Machining method for preparing compressor blade from TC4 alloy radial forging bar
By modifying the extrusion die to perform electrically assisted heating deformation and constant-temperature slow-speed rod extrusion deformation, the problems of texture "macro zones" and grain coarsening in the processing of TC4 alloy blades were solved, and the fatigue performance and processing efficiency of the blades were improved.
Patent Information
- Application Number
- CN202411054775.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-10-22
AI Technical Summary
In the existing TC4 alloy blade processing method, the diameter forged bar is prone to form texture "macro zones" during the precision forging process, which affects the fatigue performance of the blade, and the grain coarsening of the thin rod during the heading process affects the performance.
The modified extrusion die is used for electrically assisted heating deformation to improve the high-temperature plasticity of the blank, control the deformation of the extrusion rod to constant temperature and slow deformation, reduce deformation energy, avoid the formation of strong texture, and simplify the heading processing process.
It improves the fatigue performance of the blade, extends its service life, improves the uniformity of the mechanical properties and processing efficiency of the blade, and avoids empty burning in the texture "macro zone" and thin rod areas.
Smart Images

Figure CN118809105A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of titanium alloy blade preparation, and in particular relates to a processing method for preparing compressor blades from TC4 alloy radial forging bars. Background Art
[0002] TC4 alloy is an α+β alloy developed by the United States in 1954. Due to its high specific strength, excellent corrosion resistance and high operating temperature range, it has been widely used in aviation, aerospace, weapons, automobiles, energy, medical equipment and sports equipment. The application of TC4 alloy in aircraft engines is mainly fan and compressor discs, blades and various types of fasteners. TC4 compressor blades are one of the key parts of aircraft engines. They are usually used in extremely complex and harsh conditions and are subjected to huge aerodynamic stress, centrifugal stress and temperature loads. Compared with other parts, blades are not only complex in structure, high in precision requirements, and complicated in processing procedures, but also have high requirements on the balance of mechanical properties and fatigue life.
[0003] At present, the main material used in the production of aircraft engine blades is TC4 small-sized bars prepared by rolling. Recent research literature reports that TC4 small-sized bars prepared by radial forging have higher strength and uniformity of mechanical properties than rolled bars. Moreover, since the grains of radial forged bars are finer, it is beneficial to the grain control in the subsequent processing of blades. Therefore, the use of radial forged bars is expected to produce compressor blades with better performance. However, the texture strength of radial forged bars is relatively high. During the fine forging process of the blades, "macro zones" are easily generated due to the accumulation of deformation, which affects the load-holding fatigue performance of the blades.
[0004] The production of titanium alloy blades through precision forging is highly efficient, eliminating a large amount of mechanical processing, greatly saving raw materials, ensuring the integrity of the blade surface and the continuity of the metal streamline, improving the strength and fatigue life of the blade, and meeting the high performance index requirements of aircraft engines for blades. The existing precision forging process often uses four-fire precision forging, such as Figure 1 As shown in the figure: the titanium alloy rod is cut into a cylindrical raw material billet 1, and then the extruded part 2 is prepared by heating and extruding, and then the head part 3 is prepared by heating and upsetting, and finally the pre-forging part 4 and the final forging part 5, i.e. the blade blank, are prepared by heating and pre-forging and heating and final forging. Multi-fire forging has an impact on the control of the grain of the blade material and the evolution of the texture. In particular, during the extrusion process, the rod is deformed along the axial direction to reduce the diameter, which further aggravates the <10-10> / / axial wire texture, and easily forms a texture "macro zone", which affects the fatigue performance of the finished blade. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a processing method for preparing compressor blades from TC4 alloy radial forging bars in view of the deficiencies of the above-mentioned prior art. The method uses a modified extrusion die to electrically assist heating and deform the TC4 alloy radial forging bars, thereby improving the high-temperature plasticity of the blank, and controlling the extrusion deformation to be a constant temperature and slow deformation, thereby reducing the deformation energy of the blank, regulating the texture strength in the blade, avoiding the occurrence of texture "macro zones", improving the fatigue performance of the blade, and extending the service life of the blade, thereby solving the problem that the existing four-fire precision forging aggravates the formation of texture "macro zones" and affects the fatigue performance of the finished blade.
[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is: a processing method for preparing compressor blades from TC4 alloy radial forging bars, characterized in that the method comprises the following steps:
[0007] Step 1: Cut a cylindrical billet from the TC4 alloy radial forging bar, and spray an anti-oxidation coating on the circumferential surface of the cylindrical billet;
[0008] Step 2: Place the cylindrical blank sprayed in step 1 in the modified extrusion die, then turn on the power, and use alternating current to simultaneously perform resistance heating on the die and the blank, and use an infrared temperature measuring device to measure the temperature of the blank. When the temperature of the blank reaches the deformation temperature, keep it warm, then perform extrusion deformation, complete the preparation of the extruded part, and maintain the deformation temperature to obtain the heated extruded part.
[0009] Step 3, unloading and taking out the heated extruded part in step 2, and then placing it in a heading die for stamping, and obtaining a heading part after air cooling;
[0010] Step 4: The heading piece in step 3 is subjected to heating pre-forging and heating final forging in sequence to prepare a blade blank, which is then subjected to trimming, chemical milling, vibration finishing, and heat treatment to obtain a compressor blade.
[0011] Although the grains of small-diameter forged TC4 bars for blades are finer, and the tensile strength and yield strength are far higher than those of rolled bars, their texture is very strong, and the extreme densities of the edge and core are 7.81 and 6.84, respectively. Figure 2As shown. This strong texture is further strengthened during the rod extrusion deformation process of the bar billet, and it is very easy to form a "macro-zone" structure, which affects the fatigue performance of the finished blade. In response to this technical problem, the present invention uses TC4 alloy radial forging bar as raw material to cut the billet, and the billet weight deviation is controlled within ±2g. By modifying the extrusion die, the TC4 alloy radial forging bar is subjected to rod extrusion deformation by means of electric assisted heating deformation. Since the die and the billet are simultaneously resistively heated by alternating current, the billet is affected by the electroplastic effect, and the current can impact and eliminate dislocations, thereby improving the high-temperature plasticity of the billet and reducing the rheological resistance. Since the die and the billet are heated at the same time, the rod extrusion deformation is a constant temperature and slow deformation, and the deformation energy acting on the billet is greatly reduced, which effectively avoids the formation of strong texture, improves the fatigue performance of the blade, and extends the service life of the pressed billet.
[0012] In addition, in the existing four-diameter forging process of titanium alloy blades, the extrusion part needs to be heated and kept warm during the upsetting process, but the thin rod part of the extrusion part does not deform during the upsetting process, and the grain size of the thin rod part grows rapidly and coarsens during the process, affecting the performance of the blade. In view of the technical difficulties, the extrusion deformation of the present invention adopts constant temperature deformation, and the heated extrusion part obtained after deformation can be directly transferred to the upsetting die for upsetting deformation, avoiding the secondary heating process and simplifying the precision forging process of the blade.
[0013] The above-mentioned processing method for preparing compressor blades from a TC4 alloy radial forging bar is characterized in that the modified extrusion die in step 2 is made of tungsten-based metal ceramic material, including a matching upper die and a lower die, and copper electrodes are provided outside the upper die and the lower die, and the copper electrodes are connected to a power supply, and the modified extrusion die also includes a control system. The modified extrusion die of the present invention is made of tungsten-based metal ceramic material, usually composed of W, Pt, and ZrC, has high temperature resistance and oxidation resistance, and is suitable for the extrusion deformation process of electrically assisted heating.
[0014] The above-mentioned method for preparing compressor blades from TC4 alloy radial forging bars is characterized in that the heating rate of the resistance heating in step 2 is 10°C / s, and the holding time after reaching the deformation temperature is 1 minute. By adopting a faster heating rate and holding the temperature for 1 minute after reaching the temperature, the temperature of each part of the blank is consistent, which greatly saves the heating time.
[0015] The above-mentioned processing method for preparing compressor blades from TC4 alloy radial forging bars is characterized in that the extrusion deformation in step 2 is constant temperature deformation, the deformation temperature is 20℃-30℃ below the phase transition point, and the deformation rate is 2mm / s~3mm / s. The present invention controls the extrusion deformation temperature so that the rheological resistance of the TC4 alloy radial forging bar blank in this temperature range is further reduced, which is conducive to the completion of slow extrusion deformation and the extension of the service life of the mold; at the same time, by controlling the deformation rate to 2mm / s~3mm / s, that is, using slow deformation, the pressure used for extrusion deformation is reduced, the energy acting on the blank is reduced, and there is not enough energy to deflect the grains to form a strong texture, further avoiding the appearance of texture "macro zone". In addition, although a higher deformation temperature will accelerate the rate of grain growth, the heating rate of the electrically assisted heating deformation adopted by the present invention is fast, and the total time from heating to the end of deformation is within 3 minutes, which will not have an adverse effect on the microstructure of the blade.
[0016] Compared with the prior art, the present invention has the following advantages:
[0017] 1. The present invention uses TC4 alloy radial forging bar as raw material, and adopts electric-assisted heating deformation to perform rod extrusion deformation on the TC4 alloy radial forging bar, so that the mold and the blank are simultaneously subjected to resistance heating, thereby improving the high-temperature plasticity of the blank, and changing the original rapid stamping rod extrusion deformation into constant temperature slow deformation, thereby reducing the deformation energy of the blank, effectively avoiding the formation of strong texture, improving the fatigue performance of the blade, and extending the service life of the pressed blank.
[0018] 2. The present invention uses TC4 alloy forged rods as raw materials. The initial grains of the raw material rods are finer, the strength is higher, the mechanical properties of the rods are more uniform, and the performance of the blades after extrusion deformation and forging or preparation is better.
[0019] 3. The present invention completes the deformation of the extruded rod and the deformation of the upsetting head through one heating, which not only shortens the processing flow and improves the efficiency of blade processing, but also avoids the empty burning of the thin rod area and improves the blade organization.
[0020] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a diagram of the various stages of forging of titanium alloy blades prepared by four-fire precision forging in the prior art.
[0022] Figure 2 Polar diagram of the edge and core of a small diameter forged TC4 bar for a blade.
[0023] Figure 3 It is a schematic diagram of the structure of the modified extrusion die in the present invention.
[0024] Figure 4 This is the microstructure diagram of the heading piece prepared in Example 1 of the present invention.
[0025] Description of Reference Numerals
[0026] 1—upper mold; 2—lower mold; 3—copper electrode;
[0027] 4—Control system; 5—Power supply. DETAILED DESCRIPTION
[0028] like Figure 3 As shown, the modified extrusion die in the present invention includes a matching upper die 1 and a lower die 2, and copper electrodes 3 are provided outside the upper die 1 and the lower die 2, and the copper electrodes 3 are connected to a power supply 5. The modified extrusion die also includes a control system 4; the modified extrusion die adopts tungsten-based metal ceramic material.
[0029] The use process of the modified extrusion die in the present invention is: placing the blank of the TC4 alloy diameter forging bar in the cavity of the lower die 2, and installing the upper die 1 in a matching manner, turning on the power supply, and simultaneously performing resistance heating on the die and the blank through the copper electrode 3, and then applying pressure to perform extrusion deformation. During this use process, the resistance heating process of the copper electrode 3 is adjusted by the control system 4 to achieve temperature control; usually, the control system 4 can use a system of a conventional equipment Gleeble thermal simulation test machine or an SPS thermal sintering equipment.
[0030] Example 1
[0031] This embodiment includes the following steps:
[0032] Step 1: Cut a cylindrical billet with a height of 55.5 mm from a TC4 alloy forged bar with a diameter of 28.5 mm by wire cutting, the billet weight deviation is 1 g, and spray an anti-oxidation coating on the circumferential surface of the cylindrical billet;
[0033] Step 2: Place the cylindrical billet sprayed in step 1 in the modified extrusion die, then turn on the power, and perform resistance heating on the die and the billet simultaneously by alternating current, with a heating rate of 10°C / s, and measure the billet temperature by an infrared temperature measuring device. When the billet temperature reaches 975°C, keep it warm for 1 minute, then perform extrusion deformation, with a deformation rate of 2mm / s, a pressing height of 29mm, and a deformation time of 14.5s, to complete the preparation of the extruded part, and keep the deformation temperature at 975°C to obtain a heated extruded part;
[0034] Step 3: Unload and take out the heated extruded part in step 2, and then place it in a heading die for stamping. After air cooling, a heading part is obtained, and its microstructure is as follows: Figure 4 As shown, from Figure 4It can be seen that the microstructures of the thin rod area (1#) and the head area (2#) of the upsetting piece are both two-phase microstructures, and the microstructures are uniform;
[0035] Step 4: The heading piece in step 3 is subjected to heating pre-forging and heating final forging in sequence to prepare a blade blank, which is then subjected to trimming, chemical milling, vibration finishing, and heat treatment to obtain a compressor blade.
[0036] Example 2
[0037] This embodiment includes the following steps:
[0038] Step 1: Cut a cylindrical billet with a height of 50.1 mm from a TC4 alloy forged bar with a diameter of 30 mm by wire cutting, the billet weight deviation is 1 g, and spray an anti-oxidation coating on the circumferential surface of the cylindrical billet;
[0039] Step 2: Place the cylindrical billet sprayed in step 1 in the modified extrusion die, then turn on the power, and perform resistance heating on the die and the billet simultaneously by alternating current, with a heating rate of 10°C / s, and measure the billet temperature by an infrared temperature measuring device. When the billet temperature reaches 980°C, keep it warm for 1 minute, then perform extrusion deformation, with a deformation rate of 3mm / s, a pressing height of 27mm, and a deformation time of 9s, to complete the preparation of the extruded part, and keep the deformation temperature at 980°C to obtain a heated extruded part;
[0040] Step 3, unloading and taking out the heated extruded part in step 2, and then placing it in a heading die for stamping, and obtaining a heading part after air cooling, wherein the microstructure thereof is a two-phase structure and the structure is uniform;
[0041] Step 4: The heading piece in step 3 is subjected to heating pre-forging and heating final forging in sequence to prepare a blade blank, which is then subjected to trimming, chemical milling, vibration finishing, and heat treatment to obtain a compressor blade.
[0042] Example 3
[0043] This embodiment includes the following steps:
[0044] Step 1: Cut a cylindrical billet with a height of 53.6 mm from a TC4 alloy forged bar with a diameter of 29 mm by wire cutting, the billet weight deviation is 1 g, and spray an anti-oxidation coating on the circumferential surface of the cylindrical billet;
[0045] Step 2: Place the cylindrical billet sprayed in step 1 in the modified extrusion die, then turn on the power, and perform resistance heating on the die and the billet simultaneously by alternating current, with a heating rate of 10°C / s, and measure the billet temperature by an infrared temperature measuring device. When the billet temperature reaches 970°C, keep it warm for 1 minute, then perform extrusion deformation, with a deformation rate of 2.5mm / s, a pressing height of 25mm, and a deformation time of 10s, to complete the preparation of the extruded part, and keep the deformation temperature at 970°C to obtain a heated extruded part;
[0046] Step 3, unloading and taking out the heated extruded part in step 2, and then placing it in a heading die for stamping, and obtaining a heading part after air cooling, wherein the microstructure thereof is a two-phase structure and the structure is uniform;
[0047] Step 4: The heading piece in step 3 is subjected to heating pre-forging and heating final forging in sequence to prepare a blade blank, which is then subjected to trimming, chemical milling, vibration finishing, and heat treatment to obtain a compressor blade.
[0048] In summary, compared with blades prepared by traditional four-fire precision forging, the method for preparing tablet press blades of the present invention shortens the processing process, improves the efficiency of blade processing, improves the uniformity of the blade's structure and mechanical properties, and thus improves the fatigue performance of the blade.
[0049] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent change made to the above embodiment according to the technical essence of the invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A method for preparing compressor blades from TC4 alloy radial forging bars, characterized in that: The method comprises the following steps: Step 1: Cut a cylindrical billet from the TC4 alloy radial forging bar, and spray an anti-oxidation coating on the circumferential surface of the cylindrical billet; Step 2: Place the cylindrical blank sprayed in step 1 in the modified extrusion die, then turn on the power, and use alternating current to simultaneously perform resistance heating on the die and the blank, and use an infrared temperature measuring device to measure the temperature of the blank. When the temperature of the blank reaches the deformation temperature, keep it warm, then perform extrusion deformation, complete the preparation of the extruded part, and maintain the deformation temperature to obtain the heated extruded part. Step 3, unloading and taking out the heated extruded part in step 2, and then placing it in a heading die for stamping, and obtaining a heading part after air cooling; Step 4: The heading piece in step 3 is subjected to heating pre-forging and heating final forging in sequence to prepare a blade blank, which is then subjected to trimming, chemical milling, vibration finishing, and heat treatment to obtain a compressor blade.
2. The method for preparing compressor blades from TC4 alloy radial forging bars according to claim 1, characterized in that: The modified extrusion die in step 2 is made of tungsten-based metal ceramic material, including a matching upper die (1) and a lower die (2), the upper die (1) and the lower die (2) are both provided with copper electrodes (3), and the copper electrodes (3) are both connected to a power supply (5), and the modified extrusion die also includes a control system (4).
3. The method for preparing compressor blades from TC4 alloy radial forging bars according to claim 1, characterized in that: The heating rate of the resistance heating in step 2 is 10°C / s, and the insulation time after reaching the deformation temperature is 1 minute.
4. The method for preparing compressor blades from TC4 alloy radial forging bars according to claim 1, characterized in that: The extrusion deformation in step 2 is constant temperature deformation, the deformation temperature is 20° C. to 30° C. below the phase transition point, and the deformation rate is 2 mm / s to 3 mm / s.
Citation Information
Patent Citations
Heating layer for megawatt wind turbine blade auxiliary mould and manufacturing method thereof
CN102114681A
Aviation engine blade forging method and die
CN109317588A
Micro plastic forming method of titanium alloy microgear
CN110153217A
Forging technique of aircraft engine blade based on titanium alloy
CN110369670A
Electric pulse rapid heating method for titanium alloy barrel blank
CN118080704A