High-toughness wear-resistant welding electrode
By optimizing the composition of the coating and welding core in the welding rod, and utilizing the deoxidizing properties of zinc borate, the problem of insufficient wear resistance and toughness of the welding rod is solved, a welding effect of high toughness and high wear resistance is achieved, and the welding process is improved. situation environment.
Patent Information
- Application Number
- CN202410859195.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-22
AI Technical Summary
Existing welding electrodes have insufficient wear resistance and toughness under complex working conditions that endure high impact and high wear, making it difficult to meet the requirements for high toughness and high wear resistance.
A coating composed of marble, quartz sand, titanium dioxide, ferrotitanium powder, ferrosilicon powder and zinc borate is used, combined with a welding core of manganese, chromium, molybdenum and other elements. By optimizing the composition of the coating and welding core, boric acid is used The deoxidizing performance of zinc can reduce manganese smoke and improve the toughness and wear resistance of the deposited metal after welding.
It significantly improves the toughness and wear resistance of the clad metal after welding, reduces manganese fumes, improves the welding working environment, and shows high performance in impact energy absorption and friction and wear tests.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of welding materials, and in particular to a high-toughness wear-resistant welding rod. Background Art
[0002] Welding rods, also known as welding consumable electrodes or welding rods, are key materials in the arc welding process. They consist of a welding core and a coating. They are widely used in industries such as petrochemicals, mining, electricity, aerospace, shipbuilding, and metallurgy. During arc welding, the welding core carries current to generate an arc to form electric heat, which becomes filler metal after melting and fuses with the parent metal to form a weld. The coating can improve the stability of the arc and allow the welding process to continue. The welding core and the coating work together to ensure arc stability, a smooth welding process, and weld quality.
[0003] In some complex working conditions, such as parts that are subjected to high impact and high wear, such as mixer blades, shovel teeth, spiral reamers, crushing rollers, etc., the welding rods need to have not only high wear resistance, but also high toughness, so that the welded joints can withstand high impact loads without short circuits. However, the existing welding rods have the problems of poor wear resistance and toughness, and it is difficult to meet the requirements of complex working conditions that need to withstand high impact and high wear. Therefore, it is urgent to develop a high-toughness wear-resistant welding rod to solve the above problems. Summary of the invention
[0004] The invention provides a high-toughness wear-resistant welding rod, which solves the problems of poor wear resistance and toughness of the welding rod in the related art.
[0005] The technical solution of the present invention is as follows: A high-toughness wear-resistant welding rod comprises a welding core and a coating coated on the welding core, wherein the coating is composed of the following raw materials in percentage by weight: Marble 30%~50%, quartz sand 10%~20%, titanium dioxide 5%~10%, ferrotitanium powder 4%~8%, ferrosilicon powder 2%~4%, zinc borate 1%~3%, and the balance is sodium carbonate; The welding core is composed of the following components in weight percentage: C 0.05%~0.10%, Mn 0.3%~0.6%, Ni 0.9%~1.0%, Cr 0.3%~0.6%, Mo 0.15%~0.3%, Ti0.15%~0.3%, S≤0.005%, P≤0.005%, and the rest are iron and unavoidable impurities.
[0006] In order to reduce the oxidation degree of the weld metal, manganese is usually added to the welding core of the welding rod. Although the addition of manganese can act as a deoxidizer, manganese smoke will be generated during the welding process, thereby worsening the welding working environment. In the present invention, the high affinity of boron for oxygen is utilized to introduce a boron-containing substance into the coating raw material for deoxidation. Although this can reduce the manganese content in the welding core, reduce manganese smoke during welding, and improve the welding working environment, if the boron-containing substance is boron powder, there will be a problem of boron residue in the weld, reducing the toughness of the deposited metal after welding. When the boron-containing substance zinc borate is introduced and chromium and molybdenum are introduced into the welding core, the zinc borate will cooperate with chromium and molybdenum to improve the toughness of the deposited metal after welding, thereby overcoming the problem of decreased toughness of the deposited metal after welding caused by the introduction of boron.
[0007] As a further technical solution, the welding core is composed of the following components in weight percentage: C 0.08%~0.10%, Mn 0.3%~0.5%, Ni 0.9%~1.0%, Cr 0.5%~0.6%, Mo 0.15%~0.25%, Ti 0.25%~0.3%, S≤0.005%, P≤0.005%, and the rest are iron and unavoidable impurities.
[0008] As a further technical solution, in the components of the welding core, the weight ratio of Cr and Mo to C is 10-15:1.
[0009] In the present invention, when the weight ratio of Cr and Mo to C is 10-15:1, the toughness and wear resistance of the weld metal after welding are further improved.
[0010] As a further technical solution, in the components of the welding core, the weight ratio of Cr to Mo is 2.95:1.
[0011] In the present invention, when the weight ratio of Cr to Mo is 2.95:1, the toughness and wear resistance of the cladding metal after welding are further improved.
[0012] As a further technical solution, in the raw materials of the medicine coating, the weight percentage of the zinc borate is 1.5%~2%.
[0013] In the present invention, when the weight percentage of zinc borate in the coating raw material is 1.5% to 2%, not only the deoxidation effect on the weld is improved, but also the toughness and wear resistance of the cladding metal after welding are further improved.
[0014] As a further technical solution, the diameter of the welding core is 1.6-2 mm, and the thickness of the coating is 0.5-1 mm.
[0015] The present invention also proposes a method for preparing the high-toughness wear-resistant welding rod, which comprises mixing the raw materials of the coating uniformly according to weight percentage, and then applying a binder to the welding core to obtain the high-toughness wear-resistant welding rod.
[0016] As a further technical solution, the binder is water glass or clay.
[0017] The present invention also provides an arc welding method, in which the high-toughness wear-resistant welding rod or the high-toughness wear-resistant welding rod prepared by the preparation method is used during welding.
[0018] As a further technical solution, the material of the welding parts during welding is low alloy steel.
[0019] The working principle and beneficial effects of the present invention are: In the present invention, the coating raw material and the welding core component of the welding rod are optimized and designed, zinc borate is introduced into the coating raw material, and boron deoxidation is introduced by utilizing the large affinity of boron for oxygen, thereby reducing the oxidation degree of the weld metal, and having a good deoxidation effect when the manganese content in the welding core component is low. At the same time, the chromium and molybdenum in the welding core component also react with the zinc borate in the coating raw material and diffuse into the weld, thereby improving the toughness and wear resistance of the deposited metal after welding. In addition, the reduction of the manganese content in the welding core component also reduces the manganese smoke in the arc welding process, thereby improving the working environment of the arc welding. DETAILED DESCRIPTION
[0020] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0021] In the following embodiments and comparative examples, the content of calcium carbonate in the marble is 35% to 45%, the content of silicon dioxide in the quartz sand is 99%, the content of titanium dioxide in the titanium dioxide is 97%, the ferrotitanium powder is Ti32Fe, and the ferrosilicon powder is FeSi75.
[0022] Example 1 A high-toughness wear-resistant electric welding rod comprises a welding core and a coating covering the welding core. The coating is composed of the following raw materials in percentage by weight: Marble 30%, quartz sand 20%, titanium dioxide 5%, ferrotitanium powder 8%, ferrosilicon powder 2%, zinc borate 1%, the balance is sodium carbonate; The solder core is composed of the following components in weight percentage: C 0.10%, Mn 0.3%, Ni 0.9%, Cr 0.6%, Mo 0.3%, Ti 0.15%, S≤0.005%, P≤0.005%, the rest are iron and unavoidable impurities.
[0023] After the raw materials of the coating are prepared and mixed evenly according to the above weight percentage, water glass is pressed on the welding core and dried to obtain a high-toughness wear-resistant welding electrode with a coating thickness of 1 mm and a welding core diameter φ of 2 mm.
[0024] Example 2 A high-toughness wear-resistant electric welding rod comprises a welding core and a coating covering the welding core. The coating is composed of the following raw materials in percentage by weight: Marble 40%, quartz sand 15%, titanium dioxide 7%, ferrotitanium powder 6%, ferrosilicon powder 3%, zinc borate 2%, the balance is sodium carbonate; The solder core is composed of the following components in weight percentage: C 0.08, Mn 0.5%, Ni 0.9, Cr 0.5%, Mo 0.2%, Ti 0.25%, S≤0.005%, P≤0.005%, the rest are iron and unavoidable impurities.
[0025] After the raw materials of the coating are prepared and mixed evenly according to the above weight percentage, water glass is pressed on the welding core and dried to obtain a high-toughness wear-resistant welding electrode with a coating thickness of 1 mm and a welding core diameter φ of 2 mm.
[0026] Example 3 A high-toughness wear-resistant electric welding rod comprises a welding core and a coating covering the welding core. The coating is composed of the following raw materials in percentage by weight: Marble 50%, quartz sand 10%, titanium dioxide 10%, ferrotitanium powder 4%, ferrosilicon powder 4%, zinc borate 3%, the balance is sodium carbonate; The solder core is composed of the following components in weight percentage: C 0.05%, Mn 0.6%, Ni 1.0%, Cr 0.3%, Mo 0.15%, Ti 0.3%, S≤0.005%, P≤0.005%, the rest are iron and unavoidable impurities.
[0027] After the raw materials of the coating are prepared and mixed evenly according to the above weight percentage, water glass is pressed on the welding core and dried to obtain a high-toughness wear-resistant welding electrode with a coating thickness of 1 mm and a welding core diameter φ of 2 mm.
[0028] Example 4 The difference between this embodiment and embodiment 1 is that the welding core is composed of the following components in weight percentage: C 0.05%, Mn 0.6%, Ni 1.0%, Cr 0.3%, Mo 0.2%, Ti 0.3%, S≤0.005%, P≤0.005%, the rest are iron and unavoidable impurities.
[0029] Example 5 The difference between this embodiment and embodiment 1 is that the welding core is composed of the following components in weight percentage: C 0.05%, Mn 0.6%, Ni 1.0%, Cr 0.6%, Mo 0.15%, Ti 0.3%, S≤0.005%, P≤0.005%, the rest are iron and unavoidable impurities.
[0030] Example 6 The difference between this embodiment and embodiment 1 is that the welding core is composed of the following components in weight percentage: C 0.05%, Mn 0.6%, Ni 1.0%, Cr 0.56%, Mo 0.19%, Ti 0.3%, S≤0.005%, P≤0.005%, the rest are iron and unavoidable impurities.
[0031] Example 7 The only difference between this embodiment and embodiment 6 is that the weight percentage of zinc borate in the coating raw material is 1.5%.
[0032] Example 8 The only difference between this embodiment and embodiment 7 is that the weight percentage of zinc borate in the drug covering raw material is 2%.
[0033] Comparative Example 1 The only difference between this comparative example and Example 1 is that zinc borate is not added to the coating raw material, and the weight percentage of Mn in the welding core component is 1.35%.
[0034] Comparative Example 2 The difference between this comparative example and Example 1 is that zinc borate is replaced by an equal weight of boron powder in the drug coating raw material.
[0035] Comparative Example 3 The difference between this comparative example and Example 1 is that the welding core is composed of the following components in weight percentage: C 0.05%, Mn 0.6%, Ni 1.0%, Cr 0.75%, Ti 0.3%, S≤0.005%, P≤0.005%, the rest are iron and unavoidable impurities.
[0036] Comparative Example 4 The difference between this comparative example and Example 1 is that the welding core is composed of the following components in weight percentage: C 0.05%, Mn 0.6%, Ni 1.0%, Mo 0.75%, Ti 0.3%, S≤0.005%, P≤0.005%, the rest are iron and unavoidable impurities.
[0037] Comparative Example 5 The difference between this comparative example and Example 1 is that the welding core is composed of the following components in weight percentage: C 0.05%, Mn 0.6%, Ni 1.0%, Ti 0.3%, S≤0.005%, P≤0.005%, the rest are iron and unavoidable impurities.
[0038] The high-toughness wear-resistant welding electrodes prepared in Examples 1 to 8 and Comparative Examples 1 to 5 were respectively used to perform arc welding on Q345B steel with a thickness of 20 mm (single-side groove angle of 10°, root gap of 16 mm) according to the following arc welding process; Welding process: Use DC welding machine, reverse polarity, welding current is 150A, and welding voltage is 26V.
[0039] Performance Test: 1. Toughness: The impact absorption energy of the deposited metal at -40°C is tested in accordance with GB / T 2650-2022 "Impact test of destructive tests on welds of metallic materials". The notch is a V-notch. Three samples of each group are taken for repeated testing, and the test results are averaged.
[0040] 2. Wear resistance: The friction and wear test was carried out using an M-200 pin-ring friction and wear testing machine. The friction and wear test was carried out at room temperature at a speed of 200 r / min for 3 hours. The weight of each group of 3 samples before and after the friction and wear test was tested, and the average weight loss was calculated. The weight of each sample before friction and wear was 10.0000±0.5000g.
[0041] The test results are shown in the following table:
[0042] It can be seen from Table 1 that compared with Comparative Examples 1 to 5, the impact absorption energy of the deposited metal after welding with the high-toughness wear-resistant welding rods of Examples 1 to 8 is as high as 149 to 178 J at -40°C, and the average weight loss after 3 hours of friction and wear test is as low as 0.0006 to 0.0025 g, indicating that the deposited metal after welding with the high-toughness wear-resistant welding rods prepared by the present invention has high toughness and wear resistance.
[0043] Compared with Example 1, the high-toughness wear-resistant welding rods of Examples 4 to 6 have higher impact absorption energy at -40°C and lower average weight loss after welding of the deposited metal, and among Examples 4 to 6, the high-toughness wear-resistant welding rod of Example 6 has the highest impact absorption energy at -40°C and the lowest average weight loss after welding, indicating that when the weight ratio of Cr and Mo to C is 10 to 15:1, the toughness and wear resistance of the deposited metal after welding are further improved, and when the weight ratio of Cr and Mo is 2.95:1, the toughness and wear resistance of the deposited metal after welding of the obtained high-toughness wear-resistant welding rod are further improved.
[0044] Compared with Example 6, the high-toughness wear-resistant welding rods of Examples 7 to 8 have higher impact absorption energy and lower average weight loss at -40°C after welding, indicating that when the weight percentage of zinc borate in the coating raw material is 1.5% to 2%, the toughness and wear resistance of the cladding metal after welding are further improved.
[0045] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the claims of the present invention.
Claims
1. A high toughness wear-resistant welding electrode, It is characterized in that It includes a welding core and a coating coated on the welding core, wherein the coating is composed of the following raw materials in percentage by weight: Marble 30%~50%, quartz sand 10%~20%, titanium dioxide 5%~10%, ferrotitanium powder 4%~8%, ferrosilicon powder 2%~4%, zinc borate 1%~3%, the balance is sodium carbonate; The welding core is composed of the following components in weight percentage: C 0.05%~0.10%, Mn 0.3%~0.6%, Ni 0.9%~1.0%, Cr 0.3%~0.6%, Mo 0.15%~0.3%, Ti0.15%~0.3%, S≤0.005%, P≤0.005%, and the rest are iron and unavoidable impurities.
2. A high toughness wear-resistant welding electrode according to claim 1, It is characterized in that The welding core is composed of the following components in weight percentage: C 0.08%~0.10%, Mn 0.3%~0.5%, Ni 0.9%~1.0%, Cr 0.5%~0.6%, Mo 0.15%~0.25%, Ti0.25%~0.3%, S≤0.005%, P≤0.005%, and the rest are iron and unavoidable impurities.
3. A high toughness wear-resistant welding electrode according to claim 1 or 2, It is characterized in that In the components of the welding core, the weight ratio of Cr and Mo to C is 10-15:
1.
4. A high-toughness wear-resistant welding electrode according to claim 3, It is characterized in that In the components of the welding core, the weight ratio of Cr to Mo is 2.95:
1.
5. A high-toughness wear-resistant welding electrode according to claim 4, It is characterized in that In the raw materials of the medicine coating, the weight percentage of the zinc borate is 1.5% to 2%.
6. A high toughness wear-resistant welding electrode according to claim 1, It is characterized in that The diameter of the welding core is 1.6-2 mm, and the thickness of the coating is 0.5-1 mm.
7. The method for preparing the high-toughness wear-resistant welding electrode according to any one of claims 1 to 6, It is characterized in that After the raw materials of the coating are mixed uniformly according to weight percentage, a binder is pressed and coated on the welding core to obtain a high-toughness wear-resistant welding rod.
8. The preparation method according to claim 7, It is characterized in that The binder is water glass or clay.
9. An arc welding method, It is characterized in that During welding, the high-toughness wear-resistant welding rod described in any one of claims 1 to 6 or the high-toughness wear-resistant welding rod prepared by the preparation method described in claims 7 to 8 is used.
10. The arc welding method according to claim 9, It is characterized in that The material of the welding parts during the welding is low alloy steel.
Citation Information
Cited By
Surfacing electrode for gear wear repair and preparation method thereof
CN119260241A