MgAgSb thermoelectric material and preparation method and application thereof
Through principle calculation and optimized preparation process, a high-performance pure phase MgAgSb thermoelectric material was prepared, which solved the problem of insufficient performance of magnesium-silver-antimony-based thermoelectric materials, achieved efficient thermoelectric power generation and refrigeration performance, reduced costs, and was used in thermoelectric elements. The device exhibits excellent performance.
Patent Information
- Application Number
- CN202310414394.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-18
- Publication Date
- 2024-10-22
AI Technical Summary
Existing thermoelectric materials such as bismuth telluride-based materials are expensive and have low power generation efficiency at 300°C, which limits the further large-scale use of thermoelectric devices. All-magnesium-based thermoelectric elements are constructed of magnesium-silver-antimony and magnesium-bismuth-antimony based thermoelectric materials. The device has insufficient power generation and cooling performance, which affects commercial application.
Through principle calculation and adjustment of the preparation process, a synchronous transmission high-energy ball mill and cemented carbide balls are used for ball milling, combined with an annealing treatment at 310±2°C, to prepare pure phase MgAgSb thermoelectric materials, improving its carrier mobility and power factor. Realizing high-performance p-type magnesium-silver-antimony thermoelectric materials.
A breakthrough in the performance of magnesium-silver-antimony-based thermoelectric materials has been achieved. The carrier mobility reaches 93.3cm2 V-1s-1, the power factor is 25μW cm-1K-2, the room temperature thermoelectric figure of merit zT reaches 0.97, and zT reaches 1.6 at 250°C. , surpassing the performance of traditional laboratory samples, reducing material costs, and showing excellent performance in thermoelectric power generation and refrigeration devices.
Smart Images

Figure CN118808658A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of thermoelectric materials, and in particular relates to a MgAgSb thermoelectric material and a preparation method and application thereof. Background Art
[0002] Thermoelectric materials can realize the mutual conversion between heat energy and electric energy. Thermoelectric components made of them have the characteristics of light weight, small size, no pollution, simple structure, no noise, long service life and can be used in some extreme environments such as deep sea and space. This is of great significance to solving the current energy crisis and environmental pollution problems faced by mankind, and has also been highly valued by countries around the world.
[0003] At present, the world's energy structure is still dominated by fossil fuels. Nearly 60% of the energy generated by the combustion of fossil fuels is dissipated in the form of waste heat, of which more than half is within 300°C. On the other hand, the operating temperature of computer chips and 5G optical communication modules is between 60 and 110°C, which makes their demand for refrigeration also develop towards higher temperatures. Therefore, the development and application of thermoelectric materials and thermoelectric components in the near-room temperature region (<300°C) in power generation and refrigeration has become very important.
[0004] In recent years, with the continuous discovery of new thermoelectric materials and the development of device construction technology, the performance of thermoelectric materials and thermoelectric components has been gradually improved. At present, thermoelectric components can be commercialized to a certain extent, among which bismuth telluride-based thermoelectric devices have outstanding advantages. However, since bismuth telluride materials contain some scarce and toxic elements, the preparation cost is high, and the power generation efficiency is low within 300°C, which greatly limits the further large-scale use of this material in thermoelectric devices. Therefore, the development of new thermoelectric materials with excellent performance and the construction of corresponding high-performance thermoelectric devices are the needs of the development of the entire thermoelectric field, and are also the core issue of breaking through the current performance bottleneck of thermoelectric devices.
[0005] Since their discovery, magnesium-silver-antimony alloys and magnesium-bismuth-antimony alloys have become research hotspots in the field of thermoelectric materials. After in-depth research by scientific researchers, the thermoelectric figure of merit of n-type magnesium-bismuth-antimony-based thermoelectric materials has been greatly improved through various means, and the room temperature thermoelectric figure of merit has been able to reach 0.9. However, compared with n-type magnesium-bismuth-antimony-based thermoelectric materials, p-type magnesium-silver-antimony thermoelectric materials have not made any breakthroughs since the room temperature thermoelectric figure of merit of 0.9 and the peak value of 1.4 were reported in 2014. In addition, there are still few reports on all-magnesium-based thermoelectric components constructed by magnesium-silver-antimony and magnesium-bismuth-antimony alloys.
[0006] Currently, thermoelectric devices widely used in automotive air-conditioning seats, environmentally friendly refrigerators, high-power chips, etc. still use traditional bismuth telluride-based thermoelectric materials. However, compared with magnesium-silver-antimony and magnesium-bismuth-antimony-based thermoelectric materials, bismuth telluride-based thermoelectric materials are too expensive, and the prices of raw materials such as tellurium and bismuth are much higher than those of raw materials such as magnesium-silver-antimony. Before the discovery of high-performance magnesium-based thermoelectric materials, bismuth telluride-based thermoelectric materials were an irreplaceable choice for the application of thermoelectric refrigeration and power generation devices. With continuous research, the performance of magnesium-based thermoelectric materials is also gradually improving. In the room temperature range, the performance is comparable to that of bismuth telluride-based thermoelectric materials, and in the high temperature range, it surpasses bismuth telluride, which provides a basis and possibility for the application of magnesium-based thermoelectric materials in thermoelectric power generation and refrigeration devices.
[0007] However, to turn new thermoelectric materials into devices, good thermoelectric performance alone is far from enough. Thermoelectric materials also need to be constructed into thermoelectric components with excellent performance before they can be further assembled into thermoelectric power generation and refrigeration systems. So far, all-magnesium-based thermoelectric components constructed from magnesium-silver-antimony and magnesium-bismuth-antimony-based thermoelectric materials have far from adequate power generation and refrigeration performance. This is mainly because the p-type magnesium-silver-antimony-based thermoelectric materials prepared have low performance, which affects the commercial application of all-magnesium-based thermoelectric devices.
[0008] The inventor of the present application previously disclosed a thermoelectric material in US Pat. No. 20160326615A1, which is prepared by processing raw material powders by ball milling and hot pressing to prepare a thermoelectric material including MgAgSb, MgAg 0.97 Sb 0.99 As well as materials that replace Mg, Ag and Sb with other elements, in order to obtain thermoelectric merit zT suitable for thermoelectric applications. According to the patent, some impurity phase peaks were found in the XRD spectrum of MgAgSb, and phase analysis identified that they may be Sb and Ag-Sb related impurity phases. Therefore, in order to eliminate impurities and obtain pure phase samples, according to the chemical formula MgAg 0.97 Sb 0.99 By removing some Ag and Sb, the pure phase sample MgAg was obtained. 0.97 Sb 0.99 , and then Mg, Ag and Sb were further substituted based on this composition.
[0009] According to the records of US20160326615A1, the material is prepared according to the disclosed method, and the thermoelectric figure of merit zT of the material with the stoichiometric composition of MgAgSb at 300K is about 0.5; MgAg 0.97 Sb 0.99The zT value of the composition reaches about 0.7 at 300K and about 1.2 at 450K. The grain size in the SEM image is less than 200nm, and the crystallite size in the TEM image is 10-20nm, showing a mosaic microstructure. 0.97 Sb 0.99 All materials showed an improvement in thermoelectric figure of merit, among which nickel-doped MgAg 0.965 Ni 0.005 Sb 0.99 It has the highest zT value, achieving a zT of about 1 at 325K and a peak zT of about 1.4 at 450K.
[0010] On the basis of the above work, the inventors of the present application have been committed to further improving the performance of MgAgSb-based thermoelectric materials for near-room temperature refrigeration and power generation applications for many years. Summary of the invention
[0011] The purpose of the present invention is to further improve the performance of MgAgSb thermoelectric materials by principle calculation, adjustment of preparation process and material composition, so as to save material costs, improve economic benefits and promote the commercial application of thermoelectric components prepared from magnesium-silver-antimony and magnesium-bismuth-antimony based thermoelectric materials.
[0012] Based on the previous research results, the inventors have studied MgAgSb and MgAg 0.97 Sb 0.99 The formation energy of two compositions of magnesium-silver-antimony-based thermoelectric materials was calculated by first principles. The calculation process includes: (1) using the finite displacement method to calculate the dynamic matrix, thereby completing the phonon spectrum calculation, and the supercell size used is 2×2×1; (2) using the virtual crystal approximation to construct the atomic vacancies in the system, and using the AkaiKKR software package to complete the formation energy calculation. Among them, the software uses the Green's function method to solve the Kohn-Sham equation; the calculation uses the scalar mode to solve the Dirac equation to obtain the core state and valence state of the electron; the exchange potential is simulated by the MJW (Moruzzi, Janak and Williams) method; the experimentally measured lattice parameters are used to calculate the formation energy, and the atomic positions are obtained according to the symmetry.
[0013] The above first-principles calculations show that the phonon spectrum of α-MgAgSb has a small amount of imaginary frequency, indicating that its structural dynamics energy is higher, while MgAg 0.97 Sb 0.99 The system has no imaginary frequency, indicating that the formation of Ag and Sb vacancies enhances the stability of the system. Fig.18 and Fig.19 . Fig. 20 The formation energy calculations shown show that MgAgSb material is stronger than MgAg 0.97 Sb0.99 The formation energy of the material is 228Ry higher, which further indicates that MgAgSb material is less likely to form a pure alloy phase from the perspective of structural dynamics.
[0014] A first aspect of the present invention provides a method for preparing a MgAgSb thermoelectric material, the method comprising:
[0015] (1) placing raw materials in a stoichiometric ratio according to the chemical formula MgAg into a ball mill, and using a synchronous transmission high-energy ball mill to obtain uniform powder;
[0016] (2) adding Sb according to the chemical formula MgAgSb to the powder obtained in step (1), and continuing to use a synchronous transmission high-energy ball mill to obtain a mixture powder;
[0017] (3) sintering the mixture powder obtained in step (2) into a bulk material;
[0018] (4) Annealing the bulk material obtained in step (3) at a temperature of 310±2°C for 12 to 30 hours.
[0019] The inventors of the present invention have found through a large number of experimental studies that, compared with the traditional belt-driven ball milling method, the operation of the synchronous drive high-energy ball mill described in steps (1) and (2) is more stable and efficient, which is conducive to the formation of the pure alloy phase of MgAgSb; combined with the annealing treatment at the critical phase transition temperature of 310±2°C in step (4), a pure phase MgAgSb material with larger grains and fewer defects is obtained. Based on the above findings, the present invention has achieved a major breakthrough in the performance of p-type magnesium-silver-antimony-based thermoelectric materials: since 2014, when it was reported that the room temperature thermoelectric figure of merit of p-type magnesium-silver-antimony thermoelectric materials reached 0.9 and the peak value after doping reached 1.4, there has been no breakthrough so far; however, the present invention has obtained a pure phase MgAgSb material that has not been obtained in previous studies by adopting the above-mentioned preparation process, and its carrier mobility in the undoped state can reach 93.3cm 2 V -1 s -1 , the power factor can reach 25μW cm -1 K -2 The room temperature thermoelectric figure of merit zT is 0.97, and zT reaches 1.6 at 250℃ (the traditionally reported room temperature zT of laboratory spark plasma sintered samples is 0.7, and zT is 1.2 at 250℃).
[0020] According to a preferred embodiment of the present invention, cemented carbide balls are used in the ball milling process described in steps (1) and (2). The inventors have found that for MgAgSb materials, compared with the use of traditional stainless steel balls, the use of cemented carbide balls made of materials such as tungsten steel for ball milling can further improve the thermoelectric properties of the material. It is believed that this may be because the use of a synchronous transmission high-energy ball mill and cemented carbide balls improves the ball milling energy and ball milling stability while avoiding cold welding of the material on the wall of the ball mill during the high-energy mechanical alloying process.
[0021] According to the preparation method provided by the present invention, the time of ball milling in steps (1) and (2) can be independently 8 to 12 hours.
[0022] In a preferred embodiment, the mass of the cemented carbide ball is 2 to 30 grams, preferably 8 to 15 grams; the radius of the cemented carbide ball can be 2 to 20 mm, preferably 8 to 15 mm.
[0023] According to the preparation method provided by the present invention, the sintering conditions in step (3) may include: heating to 275-290° C. at a rate of 20-80° C. / min under a pressure of 10-100 MPa, and keeping the temperature for 1-30 min.
[0024] According to a preferred embodiment of the present invention, the annealing process in step (4) may include: heating the bulk material to a temperature of 310±2°C at a rate of 2-10°C / min, keeping the temperature at this temperature for 20-25 hours, and then cooling to room temperature.
[0025] The inventors found that in the conventional annealing process for preparing MgAgSb-based materials, the furnace temperature is only set to about 300°C, and the temperature of the material itself is not monitored or considered, which may be an important reason for the failure to obtain pure phase MgAgSb material and the small grain size of the material. Therefore, the present invention creatively uses a thermocouple in contact with the material to monitor the temperature of the material, and controls the heat supply in the furnace according to the monitored temperature, so that the temperature of the bulk material is maintained at 310±2°C during the annealing process.
[0026] A second aspect of the present invention provides a magnesium-silver-antimony-based thermoelectric material, which is a MgAgSb thermoelectric material prepared by the above-mentioned preparation method, wherein the magnesium-silver-antimony-based thermoelectric material is a pure-phase MgAgSb material.
[0027] According to the magnesium-silver-antimony-based thermoelectric material provided by the present invention, the thermoelectric figure of merit zT of the pure phase MgAgSb material is 0.97-1.6 at 25° C.-250° C.
[0028] According to the magnesium-silver-antimony-based thermoelectric material provided by the present invention, the carrier mobility of the pure phase MgAgSb material is about 93.3 cm 2 V -1 s -1 .
[0029] Preferably, the power factor of the pure phase MgAgSb material is about 25 μW cm -1 K -2 .
[0030] The third aspect of the present invention provides the use of the MgAgSb thermoelectric material or the MgAgSb thermoelectric material prepared according to the method of the present invention in thermoelectric components for thermoelectric power generation and refrigerators.
[0031] According to the application provided by the present invention, the thermoelectric component is preferably a fully magnesium-based thermoelectric component, which includes a p-type magnesium-silver-antimony thermoelectric material and an n-type magnesium-bismuth-antimony-based thermoelectric material, wherein the p-type magnesium-silver-antimony thermoelectric material is the magnesium-silver-antimony-based thermoelectric material provided by the present invention or the magnesium-silver-antimony-based thermoelectric material prepared according to the preparation method of the present invention.
[0032] The thermoelectric component composed of a p-type magnesium silver antimony thermoelectric material and an n-type magnesium bismuth antimony-based thermoelectric material prepared by the present invention can achieve the cooling performance of existing bismuth telluride-based thermoelectric components, far surpassing the power generation performance of existing bismuth telluride-based thermoelectric components, while achieving a significant reduction in cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] The embodiments of the present invention are described in detail below with reference to the accompanying drawings, wherein:
[0034] Figure 1 This is a grain size diagram of the MgAgSb material obtained in step (3) of Example 1 of the present invention before annealing.
[0035] Figure 2 This is a grain size diagram of the MgAgSb material after annealing in step (4) of Example 1 of the present invention.
[0036] Figure 3 The following are comparison photos of the Hi-Energy / Mill 8000D synchronous drive high energy ball mill (a) used in Example 1 of the present invention and the SPEX 8000D Mixer / Mill belt drive ball mill (b) used in Comparative Example 1.
[0037] Figure 4 It is an X-ray diffraction (XRD) comparison chart of the MgAgSb mixture powder prepared in step (2) of Example 1 of the present invention and the MgAgSb mixture powder prepared in Comparative Example 1 and the MgAgSb standard peak.
[0038] Figure 5 It is a comparison chart of the yield of MgAgSb mixture powder prepared by using a synchronous drive high energy ball mill in Example 1 of the present invention and the yield of MgAgSb mixture powder prepared by using a belt drive ball mill in Comparative Example 1.
[0039] Figure 6 The MgAg prepared in Comparative Example 2 0.97 Sb 0.99 Comparison of carrier concentration and mobility of the material and the MgAgSb material prepared in Example 1 before and after annealing.
[0040] Figure 7 The MgAg prepared in Comparative Example 2 0.97 Sb 0.99 The conductivity comparison diagram of the material and the MgAgSb material prepared in Example 1 before and after annealing.
[0041] Figure 8 The MgAg prepared in Comparative Example 2 0.97 Sb 0.99 The relationship between the lower Seebeck coefficient and temperature of the MgAgSb material prepared in the material and Example 1 before and after annealing.
[0042] Fig. 9 The MgAg prepared in Comparative Example 2 0.97 Sb 0.99 A comparison of the thermal conductivity and lattice thermal conductivity of the material and the MgAgSb material prepared in Example 1 before and after annealing as a function of temperature.
[0043] Fig.10 The MgAg prepared in Comparative Example 2 0.97 Sb 0.99 Comparison of the change of the thermoelectric figure of merit zT of the material and the MgAgSb material prepared in Example 1 with temperature before and after annealing.
[0044] Fig.11 The figure is a comparison chart of the thermoelectric figure of merit zT of the MgAgSb material of the present invention and two MgAgSb samples reported in the literature as a function of temperature.
[0045] Fig.12 This is a comparison chart of the conductivity and Seebeck coefficient of the MgAgSb material in Comparative Example 3 after annealing at different temperatures.
[0046] Fig.13 This is a comparison chart of the power factors of the MgAgSb material in Comparative Example 3 after annealing at different temperatures.
[0047] Fig.14 This is a graph showing the change in thermoelectric power generation efficiency of the all-magnesium-based device prepared in Example 2 of the present invention as a function of the hot end temperature.
[0048] Fig.15 This is a graph showing how the thermoelectric power generation efficiency of existing all-magnesium-based devices varies with the hot-end temperature as reported in the literature.
[0049] Fig.16 This is a graph showing the change in cooling temperature difference of the all-magnesium-based device as a function of the hot-end temperature of the all-magnesium-based device prepared in Example 2 of the present invention.
[0050] Fig.17 This is a graph of the cooling temperature difference of existing all-magnesium-based devices reported in the literature as a function of the hot-end temperature.
[0051] Fig.18 MgAg prepared in Comparative Example 2 obtained by first principle calculation 0.97 Sb 0.99 Phonon spectrum of a material.
[0052] Fig.19 The phonon spectrum of the MgAgSb material prepared in Example 1 obtained by first-principles calculation.
[0053] Fig. 20 MgAg prepared in Comparative Example 2 obtained by first principle calculation 0.97 Sb 0.99 The material forms an energy comparison diagram with the MgAgSb material prepared in Example 1. DETAILED DESCRIPTION
[0054] The present invention is further described in detail below in conjunction with specific embodiments. The given examples are only for illustrating the present invention, but not for limiting the scope of the present invention.
[0055] Example 1
[0056] Preparation of MgAgSb thermoelectric material of the present invention
[0057] (1) Mg chips and Ag blocks were weighed in a glove box according to the chemical formula MgAg, with a total weight of 5.2 g, and placed in a stainless steel ball mill containing two carbide balls (each with a mass of 10 g and a radius of 10.5 mm). The Mg chips and Ag blocks were then placed in a high-energy ball mill (model: Hi-Energy / Mill 8000D, transmission mode: synchronous transmission, working mode: three-position ∞-type swing vibration, rotation speed: 875 times / min) and ball milled for 10 h to obtain MgAg alloy powder.
[0058] (2) According to the chemical formula MgAgSb, Sb blocks were added to the MgAg alloy powder obtained in step (1), and the mixture was milled for 10 h to obtain a mixed powder.
[0059] (3) The mixed powder and the electrode material Ag powder were placed in batches into a graphite mold with a diameter of 12.7 mm and flattened layer by layer to form a sandwich-shaped Ag / MgAgSb / Ag structure, which was then sintered into a cylindrical block material by spark plasma sintering. The sintering process was as follows: heating to 285°C at a rate of 50°C / min, keeping the temperature for 5 minutes, and the pressure during the sintering process was 80 MPa. After sintering, a block material with a thickness of 3 mm and a diameter of 12.7 mm was obtained, of which the thickness of the electrode layer was 0.1 mm.
[0060] (4) The obtained sample is loaded into a quartz tube, evacuated to 0.5 Pa, melted and sealed under a high-temperature flame gun, and then the quartz tube containing the sample is placed in a muffle furnace and heated at a rate of 5°C / min until the temperature of the bulk material reaches 310°C, and maintained at this temperature for 24 hours, and then cooled to room temperature with the furnace.
[0061] In order to characterize the effect of annealing process on grain size, electron backscattered diffraction (EBSD) analysis was carried out on the MgAgSb materials before and after annealing. Figure 1 This is a grain size diagram of the MgAgSb material obtained in step (3) before annealing, and the figure shows that the average grain size is about 200nm. Figure 2 The figure is a grain size diagram of the MgAgSb material after annealing in step (4), which shows that the average grain size is about 2 μm. Figure 1 and Figure 2 It can be seen from the comparison that the annealing process of the present invention makes the MgAgSb grains with a size of about 200nm grow into large grains with a size of about 2μm. Thanks to the reduction of the influence of the grain boundary, its thermal conductivity will be reduced, as shown in the carrier mobility test below, and its carrier mobility will also be greatly increased.
[0062] Comparative Example 1
[0063] In this comparative example, MgAgSb mixture powder was prepared in a manner similar to steps (1) and (2) of Example 1, except that a conventional SPEX 8000D Mixer / Mill belt-driven ball mill and conventional stainless steel balls were used for ball milling.
[0064] Table 1 shows the parameter comparison of the ball milling technology used in Example 1 of the present invention and the ball milling technology used in Comparative Example 1.
[0065] Table 1
[0066] parameter Example 1 Comparative Example 1 Transmission mode Synchronous transmission Belt drive Engine speed 1425RPM 1425RPM Belt speed 875RPM 875RPM Voltage 230V / 50Hz 230V / 50Hz Ball material Carbide ball Steel ball Diameter of the ball 10.5mm 12.6mm The mass of each ball 10g 8g
[0067] Figure 3The following are comparison photos of the Hi-Energy / Mill 8000D synchronous transmission high energy ball mill (a) used in Example 1 of the present invention and the SPEX 8000D Mixer / Mill belt transmission ball mill (b) used in Comparative Example 1. It can be seen from the photos of the two transmission modes that the belt transmission mode is prone to problems such as belt loosening and poor contact during operation, resulting in speed reduction. The synchronous transmission mode solves this problem well, ensuring that the ball mill can maintain a stable speed during long-term operation.
[0068] Figure 4 1 is an X-ray diffraction (XRD) comparison chart of the MgAgSb mixture powder obtained in step (2) of Example 1 and the MgAgSb mixture powder obtained in Comparative Example 1 and the MgAgSb standard peak. Figure 4 It can be seen that within the same 10-hour ball milling time, the XRD of the MgAgSb mixture powder obtained in step (2) of Example 1 is very close to the standard peak, and there is almost no impurity. However, the XRD of the MgAgSb mixture powder obtained in Comparative Example 1 contains many impurity peaks that do not belong to MgAgSb, indicating that the purity of the prepared material is low.
[0069] Figure 5 1 is a comparison chart of the yield of MgAgSb mixture powder prepared by synchronous transmission high energy ball mill in Example 1 and MgAgSb mixture powder prepared by belt transmission ball mill in Comparative Example 1. Figure 5 It can be seen that the yield of MgAgSb mixture powder prepared by synchronous drive high energy ball mill is much higher than that by belt drive ball mill.
[0070] Comparative Example 2
[0071] This comparative example adopts the same method as Example 1 to prepare MgAg 0.97 Sb 0.99 The thermoelectric material is used to compare the performance with the MgAgSb thermoelectric material prepared in Example 1.
[0072] Comparative Example 3
[0073] In this comparative example, MgAgSb mixture powder was prepared in a manner similar to that of Example 1, except that in step (4), no annealing, annealing at 250°C for 24 hours and annealing at 300°C for 24 hours were used instead of annealing at 310°C for 24 hours in Example 1.
[0074] Performance Testing
[0075] 1. Carrier concentration and mobility test: PPMS is used to test the Hall coefficient of the sample under the condition of reversible magnetic field (±2T). The carrier concentration and Hall mobility are respectively calculated by formula n H =1 / eR H and μ H =σ / (en H ) calculated. Figure 6 The MgAg prepared in Comparative Example 2 0.97 Sb 0.99 The MgAgSb material prepared in Example 1 and the comparison of carrier concentration and mobility before and after annealing are shown in FIG. Figure 6 It can be seen that the MgAgSb material prepared in Example 1 is better than the MgAg prepared in Comparative Example 2. 0.97 Sb 0.99 The material fills the vacancy defects inside, and the mobility increases from 67.8cm 2 V -1 s -1 Increased to 80.8cm 2 V -1 s -1 By further annealing to grow the grains, the mobility of the MgAgSb material prepared in Example 1 was increased to 93.3 cm 2 V -1 s -1 .
[0076] 2. Conductivity test: The samples were cut into rectangular blocks with a size of 2 mm × 3 mm × 11 mm, and the conductivity and Seebeck coefficient of the samples were tested using a Linseis LSR-3 instrument. Figure 7 The MgAg prepared in Comparative Example 2 0.97 Sb 0.99 The material is compared with the MgAgSb material prepared in Example 1 and its conductivity before and after annealing. Figure 7 As can be seen from the figure, due to the increase in mobility, the room temperature conductivity of the material increases from MgAg prepared in Comparative Example 2 to 0.97 Sb 0.99 290Scm of material -1 Increased to 356Scm -1 By further annealing to grow the grains, the room temperature conductivity of the MgAgSb material prepared in Example 1 increased to 452 Scm -1 .
[0077] Figure 8 The MgAg prepared in Comparative Example 2 0.97 Sb 0.99 The relationship between the Seebeck coefficient and temperature of the MgAgSb material prepared in Example 1 before and after annealing. Figure 8 It can be seen that the MgAg prepared in Comparative Example 2 0.97 Sb 0.99 The material is similar to the MgAgSb material prepared in Example 1 and its Seebeck coefficient before and after annealing has no significant change, which further proves that the improvement of mobility leads to the improvement of the electrical properties of the MgAgSb material.
[0078] 3. Changes of thermal conductivity and lattice thermal conductivity with temperature: The thermal diffusion coefficient D of the sample was tested using Linseis LFA 1000 laser thermal conductivity, the density ρ of the sample was measured using the Archimedean drainage method, and the heat capacity C of the sample was tested using a DSC 404 high temperature differential scanning calorimeter. p , then through the formula κ=DρC p The thermal conductivity of the material is calculated. The electronic thermal conductivity of the material is obtained by using the Wiedemann-Franz law through the electrical conductivity, and then the formula κ L =κ-κ e The lattice thermal conductivity of the sample was calculated.
[0079] Fig. 9 The MgAg prepared in Comparative Example 2 0.97 Sb 0.99 A comparison of the thermal conductivity and lattice thermal conductivity of the material and the MgAgSb material prepared in Example 1 before and after annealing as a function of temperature.
[0080] 4. Changes of thermoelectric figure of merit zT with temperature: According to the electrical conductivity, Seebeck coefficient and thermal conductivity of the sample obtained in the previous test, the formula zT = S 2 The thermoelectric figure of merit zT of the sample is calculated by σT / κ. Fig.10 The MgAg prepared in Comparative Example 2 0.97 Sb 0.99 The comparison of the thermoelectric figure of merit zT of the MgAgSb material prepared in Example 1 before and after annealing with the temperature. Fig.10 It can be seen that the thermoelectric figure of merit zT of the sample increased from 0.72 at room temperature and a maximum of 1.2 for MgAg0.97Sb0.99 to 0.97 at room temperature and a maximum of 1.6 for MgAgSb after annealing, an overall increase of 30%.
[0081] Fig.11 The figure is a comparison of the thermoelectric figure of merit zT of the MgAgSb material of the present invention and two MgAgSb samples reported in the literature with the change of temperature.
[0082] ref[1]: Zhao, H., et al., High thermoelectric performance of MgAgSb-basedmaterials. Nano Energy, 2014.7: p.97-103;
[0083] ref[2]: Kirkham, MJ, et al., Abinitiodetermination of crystalstructures of the thermoelectric material MgAgSb. Physical Review B, 2012.85(14).
[0084] from Fig.11 It can be seen that the thermoelectric figure of merit zT of the MgAgSb sample of the present invention is much higher than that of the two MgAgSb samples reported in the literature in the entire test temperature range, which reflects the superiority of the material of the present invention in terms of performance.
[0085] 5. Fig.12 This is a comparison chart of the conductivity and Seebeck coefficient of the MgAgSb material in Comparative Example 3 after annealing at different temperatures. Fig.13 This is a comparison chart of the power factors of the MgAgSb material after annealing at different temperatures in Comparative Example 3. It can be seen from the figure that the room temperature conductivity of the MgAgSb material after annealing at 250℃ and 300℃ for 1 day has no obvious change, while the room temperature conductivity after annealing at 310℃ for 1 day has been significantly improved, and the Seebeck coefficient has not changed significantly, which ultimately improves the power factor of the sample. The advantage of annealing at 310℃ is confirmed.
[0086] Example 2
[0087] Preparation of thermoelectric devices
[0088] The MgAgSb material prepared in Example 1 was cut into small pieces with a size of 1.3 mm*1.3 mm*3 mm, namely, magnesium silver antimony-based thermoelectric elements. The elements were assembled with n-type magnesium bismuth antimony-based thermoelectric elements with a size of 1.3 mm*1.3 mm*3 mm through a soldering process to prepare 7 pairs of thermoelectric devices.
[0089] The power generation and cooling performance of the thermoelectric device were tested using Mini-PEM. The device achieved a thermoelectric power generation efficiency of 12% at a temperature difference of 300K near room temperature, which is much higher than that of bismuth telluride-based power generation devices. At the same time, its room temperature cooling temperature difference reached 61K, which is comparable to that of bismuth telluride-based cooling devices.
[0090] Fig.14This is a graph showing the thermoelectric power generation efficiency of the all-magnesium-based device prepared in this embodiment as a function of the hot end temperature. Fig.15 The figure shows the change of thermoelectric power generation efficiency of existing all-magnesium-based devices with the hot end temperature, as reported in ref[3]: P. Ying et al., Robust thermoelectric module based on MgAgSb / Mg3(Sb,Bi)2 with an 8.5% conversion efficiency and a 72K maximum cooling. Energy Environ. Sci, 2022.15: p.2557-2566. Fig.14 and Fig.15 By comparison, it can be seen that the thermoelectric power generation efficiency of the all-magnesium-based device prepared in this embodiment can reach 12% at a temperature difference of 300K, which is much higher than the thermoelectric power generation efficiency of the existing all-magnesium-based devices that have been reported.
[0091] Fig.16 This is a graph showing the change in cooling temperature difference of the all-magnesium-based device prepared in this embodiment as a function of the hot-end temperature. Fig.17 The figure below shows the temperature difference of the existing all-Mg-based device compared with the hot-end temperature reported in ref[3]. Fig.16 and Fig.17 By comparison, it can be seen that the room temperature cooling temperature difference of the all-magnesium-based device prepared in this embodiment can reach 62K, which is higher than the room temperature cooling temperature difference of 52K of the existing all-magnesium-based device reported.
Claims
1. A method for preparing a MgAgSb thermoelectric material, the preparation method comprising: (1) placing raw materials in a stoichiometric ratio according to the chemical formula MgAg into a ball mill, and using a synchronous transmission high-energy ball mill to obtain uniform powder; (2) adding Sb according to the chemical formula MgAgSb to the powder obtained in step (1), and continuing to use the synchronous transmission high-energy ball mill to obtain a mixture powder; (3) sintering the mixture powder obtained in step (2) into a bulk material; (4) Annealing the bulk material obtained in step (3) at a temperature of 310±2°C for 12 to 30 hours.
2. The preparation method according to claim 1, wherein In the ball milling process described in steps (1) and (2), a hard alloy ball is used for ball milling, for example, a tungsten steel ball is used for ball milling; Preferably, the mass of the cemented carbide ball is 2 to 30 grams, preferably 8 to 15 grams; the radius of the cemented carbide ball is 2 to 20 mm, preferably 8 to 15 mm.
3. The preparation method according to claim 1 or 2, wherein The ball milling time in steps (1) and (2) is independently 8 to 12 hours.
4. The preparation method according to any one of claims 1 to 3, wherein The sintering conditions in step (3) include: heating to 275-290° C. at a rate of 20-80° C. / min under a pressure of 10-100 MPa, and keeping the temperature for 1-30 min, preferably 2-10 min.
5. The preparation method according to any one of claims 1 to 4, wherein The annealing process in step (4) includes: heating the bulk material to a temperature of 310±2°C at a rate of 2-10°C / min, keeping the temperature at this temperature for 20-25 hours, and then cooling to room temperature.
6. The MgAgSb thermoelectric material prepared by the preparation method according to any one of claims 1 to 5, wherein: The MgAgSb thermoelectric material is a pure phase MgAgSb material.
7. The MgAgSb thermoelectric material according to claim 6, wherein: At 25° C. to 300° C., the thermoelectric figure of merit zT of the pure phase MgAgSb material is 0.97 to 1.
6.
8. The MgAgSb thermoelectric material according to claim 6 or 7, wherein: The carrier mobility of the pure phase MgAgSb material is about 93.3 cm 2 V -1 s -1 ; Preferably, the power factor of the pure phase MgAgSb material is about 25 μW cm -1 K -2 .
9. Use of the MgAgSb thermoelectric material according to any one of claims 6 to 8 or the MgAgSb thermoelectric material prepared by the preparation method according to any one of claims 1 to 5 in thermoelectric components for thermoelectric power generation and refrigerators.
10. The use according to claim 9, wherein: The thermoelectric component is a fully magnesium-based thermoelectric component, which includes a p-type magnesium-silver-antimony thermoelectric material and an n-type magnesium-bismuth-antimony-based thermoelectric material, wherein the p-type magnesium-silver-antimony thermoelectric material is the MgAgSb thermoelectric material described in any one of claims 6 to 8 or the MgAgSb thermoelectric material prepared according to the preparation method described in any one of claims 1 to 5.
Citation Information
Cited By
P-type alpha-MgAgSb-based thermoelectric material and preparation method thereof
CN122773158A