium material prepared by the above preparation method.

[0030] Preferably, the titanium material is a rod, and the diameter of the rod is 400 mm.

[0031] The technical solution of the present invention has the following advantages over the prior art:

[0032] The invention is aimed at processing large bar products of titanium and titanium alloys, successfully reduces the number of forging fires, and improves the mechanical properties of forged products.

[0033] The above TC4 titanium and titanium alloy large bars adopt this technical solution and their performance meets GB / T 2965-2007; DETAILED DESCRIPTION

[0034] The present invention is further described below in conjunction with specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.

[0035] Example 1

[0036] A forging method for titanium material, the steps are as follows:

[0037] (1) TC4 titanium alloy was heated at 1150°C and then subjected to reversing upsetting with a maximum deformation of 35%;

[0038] (2) the processed material after the reversing upsetting in step S1 is heated at 1050° C. and then reversing upsetting with a maximum deformation of 35%;

[0039] (3) The processed material after the reversing upsetting in step S2 is heated at 980° C. for three times and then deformed by 32% reversing upsetting;

[0040] (4) the processed material after the reversing upsetting in step S3 is heated at 950° C. and then deformed by 32% reversing upsetting;

[0041] (5) The processed material after the reversing upsetting in step S4 is heated at 930° C. for five times and then deformed by 32% conventionally to form a round shape;

[0042] (6) The processed material after the rounding in step S5 is annealed at 730° C. to complete the forging method of the titanium material.

[0043] Example 2

[0044] A forging method for titanium material, the steps are as follows:

[0045] (1) TC4 titanium alloy was heated at 1148°C and then subjected to reversing upsetting with a maximum deformation of 35%;

[0046] (2) the processed material after the reversing upsetting in step S1 is heated at 1048°C for a second time and then reversing upsetting with a maximum deformation of 35%;

[0047] (3) The processed material after the reversing upsetting in step S2 is heated at 978°C for three times and then deformed by 32% reversing upsetting;

[0048] (4) the processed material after the reversing upsetting in step S3 is heated at 948°C and then deformed by 32% reversing upsetting;

[0049] (5) The processed material after the reversing upsetting in step S4 is heated at 928° C. for five times and then deformed by 32% conventionally to form a round shape;

[0050] (6) The processed material after the rounding in step S5 is annealed at 728°C to complete the forging method of the titanium material.

[0051] Example 3

[0052] A forging method for titanium material, the steps are as follows:

[0053] (1) TC4 titanium alloy was heated at 1152°C and then subjected to reversing upsetting with a maximum deformation of 40%;

[0054] (2) the processed material after the reversing upsetting in step S1 is heated at 1052°C for a second time and then reversing upsetting with a maximum deformation of 40%;

[0055] (3) The processed material after the reversing upsetting in step S2 is heated at 982° C. for three times and then deformed by 35% reversing upsetting;

[0056] (4) The processed material after the reversing upsetting in step S3 is heated at 952° C. and then deformed by 35% reversing upsetting;

[0057] (5) The processed material after the reversing upsetting in step S4 is heated at 932° C. for five times and then deformed by 35% conventionally to form a round shape;

[0058] (6) The processed material after the rounding in step S5 is annealed at 732° C. to complete the forging method of the titanium material.

[0059] Example 4

[0060] A forging method for titanium material, the steps are as follows:

[0061] (1) The titanium metal is heated at 1150°C and then subjected to reversing upsetting with a maximum deformation of 35%;

[0062] (2) the processed material after the reversing upsetting in step S1 is heated at 1050° C. and then reversing upsetting with a maximum deformation of 35%;

[0063] (3) The processed material after the reversing upsetting in step S2 is heated at 980° C. for three times and then deformed by 32% reversing upsetting;

[0064] (4) the processed material after the reversing upsetting in step S3 is heated at 950° C. and then deformed by 32% reversing upsetting;

[0065] (5) The processed material after the reversing upsetting in step S4 is heated at 930° C. for five times and then deformed by 32% conventionally to form a round shape;

[0066] (6) The processed material after the rounding in step S5 is annealed at 730° C. to complete the forging method of the titanium material.

[0067] Effect evaluation 1

[0068] The above TC4 titanium and titanium alloy large bars adopt this technical solution, and their performance meets GB / T 2965-2007; the flaw detection grade reaches Class A standard.

[0069] Obviously, the above embodiments are merely examples for clear explanation and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the protection scope of the invention.

Claims

1. A forging method for titanium material, It is characterized in that The forging is performed by using 5 firings, and each firing is performed by using a three-pier and three-draw process; the forging method comprises the following steps: S1: heating the workpiece at 1148-1152°C and then performing reversing upsetting with a large deformation of 35-40%; the workpiece is titanium or titanium alloy; S2: After the reversing upsetting in step S1, the processed material is heated at 1048-1052°C and then subjected to reversing upsetting with a large deformation of 35-40%; S3: the processed material after the reversing upsetting in step S2 is heated at 978-982°C for three times and then deformed by 32-35% reversing upsetting; S4: the processed material after the reversing upsetting in step S3 is heated at 948-952°C and then deformed by 32-35% reversing upsetting; S5: the processed material after the reversing upsetting in step S4 is heated at 928-932°C for five times and then deformed by 32-35% conventionally to be shaped and rounded; S6: Annealing the processed material after the shaping and rounding in step S5 to complete the forging method of the titanium material.

2. The forging method of titanium material according to claim 1, It is characterized in that The heating temperature for the blank opening is 1150°C.

3. The forging method of titanium material according to claim 1, It is characterized in that The temperature of the second fire heating is 1050°C.

4. The forging method of titanium material according to claim 1, It is characterized in that The temperature of the three-fire heating is 980°C.

5. The forging method of titanium material according to claim 1, It is characterized in that The temperature of the four-fire heating is 950°C.

6. The forging method of titanium material according to claim 1, It is characterized in that The temperature of the five-fire heating is 930°C.

7. The forging method of titanium material according to claim 1, It is characterized in that The processed material is TC4 titanium alloy material.

8. The forging method of titanium material according to claim 1, It is characterized in that The annealing temperature is 728-732°C.

9. A titanium material prepared by the preparation method according to any one of claims 1 to 8.