Method for improving performance of magnesium alloy casting by optimizing self-lubricating property of die
By depositing a chromium aluminum nitride or titanium aluminum nitride coating on the surface of the mold and spraying a water-based release agent, the problem of reduced corrosion resistance of magnesium alloy castings during the demoulding process is solved, achieving results comparable to silicone oil-based release agents. Filling and demoulding properties while maintaining the corrosion resistance of the material.
Patent Information
- Application Number
- CN202410970763.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-10-22
AI Technical Summary
The use of silicone oil-based release agents in the demoulding process of existing magnesium alloy castings has resulted in a significant decrease in the material's corrosion resistance. Moreover, the traditional water-emulsion type release agents have poor filling and demoulding effects, making it difficult to maintain the material's resistance while ensuring performance. corrosive.
By depositing a chromium aluminum nitride or titanium aluminum nitride coating on the surface of the mold, and spraying a water-based release agent on it, the PVD process is used to form a high-temperature and durable coating, combined with a moderate friction coefficient and hardness, for magnesium alloy die-casting. Replaces silicone oil-based release agents.
It achieves filling and demoulding performance comparable to silicone oil-based release agents, while maintaining the corrosion resistance of magnesium alloy materials and avoiding the reduction in corrosion resistance caused by silicone oil residues.
Abstract
Description
Technical Field
[0001] The invention relates to the field of magnesium alloy casting, and in particular to a method for improving the performance of magnesium alloy castings by optimizing the self-lubricating property of a mold. Background Art
[0002] With the rapid development of the electronics industry and new energy vehicles, magnesium alloy materials are favored by designers and consumers for their low density, high specific strength, high damping and shock absorption, especially magnesium alloy die-casting or semi-solid injection molding parts, which are widely used due to their high degree of automation and production efficiency. In order to cool and demold the castings in the shortest possible time, a large amount of release agent is usually required. At present, the best mold filling and demolding effect on the market is silicone oil-based release agent, such as Chinese patent 201010239348.8; there are also a small number of silicone-free water-emulsion release agents, such as Chinese patent 201310466321.6, but the filling and demolding effects are not as good as traditional silicone oil-based release agents. Although silicone oil-based mold release agents can help with mold filling and demolding, the silicone oil remaining on the casting has the disadvantage of significantly reducing the corrosion resistance of magnesium alloy castings. Even materials with good corrosion resistance will have their corrosion resistance significantly reduced after die casting or semi-solid injection molding. In other words, the good corrosion resistance of the material is masked by the side effects of the mold release agent.
[0003] Therefore, it is an urgent need to develop a release agent that can ensure the filling and demolding effects without affecting the corrosion resistance of magnesium alloy materials, or to take other demolding measures to minimize the use of silicone oil-based release agents. Summary of the invention
[0004] The purpose of the present invention is to provide a method for improving the performance of magnesium alloy castings by optimizing the self-lubricating property of the mold, thereby solving the problem that the silicone oil in the existing mold release agent easily remains on the magnesium alloy castings, resulting in a significant decrease in the corrosion resistance of the magnesium alloy castings.
[0005] In order to achieve the above-mentioned purpose, the present invention provides a method for improving the performance of magnesium alloy castings by optimizing the self-lubricating property of the mold, characterized in that the method comprises: using a PVD process to deposit a chromium aluminum nitride coating or a titanium aluminum nitride coating on the surface of the mold steel, then spraying a water-based mold release agent on the coating, and using the treated mold to die-cast the magnesium alloy material. The method provided by the present invention first deposits a chromium aluminum nitride coating or a titanium aluminum nitride coating on the surface of the mold, and the coating has excellent high temperature resistance, a moderate friction coefficient, and a high hardness. When used in conjunction with a water-based mold release agent, it not only exceeds the filling and demolding performance of the magnesium alloy material using a silicone oil-based mold release agent, but also the corrosion resistance of the magnesium alloy material itself is well maintained.
[0006] Other features and advantages of the present invention will be described in detail in the following detailed description. DETAILED DESCRIPTION
[0007] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0008] Example 1
[0009] The PVD process is used to deposit a chromium aluminum nitride coating layer on the surface of the mold steel, and then a water-based mold release agent is sprayed on the coating, and the treated mold is used for die-casting of magnesium alloy materials; the high temperature resistance of the chromium aluminum nitride coating is 1000°C; the coating thickness is 3.5 microns; the friction coefficient is 0.35; and the coating hardness is 3200HV. Among them, the conditions of the PVD process include: the processing temperature is 350°C, the processing time is 4.5h, and the components of the water-based mold release agent include: relative to 100 parts by weight of deionized water, the content of paraffin is 5 parts by weight, the content of stearic acid is 2 parts by weight, the content of vegetable oil is 5 parts by weight, and the content of emulsifier is 5 parts by weight.
[0010] The magnesium alloy casting AZ91D after demolding by the method of Example 1 was subjected to a neutral salt spray resistance test, and the neutral salt spray resistance test data after the chemical coating treatment reached (48 hours, above level nine).
[0011] Example 2
[0012] The titanium aluminum nitride coating is deposited on the surface of the mold steel using the PVD process, and then a water-based mold release agent is sprayed on the coating, and the treated mold is used for die-casting of magnesium alloy materials. The high temperature resistance of the titanium aluminum nitride coating is 900°C; the coating thickness is 4 microns; the friction coefficient is 0.38; and the coating hardness is 3300HV. The conditions of the PVD process include: the processing temperature is 350°C and the processing time is 4.5h. The components of the water-based mold release agent include: relative to 100 parts by weight of deionized water, the content of paraffin is 20 parts by weight, the content of stearic acid is 6 parts by weight, the content of vegetable oil is 10 parts by weight, and the content of emulsifier is 8 parts by weight.
[0013] The magnesium alloy casting AZ91D after demolding by the method of Example 2 was subjected to a neutral salt spray resistance test, and the neutral salt spray resistance test data after the chemical coating treatment reached (72 hours, above level nine).
[0014] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0015] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0016] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
Claims
1. A method for improving the performance of magnesium alloy castings by optimizing the self-lubricating property of a mold, characterized in that: The method comprises: using a PVD process to deposit a chromium aluminum nitride coating or a titanium aluminum nitride coating on the surface of a mold steel, then spraying a water-based mold release agent on the coating, and using the processed mold to die-cast a magnesium alloy material.
2. The method according to claim 1, characterized in that The high temperature resistance of the chromium aluminum nitride coating is 900-1100°C; the coating thickness is 2-5 microns; The friction coefficient is 0.3-0.4; The coating hardness is 3100-3300HV.
3. The method according to claim 1, characterized in that The high temperature resistance of the titanium aluminum nitride coating is 800-1000° C.; the coating thickness is 2-6 microns; the friction coefficient is 0.35-0.4; and the coating hardness is 3200-3400 HV.
4. The method according to claim 1, characterized in that The conditions of the PVD process include: processing temperature of 250-450°C and processing time of 3-6h.
5. The method according to claim 1, characterized in that The components of the water-based release agent include paraffin, stearic acid, vegetable oil, emulsifier and deionized water.
6. The method according to claim 5, characterized in that The components of the aqueous release agent include: relative to 100 parts by weight of deionized water, 5-20 parts by weight of paraffin, 2-6 parts by weight of stearic acid, 5-10 parts by weight of vegetable oil, and 5-8 parts by weight of emulsifier.