Zn-based hexabasic alloy soldering lug and welding method thereof

Through Zn-based six-element alloy welding sheet and discharge plasma vacuum welding technology, the problems of overheating and virtual welding during magnesium alloy welding are solved, low-temperature welding and high-strength welding are achieved, and the mechanical properties and welding rate of the weld are improved.

CN118808989APending Publication Date: 2024-10-22SOUTHEAST UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411004212.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

The low melting point and high thermal conductivity of magnesium alloys lead to overheating, grain growth, crystal segregation and other phenomena during welding, which reduces joint performance. The surface of magnesium alloys is active and easily oxidized, making it difficult to wet the solder, causing problems such as virtual soldering and reducing the joint performance. the bonding strength.

Method used

The Zn-based six-element alloy welding sheet is used, containing 4.5~5.5wt.%Mg, 4.5~5.5wt.%Al, 0.5~1wt.%Mn, 0.5~1wt.%Zr and 1.0~1.5wt.% rare earth elements. Discharge plasma vacuum welding technology uses high-temperature fields to destroy the oxide layer, promote micro-metallurgical reactions, reduce welding temperature, control grain refinement, and improve welding strength.

Benefits of technology

Low-temperature welding is achieved, internal stress is reduced, and the mechanical properties of the weld are improved. The shear strength of the welded joint reaches 102.84MPa, and the welding rate can reach more than 99%, solving the problems of virtual welding and tissue coarsening.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118808989A_ABST
    Figure CN118808989A_ABST
Patent Text Reader

Abstract

The invention discloses a Zn-based hexabasic alloy soldering lug and a welding method thereof, and the Zn-based hexabasic alloy soldering lug comprises the following substances in percentage by mass: 4.5 to 5.5 wt.% of Mg, 4.5 to 5.5 wt.% of Al, 0.5 to 1 wt.% of Mn, 0.5 to 1 wt.% of Zr, 1.0 to 1.5 wt.% of rare earth element and the balance of Zn. The rare earth element is one or more of Ce, Y, Er and Gd. The welding method comprises the following steps that the surface of magnesium alloy base metal to be welded is polished, cleaned and dried, and the magnesium alloy base metal to be welded is obtained; assembling on a graphite gasket in an SPS sintering furnace according to an assembling sequence; welding pressure is adjusted, vacuumizing is conducted, the temperature reaches 340-350 DEG C firstly, heat preservation is conducted, then the temperature is reduced to 90-100 DEG C at a constant speed, and finally water cooling is conducted to reduce the temperature to the room temperature. Internal stress generated by welding is reduced, deformation-free welding of the magnesium alloy is achieved, and the overall welding rate reaches 99% or above.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a welding sheet and a welding method thereof, in particular to a Zn-based hexa-element alloy welding sheet and a welding method thereof. Background Art

[0002] Magnesium alloy has low melting point (such as AZ91D magnesium alloy melting point is 596 ℃, AZ31B magnesium alloy melting point is 650 ℃, AM60B magnesium alloy melting point is 615 ℃), so the diffusion activation energy of elements is low during welding heating, the tendency of coarsening of organization and reduction of mechanical properties increases with the increase of welding temperature, and high-power welding heat source is required during welding. The weld and near-seam area are prone to overheating, grain growth, crystal segregation and other phenomena, which reduce the joint performance. At the same time, magnesium alloy has good thermal conductivity, large linear expansion coefficient, and is easy to form low-melting eutectic with some alloy elements (such as Zn, Cu, Al, Ni, etc.) (such as Mg-Zn eutectic temperature is 340 ℃, Mg-Cu eutectic temperature is 480 ℃, Mg-Al eutectic temperature is 430 ℃, Mg-Ni eutectic temperature is 508 ℃), the brittle temperature range is wide, and the temperature gradient of each part of the component is large during welding heating, which is easy to generate internal stress and thus initiate cracks.

[0003] Therefore, the welding materials of magnesium alloys first need a lower melting point, so that the welding temperature can be reduced, and the post-welding deformation and the degradation of the mechanical properties of the substrate can be controlled. Secondly, in order to obtain a good metallurgical bond, the solder needs to have good wettability to the magnesium alloy. However, the surface properties of magnesium alloys are active, and oxides or hydroxides are often formed when the magnesium alloy is welded and heated, which makes it difficult for the solder on the surface of the magnesium alloy to wet and spread, resulting in problems such as cold welding, and reducing the bonding strength. The development of low-melting-point, high-strength and film-breaking solders and their supporting processes for high-strength, high-conductivity weldable magnesium alloys is an urgent problem to be solved. The three components of Zn, Mg and Al form a low-melting-point alloy, and the three components have good compatibility with the parent material components, which is conducive to low-temperature welding. However, the welding performance of the ternary solder alloy is still insufficient, mainly reflected in the excessively fast diffusion reaction rate, the coarse structure of the reaction layer formed, and the insufficient bonding force. Summary of the invention

[0004] Purpose of the invention: In order to overcome the deficiencies in the prior art, the purpose of the present invention is to provide a Zn-based hexa-alloy welding sheet capable of improving the mechanical properties of the weld. Another purpose of the present invention is to provide a welding method for a Zn-based hexa-alloy welding sheet with reduced welding temperature and high welding rate.

[0005] Technical solution: The Zn-based hexavalent alloy welding sheet described in the present invention includes the following substances in percentage by mass: 4.5-5.5wt.% Mg, 4.5-5.5wt.% Al, 0.5-1wt.% Mn, 0.5-1wt.% Zr, 1.0-1.5wt.% rare earth elements, and the balance is Zn.

[0006] Furthermore, the rare earth element is one or more of Ce, Y, Er, and Gd.

[0007] Furthermore, the melting temperature is 340-382°C.

[0008] The welding method of a Zn-based hexavalent alloy welding sheet described in the present invention comprises the following steps:

[0009] Step 1, grinding the surface of the magnesium alloy base material to be welded with sandpaper, cleaning, and drying to obtain the magnesium alloy base material to be welded;

[0010] Step 2: assemble the magnesium alloy base material to be welded onto the graphite gasket in the SPS sintering furnace in the order of graphite pressure head, graphite paper gasket, magnesium alloy base material to be welded, Zn-based hexavalent alloy welding sheet, magnesium alloy base material to be welded, graphite paper gasket, and lower graphite punch from top to bottom;

[0011] Step three, adjust the welding pressure, evacuate the vacuum, and ensure that the temperature continues to rise steadily during the welding process. During the welding operation, the connection temperature of the magnesium alloy is first reached at 340-350°C, and then kept warm, and then the temperature is uniformly reduced to 90-100°C, and finally cooled to room temperature by water cooling to obtain a magnesium alloy welded part.

[0012] Furthermore, in step one, the sandpaper is SiC sandpaper, and 400 mesh, 800 mesh, and 1500 mesh SiC sandpaper are used for grinding, respectively. Cleaning is laser cleaning, which uses a high-energy laser beam to irradiate the surface of the welding piece, so that the dirt, rust or coating on the surface evaporates or peels off instantly, and the surface attachments or surface coatings of the welding piece are removed quickly and effectively. The surface of the magnesium alloy base material to be welded is formed with a pit lattice with a depth of 1 to 5 microns and a diameter of 3 to 5 microns, and the number of micro-pits per unit area is 40,000 / mm 2 These surface micro-pits are conducive to the formation of discharge plasma, improving welding strength and welding rate.

[0013] Further, in step three, the welding pressure is 3 to 10 kN, and the vacuum degree is less than 1 Pa. The heating rate is 30 to 50 ° C / min, the heating time is 5 to 8 min, and the insulation time is 1 to 10 min. The cooling rate is 24 to 30 ° C / min, and the cooling time is 8 to 12 min. The water cooling time is 5 to 10 min. The welding connection temperature is preferably 340 ° C. The low welding temperature is conducive to achieving rapid microscopic metallurgical reaction and metallurgical bonding. The stress concentration caused by excessive cooling speed is reduced during the uniform cooling process, and the obtained welded joint becomes smaller and the residual stress is low, which solves the technical problems such as low welding strength of the virtual weld.

[0014] Preparation principle: Mn, Zr, and RE (rare earth elements) were added to optimize the reaction layer structure. The effects are as follows: (1) Mn is enriched at the reaction interface and can exist in the MgZn phase. This may be because Mn, as a substitutional solid solution element, diffuses slowly in the MgZn phase, thus inhibiting the excessive growth of the reaction layer compound, resulting in a decrease in the thickness of the MgZn phase reaction layer, which can reduce the internal stress generated by the reaction and improve the bonding strength of the interface; (2) Zr can be dispersed at the reaction interface and has a very low solid solubility in magnesium. It has a strong grain refining effect, refines the reaction layer structure, can effectively reduce internal stress, improve joint quality, and has a certain strengthening effect. (3) The addition of an appropriate amount of rare earth elements can make the solder wettability better, improve the reaction layer structure to a certain extent, make it uniform and fine, and can improve the mechanical properties of the reaction layer through solid solution and aging strengthening.

[0015] Zn-based solder has great advantages in the field of Mg alloy brazing. Zn is a low melting point metal with a melting point of only 419.53℃. It is also one of the alloying elements of magnesium alloys and can play a good strengthening effect in magnesium alloys. Both Zn and Mg have a close-packed hexagonal structure. When the Zn content is small (Zn<1wt.%), the role of Zn in Mg is on the one hand its own solid solution strengthening, and on the other hand, a small amount of Zn can also increase the solubility of A1 in Mg and improve the solid solution strengthening effect of A1; in Mg-Zn alloys, when the Zn content is <6wt.%, as the Zn content increases, the tensile strength and yield strength increase, and the elongation decreases; when Zn>6wt.%, the tensile strength decreases with the increase of Zn content, and the elongation decreases more. Zn can improve the creep resistance of castings, and when the Zn content is greater than 2.5wt.%, it has a negative effect on the corrosion resistance of the alloy. Therefore, the Zn content of Mg-Zn alloys used in industry is generally less than 6wt.%. Zn can improve the fluidity and strength of magnesium alloys through solid solution strengthening, but Zn greater than 2wt.% can cause hot cracks. Zn plays an effective protective role against corrosion caused by Fe or Ni doping. Magnesium alloys containing Zn, zirconium and rare earth elements can improve their strength through dispersion strengthening. In addition, adding zinc to magnesium alloys can improve their liquid fluidity, lower their melting point, and refine the grains to form micro-shrinkage, which can produce precipitation strengthening.

[0016] The magnesium alloy substrate is highly active and its surface is easily oxidized. It is difficult for general brazing fluxes to effectively remove surface oxides, and the corrosion of its residues has a great impact on the substrate. Zn-based brazing filler metal has a lower melting point than Al-based and Mg-based brazing filler metals. As an intermediate layer brazing filler metal, it has a good welding effect on magnesium alloys under vacuum atmosphere protection and has high strength.

[0017] Discharge plasma welding technology can use the gas discharge effect of the metal gap to stimulate plasma generation, forming a microscopic local high temperature (2000℃), effectively breaking the oxide layer of the magnesium alloy, and achieving rapid microscopic metallurgical reaction and metallurgical bonding under the premise that the welding temperature is lower than the melting point of the solder. Appropriate pressure (5-15MPa) will promote the connection between powder particles and enhance the welding effect. Its heat preservation process can also promote the grain refinement in the weld and heat-affected zone, further improving the organization, thereby improving the strength and toughness of the weld.

[0018] The invention discloses a method for low temperature welding of MgZn magnesium alloy by using discharge plasma vacuum welding technology. During the welding process, the current flows through the mold and the welding piece to generate a large amount of Joule heat for heating. The current passing through the welding piece to be welded will generate spark discharge between adjacent particles due to the gaps between the particles in the initial stage. Some gas molecules are ionized, and the positive ions and electrons generated move to the cathode and the anode respectively, and discharge between the particles to form plasma. As the density of the plasma increases, the high-speed reverse-moving particle flow generates a large electric spark impact force on the particle surface, which can not only remove the adsorbed gas or the broken Mg alloy oxide film, but also purify and activate the surface particles, and at the same time promote the migration rate of the material, so that it can diffuse rapidly, reduce the welding temperature and shorten the welding time. The edge of the powder particle generates Joule heat under the action of the pulse electric field to form a high temperature field instantly. Under the action of pressure, the plastic deformation of the powder particle is improved, which is conducive to the deformation-free, high-strength and low-temperature welding of the Mg alloy.

[0019] Beneficial effects: Compared with the prior art, the present invention has the following significant features:

[0020] 1. It can reduce the welding temperature and inhibit the formation of coarse compounds in the diffusion reaction layer and the weld structure, so that the structure of the magnesium alloy parent material is almost unaffected during the welding process, reduce the internal stress generated during the welding process, and achieve deformation-free welding of magnesium alloys. The overall welding rate can reach more than 99%, and the mechanical properties of the weld are improved;

[0021] 2. It can remove adsorbed gas or broken Mg alloy oxide film, purify and activate surface particles, and promote the migration rate of substances, making them diffuse rapidly, thus reducing welding temperature and shortening welding time;

[0022] 3. The discharge plasma vacuum welding technology uses the gas discharge effect of the metal gap to stimulate the plasma to form a microscopic local high temperature (2000℃), effectively breaking the oxide layer, and realizing rapid microscopic metallurgical reaction and metallurgical bonding under the premise that the ambient temperature is lower than the melting point of the solder. Under the premise of reducing the welding temperature as much as possible, the melting point of the solder is reduced, the melting range of the solder is controlled, and the formation of coarse compounds in the diffusion reaction layer and the weld structure is inhibited, thereby improving the mechanical properties of the weld. The shear strength of the welded joint reaches 102.84MPa;

[0023] 4. The welding piece was pre-treated in accordance with the discharge plasma welding process, which is conducive to the formation of discharge plasma and improves the welding strength and welding rate. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 It is a schematic diagram of a mold of the present invention;

[0025] Figure 2 The DSC curve diagram of the Zn-based hexavalent alloy welding sheet of the present invention;

[0026] Figure 3 is the heating curve of the discharge plasma welding of the present invention;

[0027] Figure 4 is the shear stress-displacement curve of the magnesium alloy welded joint obtained in Example 1 of the present invention;

[0028] Figure 5 This is a SEM image of the structure of the magnesium alloy welded joint obtained in Example 1 of the present invention. DETAILED DESCRIPTION

[0029] The reagents and materials used in the examples, unless otherwise specified, can be obtained from commercial sources. The welding device is a German FCT-HPD5 spark plasma sintering furnace.

[0030] Example 1

[0031] A welding method for a Zn-based hexavalent alloy welding sheet comprises the following steps:

[0032] (1) Preparation of parent material: A magnesium alloy parent material with a diameter of 29.5*1mm and a height of 2mm was used to grind the surface of the magnesium alloy parent material with 400 mesh, 800 mesh, and 1500 mesh SiC sandpaper, respectively. The surface stains were then removed by ultrasonic cleaning with anhydrous ethanol, and laser cleaning was performed. The surface of the welding piece was irradiated with a high-energy laser beam to form a pit lattice with a depth of 5 microns and a diameter of 3 microns on the surface of the magnesium alloy parent material to be welded, and the number of micro-pits per unit area was 40,000 / mm. 2 After drying, the magnesium alloy base material to be welded is obtained.

[0033] (2) Assembly: The magnesium alloy base material to be welded is assembled onto the graphite gasket in the SPS sintering furnace in the order of graphite pressure head, graphite paper gasket, magnesium alloy base material to be welded, Zn-based hexavalent alloy welding sheet, magnesium alloy base material to be welded, graphite paper gasket, and lower graphite punch. The assembled magnesium alloy base material to be welded is as follows: Figure 1 The Zn-based hexavalent alloy welding sheet includes the following substances in percentage by mass: 5wt.% Mg, 5wt.% Al, 1wt.% Mn, 1wt.% Zr, 1.5wt.% rare earth element Ce, and the balance is Zn.

[0034] like Figure 2 This is the DSC curve of the Zn-based hexa-alloy solder sheet. According to its melting endothermic peak data, it can be obtained that its melting range is 343-382°C, it is completely melted at 382°C, and the melting point is 343°C.

[0035] (3) Discharge plasma welding: Prepare the magnesium alloy base material to be welded assembled in step (2) for discharge plasma welding. Fix the thermocouple equipped with the discharge plasma sintering system itself in contact with the end of the magnesium alloy to be welded, monitor the temperature, adjust the welding pressure to 10kN, turn on the vacuum pump to make the vacuum degree in the sintering furnace less than 1Pa, change the temperature control mode to manual temperature control, and ensure that the temperature rises continuously and stably during the welding process. Figure 3 As shown, the connection temperature of the magnesium alloy first reaches 340°C at 7 minutes of welding, the heating rate is 45°C / min, and the temperature is kept for 10 minutes. Then, the temperature is uniformly reduced at 24°C / min for 10 minutes to 100°C, and finally, the temperature is water-cooled for 5 minutes to room temperature to obtain a magnesium alloy weldment.

[0036] The welded joint obtained in this example was subjected to a shear test. The shear test was conducted on a CMT4503 microcomputer-controlled electronic universal testing machine. The loading rate of the testing machine was set to 0.5 mm / min. The maximum shear force divided by the shear area was used as the evaluation standard for the shear strength. Figure 4 As shown, the shear strength of the welded joint in Example 1 is 102.84 MPa.

[0037] The welded joint of Example 1 was cut perpendicular to the weld surface, and the weld interface was observed using SEM after polishing. Figure 5 It can be seen that there are no obvious welds and holes after welding, and the magnesium alloys on both sides are well bonded, which indicates that the magnesium alloy after welding has almost no damage to the organizational structure of the magnesium alloy base material while ensuring the welding strength.

[0038] Example 2

[0039] A welding method for a Zn-based hexavalent alloy welding sheet comprises the following steps:

[0040] (1) Preparation of parent material: A magnesium alloy parent material with a diameter of 29.5*1mm and a height of 2mm was used to grind the surface of the magnesium alloy parent material with 400 mesh, 800 mesh, and 1500 mesh SiC sandpaper, respectively. The surface stains were then removed by ultrasonic cleaning with anhydrous ethanol, and laser cleaning was performed. The surface of the welding piece was irradiated with a high-energy laser beam to form a pit lattice with a depth of 1 micron and a diameter of 3 microns on the surface of the magnesium alloy parent material to be welded, and the number of micro-pits per unit area was 40,000 / mm. 2 After drying, the magnesium alloy base material to be welded is obtained.

[0041] (2) Assembly: The magnesium alloy base material to be welded is assembled onto the graphite gasket in the SPS sintering furnace in the order of graphite pressure head, graphite paper gasket, magnesium alloy base material to be welded, Zn-based hexavalent alloy welding sheet, magnesium alloy base material to be welded, graphite paper gasket, and lower graphite punch. The assembled magnesium alloy base material to be welded is as follows: Figure 1As shown, the Zn-based hexa-alloy welding sheet includes the following substances in mass percentage: 4.5wt.% Mg, 4.5wt.% Al, 0.5wt.% Mn, 0.5wt.% Zr, 1.0wt.% rare earth element Y, and the balance is Zn. The melting range is 341-370°C.

[0042] (3) Discharge plasma welding: Prepare the magnesium alloy base material to be welded assembled in step (2) for discharge plasma welding, fix the thermocouple equipped with the discharge plasma sintering system itself in contact with the end of the magnesium alloy to be welded, perform temperature monitoring, adjust the welding pressure to 3 kN, turn on the vacuum pump to make the vacuum degree in the sintering furnace less than 1 Pa, change the temperature control mode to manual temperature control, ensure that the temperature rises continuously and stably during the welding process, first reach the connection temperature of the magnesium alloy of 340°C, the heating rate is 30°C / min, keep warm for 1 min, then cool at a uniform rate of 30°C / min to 90°C, and finally cool to room temperature with water for 10 min to obtain a magnesium alloy weldment.

[0043] The shear strength of the magnesium alloy welded part obtained in this embodiment is 93.53 MPa.

[0044] Example 3

[0045] A welding method for a Zn-based hexavalent alloy welding sheet comprises the following steps:

[0046] (1) Preparation of parent material: A magnesium alloy parent material with a diameter of 29.5*1mm and a height of 2mm was used to grind the surface of the magnesium alloy parent material with 400 mesh, 800 mesh, and 1500 mesh SiC sandpaper, respectively. The surface stains were then removed by ultrasonic cleaning with anhydrous ethanol, and laser cleaning was performed. The surface of the welding piece was irradiated with a high-energy laser beam to form a pit lattice with a depth of 5 microns and a diameter of 5 microns on the surface of the magnesium alloy parent material to be welded, and the number of micro-pits per unit area was 40,000 / mm. 2 After drying, the magnesium alloy base material to be welded is obtained.

[0047] (2) Assembly: The magnesium alloy base material to be welded is assembled onto the graphite gasket in the SPS sintering furnace in the order of graphite pressure head, graphite paper gasket, magnesium alloy base material to be welded, Zn-based hexavalent alloy welding sheet, magnesium alloy base material to be welded, graphite paper gasket, and lower graphite punch. The assembled magnesium alloy base material to be welded is as follows: Figure 1 As shown. The Zn-based hexa-alloy welding sheet includes the following substances in mass percentage: 5.5wt.% Mg, 5.5wt.% Al, 1wt.% Mn, 1wt.% Zr, 1.5wt.% rare earth element Er, and the balance is Zn. The melting range is 340-376°C.

[0048] (3) Discharge plasma welding: Prepare the magnesium alloy base material to be welded assembled in step (2) for discharge plasma welding, fix the thermocouple equipped with the discharge plasma sintering system itself in contact with the end of the magnesium alloy to be welded, perform temperature monitoring, adjust the welding pressure to 6 kN, turn on the vacuum pump to make the vacuum degree in the sintering furnace less than 1 Pa, change the temperature control mode to manual temperature control, ensure that the temperature rises continuously and stably during the welding process, first reach the connection temperature of the magnesium alloy of 350°C when the welding operation is 8 minutes, the heating rate is 50°C / min, and the temperature is kept for 5 minutes, then the temperature is uniformly reduced at 27°C / min for 12 minutes to 95°C, and finally the temperature is cooled by water for 8 minutes to room temperature to obtain a magnesium alloy weldment.

[0049] The shear strength of the magnesium alloy welded part obtained in this embodiment is 90.68 MPa.

[0050] Comparative Example 1

[0051] The remaining steps of this comparative example are the same as those of Example 1, except that the rare earth element Ce is omitted. The shear strength of the obtained welded part is 65.82 MPa.

[0052] Comparative Example 2

[0053] The remaining steps of this comparative example are the same as those of Example 1, except that the rare earth element Ce is replaced by Sn. The shear strength of the obtained welded part is 68.43 Mpa.

[0054] Comparative Example 3

[0055] The remaining steps of this comparative example are the same as those of Example 1, except that the welding sheet is replaced with a material including the following mass percentages: 7wt.% Mg, 6wt.% Al, 3wt.% Mn, 2wt.% Zr, 3wt.% rare earth element Ce, and the balance is Zn. The results show that the mechanical properties of the obtained welded joint are significantly reduced, and the shear strength is only 45.23Mpa.

Claims

1. A Zn-based hexavalent alloy welding sheet, characterized in that: The invention comprises the following substances in percentage by weight: 4.5-5.5wt.% Mg, 4.5-5.5wt.% Al, 0.5-1wt.% Mn, 0.5-1wt.% Zr, 1.0-1.5wt.% rare earth elements, and the balance is Zn.

2. A Zn-based hexavalent alloy welding sheet according to claim 1, characterized in that: The rare earth element is one or more of Ce, Y, Er, and Gd.

3. The Zn-based hexavalent alloy welding sheet according to claim 1, characterized in that: The melting temperature is 340-382°C.

4. The welding method of a Zn-based hexavalent alloy welding sheet according to claim 1, characterized in that: The following steps are involved: Step 1, grinding the surface of the magnesium alloy base material to be welded with sandpaper, cleaning, and drying to obtain the magnesium alloy base material to be welded; Step 2: assemble the magnesium alloy base material to be welded onto the graphite gasket in the SPS sintering furnace in the order of graphite pressure head, graphite paper gasket, magnesium alloy base material to be welded, Zn-based hexavalent alloy welding sheet, magnesium alloy base material to be welded, graphite paper gasket, and lower graphite punch from top to bottom; Step three, adjust the welding pressure, evacuate the vacuum, and ensure that the temperature continues to rise steadily during the welding process. During the welding operation, the connection temperature of the magnesium alloy is first reached at 340-350°C, and then kept warm, and then the temperature is uniformly reduced to 90-100°C, and finally cooled to room temperature by water cooling to obtain a magnesium alloy welded part.

5. The welding method of a Zn-based hexavalent alloy welding sheet according to claim 4, characterized in that: In the step 1, the sandpaper is SiC sandpaper, and the SiC sandpapers of 400 mesh, 800 mesh, and 1500 mesh are used for grinding in sequence.

6. The welding method of a Zn-based hexavalent alloy welding sheet according to claim 4, characterized in that: In the step 1, the cleaning is laser cleaning, so that a pit matrix with a depth of 1 to 5 microns and a diameter of 3 to 5 microns is formed on the surface of the magnesium alloy base material to be welded.

7. The welding method of a Zn-based hexavalent alloy welding sheet according to claim 4, characterized in that: In the step three, the welding pressure is 3-10 kN, and the vacuum degree is less than 1 Pa.

8. The welding method of a Zn-based hexavalent alloy welding sheet according to claim 4, characterized in that: In the step 3, the heating rate is 30-50°C / min, the heating time is 5-8min, and the heat preservation time is 1-10min.

9. The welding method of a Zn-based hexavalent alloy welding sheet according to claim 4, characterized in that: In the step 3, the cooling rate is 24-30°C / min, and the cooling time is 8-12min.

10. The welding method of a Zn-based hexavalent alloy welding sheet according to claim 4, characterized in that: In the step 3, the water cooling time is 5 to 10 minutes.