Method and device for inhibiting air holes in aluminum alloy manufactured through electric arc additive manufacturing

By using a dual cooling solution that circulates coolant and a liquid nitrogen environment inside the substrate during the arc additive manufacturing of aluminum alloys, the problem of aluminum alloy pores is solved, the cooling rate and manufacturing efficiency are improved, and the mechanical properties and manufacturing of aluminum alloy components are improved. quality.

CN118808833APending Publication Date: 2024-10-22NORTHWESTERN POLYTECHNICAL UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410894231.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-04
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

Porosity problems often exist during arc additive manufacturing of aluminum alloys, which are difficult to effectively control with existing technology, affecting the mechanical properties and manufacturing efficiency of formed parts.

Method used

The cooling liquid is circulated inside the substrate and placed in a liquid nitrogen environment. At the same time, liquid nitrogen is sprayed after each layer is deposited for double cooling, which increases the cooling rate and shortens the overflow distance of the pores.

Benefits of technology

It significantly reduces the generation and elimination time of pores, improves the quality of aluminum alloy arc additive manufacturing and the reliability of components, and reduces production costs and complexity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118808833A_ABST
    Figure CN118808833A_ABST
Patent Text Reader

Abstract

The invention discloses a method and a device for inhibiting air holes in an aluminum alloy manufactured through electric arc additive manufacturing, and belongs to the technical field of additive manufacturing. According to the method, in order to solve the problems that electric arc additive manufacturing heat input is large, and air holes are easily formed in aluminum alloy, in the electric arc additive manufacturing aluminum alloy process, on one hand, cooling liquid is continuously introduced into a base plate, a deposition piece is continuously cooled through the base plate, and on the other hand, the base plate is in a liquid nitrogen environment; the molten pool forming process in the electric arc additive manufacturing process is in the liquid nitrogen environment, and further, the upper surface of a deposition layer is cooled again every time a layer is deposited, so that the upper surface of the molten pool can be rapidly cooled. According to the method, an in-situ double cooling scheme of substrate inner cooling and outer surface cooling is introduced, and the common air hole problem in the WAAM forming aluminum alloy component is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of additive manufacturing, and in particular relates to a method and a device for suppressing pores in aluminum alloys manufactured by arc additive manufacturing. Background Art

[0002] Wire+Arc Additive Manufacturing (WAAM) is an additive manufacturing technology that uses electric arc as a heat source and welding wire as an additive material. It has the characteristics of being able to directly form large-sized structural parts, high deposition efficiency, and high material utilization. It is widely used in aerospace, automobile manufacturing, medical equipment and other fields. In particular, WAAM can avoid the poor formability of aluminum alloys due to high laser reflectivity and high forming stress, and has become an important direction for aluminum alloy additive manufacturing. However, the porosity problem of WAMM forming aluminum alloys has always been a common and severe challenge. These pores damage the mechanical properties of the formed parts, greatly limiting the widespread use of this technology.

[0003] At present, the main methods for controlling porosity defects in WAAM aluminum alloys are: optimizing process parameters (arc mode, current, scanning rate, etc.), multi-energy field assistance (laser-arc composite, ultrasonic field and electromagnetic field assistance, etc.) and post-processing (interlayer rolling and laser shock, etc.). However, optimizing process parameters is a complex and time-consuming process, and is extremely sensitive to different arc additive manufacturing methods (tungsten inert gas shielded arc additive manufacturing, cold metal transition arc additive manufacturing technology, etc.) and material properties, and cannot guarantee the stability and repeatability of the forming process; multi-energy field assistance and post-processing will increase process complexity and production costs, and have great limitations in the manufacture of complex shapes and large-sized components. Summary of the invention

[0004] The purpose of the present invention is to overcome the shortcomings of the above-mentioned prior art and provide a method and device for suppressing pores in aluminum alloy produced by arc additive manufacturing. This method solves the problem of easy generation of pores and the lack of suitable control measures at this stage when aluminum alloy is manufactured by arc additive manufacturing technology.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions:

[0006] A method for suppressing pores in arc additive manufacturing of aluminum alloy, wherein during the arc additive manufacturing of aluminum alloy, a coolant flows inside a substrate and the substrate is in a liquid nitrogen environment;

[0007] The arc additive deposits one layer and sprays liquid nitrogen on the surface of the deposited layer.

[0008] A further improvement of the present invention is:

[0009] Preferably, the cooling liquid flowing inside the substrate covers the entire substrate area.

[0010] Preferably, each spraying time is greater than a threshold value, and the threshold value is determined by the single-layer deposition length, the single-layer deposition spraying time and the total deposition length.

[0011] Preferably, during the spraying process, the liquid nitrogen gun moves on the surface of the deposited layer.

[0012] A device for suppressing pores in aluminum alloy produced by arc additive manufacturing for implementing the above method, comprising a substrate, a cooling liquid channel arranged in the substrate, the substrate being located in a cavity with an upper opening, and a baffle being arranged at the edge of the cavity;

[0013] An arc additive manufacturing welding gun and a liquid nitrogen spraying gun are arranged above the cavity.

[0014] Preferably, the horizontal cross-sectional area of ​​the substrate is 5-10 times the projection area of ​​the bottom of the deposited sample.

[0015] Preferably, the cooling liquid channel covers the entire substrate.

[0016] Preferably, the height of the baffle is 50-100 mm; and sealing materials are provided between adjacent baffles and between the baffles and the substrate.

[0017] Preferably, the coolant introduced into the coolant channel is water.

[0018] Preferably, the substrate is an aluminum alloy substrate.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] The invention discloses a method for suppressing pores in arc additive manufacturing of aluminum alloy. The method introduces an in-situ double cooling scheme of substrate internal cooling and external surface cooling to solve the common pore problem in WAAM formed aluminum alloy components. In the process of arc additive manufacturing of aluminum alloy, on the one hand, coolant is continuously introduced into the substrate to continuously cool the deposited part through the substrate, and on the other hand, the substrate is in a liquid nitrogen environment, so that the molten pool formation process in the arc additive manufacturing process is in a liquid nitrogen environment. Further, each layer is deposited, and the upper surface of the deposited layer is cooled again, so that the upper surface of the molten pool can also be quickly cooled. The method reduces the size of the molten pool in the arc additive manufacturing process by more than 40% by increasing the cooling rate (reduced by more than 10%), thereby shortening the distance of pore overflow, so that the pores generated in the additive manufacturing process can be quickly discharged. The method fundamentally solves the problem that arc additive manufacturing is easy to generate pores when manufacturing aluminum alloys. Through double cooling, the cooling speed of the molten pool is fast, the generation of pores is reduced and their removal is promoted. Compared with traditional methods, this scheme is more universal, simple and effective. It can be widely applied to the arc additive manufacturing process of various aluminum alloys, with high universality and broad application prospects; the in-situ double cooling operation is simpler and more effective, easy to implement, and reduces time and economic costs while improving the pore suppression effect; this in-situ double cooling scheme can reduce heat accumulation in the forming process while reducing pores, and optimize the problem of coarse structure caused by heat accumulation during arc forming.

[0021] Further, a layer is deposited and a layer of liquid nitrogen is sprayed, so that the liquid nitrogen can be stored in large quantities around the substrate.

[0022] Furthermore, during the liquid nitrogen spraying process, the liquid nitrogen gun can move on the surface of the deposition layer, so that each deposition layer can be fully cooled.

[0023] The present invention also discloses a device for suppressing pores in arc additive manufacturing of aluminum alloy. The device is provided with a cooling channel inside and a baffle to form a cavity, so that a substrate can be placed in the cavity, and the cavity can provide a liquid nitrogen environment for the substrate; the cavity is under the welding gun and the spray gun, which facilitates the alternating operation of arc additive manufacturing deposition and spraying of liquid nitrogen. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 A schematic diagram of the in-situ dual cooling optimization scheme of the present invention;

[0025] Among them, (a) shows the single-layer forming process; (b) shows the liquid nitrogen cooling process after single-layer forming;

[0026] Figure 2 It is a finite element model (conventional cooling method);

[0027] Figure 3 is the thermal history of the center of the bottom of the substrate (conventional cooling method);

[0028] Figure 4 is the temperature field of the component under different forming conditions;

[0029] Figure 5 The tail end of the molten pool (i.e. Figure 5 Thermal history of the melt pool surface (marked points);

[0030] Figure 6 These are electron microscope images of formed parts under different cooling conditions.

[0031] Among them: 1-base plate, 2-cooling liquid channel, 3-cavity, 4-baffle, 5-welding gun, 6-spray gun; 7-molded part. DETAILED DESCRIPTION

[0032] The present invention is further described in detail below in conjunction with the accompanying drawings:

[0033] In the description of the present invention, it should be noted that the orientations or positional relationships indicated by the terms "center", "upper", "lower", "left", "right", "vertical", "horizontal", "inside", "outside", etc. are based on the orientations or positional relationships shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention; the terms "first", "second", and "third" are only used for descriptive purposes and cannot be understood as indicating or implying relative importance; in addition, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection or a detachable connection; it can be directly connected or indirectly connected through an intermediate medium, and it can be the internal communication of two elements. For those of ordinary skill in the art, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0034] The first aspect of the present invention discloses a method for suppressing pores in arc additively manufactured aluminum alloys. The method solves the common pore problem in WAAM-formed aluminum alloy components through a simple, effective and universal method. The method is that during the arc additive manufacturing of aluminum alloys, a coolant flows inside the substrate, and the substrate is in a liquid nitrogen environment; the arc additive deposits a layer, and liquid nitrogen is sprayed once on the surface of the deposited layer. The method increases the cooling rate of the WAAM process (by more than 80%), reduces the molten pool size (by more than 40%), and shortens the pore overflow distance through an in-situ double cooling optimization scheme, thereby suppressing the formation of pores and promoting the effective removal of pores. The solution aims to reduce the negative impact of pore problems in the manufacturing process, improve the quality of aluminum alloy arc additive manufacturing, and thereby enhance the reliability and performance of components, and promote further development in this field. Specifically, the method includes the following steps:

[0035] Step 1, installing the prepared substrate 1 on the WAAM experimental platform, and the experimental position is accurate to ensure the stability of the printing process;

[0036] Step 2: Set the process parameters in the WAAM forming system, including current, wire feed rate, welding gun scanning speed, etc., and select a suitable coolant, usually water. Set the parameters of the cooling system, such as the flow rate and pressure of the coolant channel. Select a suitable liquid nitrogen spray device;

[0037] Step 3: Start the WAAM equipment and cooling system and perform forming according to the preset path and parameters. After each layer is deposited, liquid nitrogen is evenly sprayed on the sample surface using a spraying device for a time greater than the threshold. Through the in-situ double cooling scheme, the molten pool size can be reduced by more than 40%, the overflow distance of hydrogen pores can be shortened, and the cooling rate can be increased by more than 80%, thereby achieving the effect of suppressing the pores of aluminum alloy components.

[0038] When setting the deposition, the single-channel deposition length is m, and the single-channel deposition spraying time is t 单 The spraying time of a single layer should be determined according to the total deposition length l of each layer. If a single layer is deposited in only one pass, the threshold of the spraying time of this layer is t 单 ; If a single layer is deposited in multiple passes, then after printing multiple passes to complete a layer. The single-pass deposition spraying time is t 单 Determine according to actual conditions. The threshold calculation formula for spraying time is:

[0039] t 总 =t 单 l / m

[0040] See also Figure 1The second aspect of the present invention discloses a device for suppressing pores in aluminum alloys produced by arc additive manufacturing, the device comprising a substrate 1, a cooling liquid channel 2 provided in the substrate 1, the substrate 1 being located in a cavity 3 with an upper opening, and a baffle 4 being provided at the edge of the cavity 3;

[0041] An arc additive manufacturing welding gun 5 and a liquid nitrogen spraying gun 6 are arranged above the cavity 3 .

[0042] In some embodiments of the present invention, an aluminum alloy material with a thickness of about 20-40 mm is selected as the substrate 1. This thickness can provide sufficient mechanical strength and ensure cooling effect. The horizontal cross-sectional area of ​​the substrate 1 should be 5-10 times the projected area of ​​the bottom of the deposited sample to provide a sufficient heat conduction path to effectively remove heat.

[0043] In some embodiments of the present invention, a U-shaped or other suitable shape of cooling liquid channel 2 is designed inside the substrate 1 to wrap the projection shape of the bottom of the deposited sample, so as to ensure that the cooling liquid can evenly cover the entire area of ​​the substrate 1. The diameter of the cooling liquid channel 2 is 6-10 mm to ensure that the flow rate and pressure of the cooling liquid are moderate.

[0044] Specifically, the cooling liquid channel 2 can be a single channel in an array, or can be a serpentine channel covering the entire substrate 1 .

[0045] When the coolant channel 2 is a single channel of the array, the spacing between the single channels is 10-20 mm. When the coolant channel 2 is a serpentine channel, the spacing between adjacent serpentine channels is 10-20 mm.

[0046] Specifically, a coolant inlet and a coolant outlet of the coolant channel 2 are respectively provided at both ends of the substrate 1, and high temperature resistant sealing rings are installed at the coolant inlet and the coolant outlet to ensure that the coolant does not leak in the channel, so as to ensure reliability in long-term use.

[0047] In some embodiments of the present invention, in order to allow the sprayed liquid nitrogen to take away the heat of the formed part while remaining on the substrate to continue to play a cooling role, baffles 4 are added around the substrate 1 to form a cavity 3, and the substrate 1 is in the cavity 3. The baffle 4 is made of high-strength, corrosion-resistant stainless steel or aluminum alloy as a baffle around the substrate, and the height is recommended to be 50-100mm to effectively control the flow of liquid nitrogen. High-temperature resistant silicone or other sealing materials are used for sealing to ensure that the baffle fits tightly with the substrate to prevent leakage of liquid nitrogen during the cooling process.

[0048] In some embodiments of the present invention, the liquid nitrogen spray device can be a liquid nitrogen spray device provided with multiple nozzles, so that a large amount of liquid nitrogen can be sprayed simultaneously to cool the entire cavity 3 and the surface of the deposition layer. It can also be a spray gun 6, which can move above the cavity 3 so that the liquid nitrogen can cover the entire cavity and provide direct cooling to the deposition layer.

[0049] In order to enable relevant personnel in the target field to better understand and implement the present invention, the present invention is now described in more detail with reference to the accompanying drawings.

[0050] The CMT-WAAM process, which is common in aluminum alloy arc additive manufacturing, is taken as an example here, and the specific process parameters are shown in the following table. 205A aluminum alloy with a diameter of 1.2 mm is selected as the forming material. A reciprocating forming strategy is adopted, with 50 forming layers and a formed part length of 160 mm. In the process of forming in-situ double cooling specimens, this experiment uses a kettle as a spraying device to cool the surface of the component. The cooling time of a single layer is greater than the total deposition length of a single layer (unit: mm) divided by 150 mm multiplied by 60 seconds, and ensure that the spraying path is consistent with the deposition path. In this embodiment, the spraying time is 64 seconds.

[0051]

[0052] In order to clarify the differences in solidification conditions of components under different forming conditions, finite element analysis was used to simulate the evolution of the temperature field. At the same time, thermocouples were used to synchronously measure the temperature of the bottom surface of the substrate during the forming process to verify the finite element simulation results, such as Figure 2 shown. Figure 3 The measured thermal history of the substrate is presented together with the results obtained from computational simulations, and it can be seen that the simulation results match the experimental results very well.

[0053] Figure 4 The temperature field of the component under different forming conditions is shown. In-situ double cooling significantly reduces the size of the molten pool and reduces the penetration depth by 46%. Figure 5 The tail end of the molten pool (corresponding to Figure 5 The thermal history of the marked point on the molten pool surface in the figure. By taking the derivative of the thermal history curve at the temperature corresponding to the liquidus line (650℃), the cooling rate of the molten pool when it starts to cool at this position can be obtained. The results show that under conventional cooling conditions, the cooling rate is 146K / s; after adopting the in-situ double cooling condition, the cooling rate of the molten pool is increased to 270K / s, an increase of 85%. Figure 6 The electron microscope images of the samples formed by conventional forming and in-situ double cooling are shown. It can be seen that the density and size of the pores in the component are significantly reduced after using the in-situ double cooling condition.

[0054] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for suppressing pores in aluminum alloy produced by arc additive manufacturing, characterized in that: During the arc additive manufacturing of aluminum alloy, coolant circulates inside the substrate and the substrate is in a liquid nitrogen environment; The arc additive deposits one layer and sprays liquid nitrogen on the surface of the deposited layer.

2. The method for suppressing pores in aluminum alloy produced by arc additive manufacturing according to claim 1, characterized in that: The cooling liquid flowing inside the substrate covers the entire substrate area.

3. The method for suppressing pores in aluminum alloy produced by arc additive manufacturing according to claim 1, characterized in that: Each spraying time is greater than a threshold value, and the threshold value is determined by the single layer deposition length, the single layer deposition spraying time and the total deposition length.

4. The method for suppressing pores in aluminum alloy produced by arc additive manufacturing according to claim 1, characterized in that: During the spraying process, the liquid nitrogen gun is moved over the surface of the deposit.

5. A device for suppressing pores in arc additively manufactured aluminum alloys for implementing the method of claim 1, characterized in that: It comprises a base plate (1), a cooling liquid channel (2) is arranged in the base plate (1), the base plate (1) is located in a cavity (3) with an upper opening, and a baffle (4) is arranged at the edge of the cavity (3); An arc additive manufacturing welding gun (5) and a liquid nitrogen spraying gun (6) are arranged above the cavity (3).

6. The device for suppressing pores in arc additively manufactured aluminum alloy according to claim 5, characterized in that: The horizontal cross-sectional area of ​​the substrate (1) is 5-10 times the projection area of ​​the bottom of the deposited sample.

7. The device for suppressing pores in arc additively manufactured aluminum alloy according to claim 5, characterized in that: The cooling liquid channel (2) covers the entire base plate (1).

8. The device for suppressing pores in aluminum alloy produced by arc additive manufacturing according to claim 5, characterized in that: The height of the baffle (4) is 50-100 mm; sealing materials are provided between adjacent baffles (4) and between the baffles (4) and the substrate (1).

9. The device for suppressing pores in arc additively manufactured aluminum alloy according to claim 5, characterized in that: The coolant introduced into the coolant channel (2) is water.