Aero-engine combustion chamber outer sleeve matching surface size repairing method

The mating surface of the combustion chamber casing is repaired through five-axis machining and thermal spraying technology, which solves the problems of complex maintenance and long cycle in the existing technology, achieves simplified process and performance improvement, and is suitable for repairing the mating surface of the combustor casing of aeroengines. .

CN118809455AActive Publication Date: 2024-10-22STATE-OWNED SICHUAN WEST MASCH FACTORY
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
CN202411243489.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-10-22
Estimated Expiration
2044-09-05

AI Technical Summary

Technical Problem

The existing combustion chamber jacket mating surface maintenance methods are complicated and require a long repair cycle, which affects engine performance and maintenance productivity.

Method used

A five-axis machining center is used for tool alignment cutting, and sand blowing and thermal spraying technology are combined to repair the mating surface of the combustion chamber jacket. The process is shortened to 6 steps, and NiAl powder and NiCrW powder are used to form a wear-resistant coating to improve performance.

Benefits of technology

The repair cycle is shortened, the process steps are simplified, the performance and maintenance efficiency of the combustion chamber jacket are improved, and the cost of parts procurement is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
Patent Text Reader

Abstract

The invention discloses an aero-engine combustion chamber outer sleeve matching surface size repairing method. The method comprises the steps that after being cut, a matching surface is cleaned and dried; protecting a non-matching surface area of the combustion chamber jacket, and then carrying out sand blasting treatment on a matching surface area; the NiAl powder and the NiCrW powder are dried; plasma equipment is adopted for sequentially conducting bottom layer spraying and surface layer spraying on the matching surface, NiAl powder is adopted for multiple times to spray the bottom layer till the thickness of the bottom layer ranges from 0.25 mm to 0.3 mm, and NiCrW powder is adopted for multiple times to spray the surface layer till the thickness of the bottom layer ranges from 0.5 mm to 0.7 mm; and the sprayed matching surfaces of the combustion chamber outer sleeve are machined until the diameter of the matching surface A ranges from 793.86 mm to 799.86 mm, and the diameter of the matching surface B ranges from 852.77 mm to 854.77 mm. According to the method, the size of the wear surface is recovered through machining and thermal spraying, the working procedure is shortened to only six steps, and the repair period is shortened; the NiAl powder and the NiCrW powder are thermally sprayed to form a coating on the matching surface of the combustion chamber jacket, so that the performance of the combustion chamber jacket is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of combustion chamber casing matching surface dimension repair, and in particular relates to a method for repairing the matching surface dimension of an aircraft engine combustion chamber casing. Background Art

[0002] During engine operation, the outer casing of the combustion chamber and the guide casing vibrate due to the alternating load transmitted by the rotation of the blades, causing eccentric wear on the matching surfaces A and B of the outer casing of the combustion chamber, resulting in a decrease in airtightness and affecting engine performance. If the size of this part is out of tolerance, it must be stopped from use and replaced with a new one or repaired by welding before it can be installed and used, which is not conducive to improving maintenance capacity and carrying out maintenance work.

[0003] In order not to affect the use of parts, the existing combustion chamber outer sleeve mating surface is repaired by argon arc welding. The repair process includes 15 processes. The specific methods are as follows: Parts receiving - runout check - machining - cleaning - pre-weld heat treatment - protection - argon arc welding - post-weld heat treatment - post-weld shaping - machining - fluorescent flaw detection - x-ray inspection - runout check - dimension measurement - inspection and acceptance.

[0004] However, the existing process for repairing the outer sleeve matching surface of the combustion chamber is complex and has a long repair period. Summary of the invention

[0005] In order to solve the problem that the existing combustion chamber outer jacket mating surface maintenance using argon arc welding has a complex repair method and a long repair cycle, the present invention provides an aircraft engine combustion chamber outer jacket mating surface size repair method, which reduces the repair process steps and shortens the repair cycle.

[0006] The purpose of the present invention is achieved through the following technical solutions: The invention discloses a method for repairing the size of the mating surface of an outer sleeve of an aero-engine combustion chamber, comprising the following steps: Place the combustion chamber outer casing on the five-axis machining center platform for fixation and centering, adjust the tool to align with the combustion chamber outer casing mating surface, and cut the worn area of ​​the mating surface flat until the mating surface size is larger than the minimum value required by the standard; Clean and dry the mating surfaces after cutting; After protecting the non-matching surface area of ​​the outer casing of the combustion chamber, the matching surface area is subjected to sandblasting treatment until the matching surface area is uniformly gray and the surface roughness is 2.0μm to 4.8μm; The NiAl powder and the NiCrW powder are dried at a temperature of 40°C to 80°C for a drying time of more than 30 minutes; The matching surface is sprayed with a plasma device in sequence for the bottom layer and the surface layer, wherein the bottom layer is sprayed with NiAl powder for multiple times until the bottom layer thickness is 0.25 mm to 0.3 mm, and the surface layer is sprayed with NiCrW powder for multiple times until the bottom layer thickness is 0.5 mm to 0.7 mm; The sprayed combustion chamber outer sleeve mating surface is machined until the diameter of the A mating surface is 793.86 mm to 799.86 mm and the diameter of the B mating surface is 852.77 mm to 854.77 mm.

[0007] Compared with the prior art, the present invention has at least the following advantages and beneficial effects: The invention restores the size of the worn surface by machining and thermal spraying, shortens the process to only 6 steps, and shortens the repair cycle; NiAl powder and NiCrW powder are thermally sprayed to form a coating on the matching surface of the outer casing of the combustion chamber, thereby improving the performance of the outer casing of the combustion chamber. BRIEF DESCRIPTION OF THE DRAWINGS

[0008] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0009] Figure 1 It is a schematic diagram of the structure of the combustion chamber outer shell. DETAILED DESCRIPTION

[0010] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Generally, the components of the embodiments of the present invention described and shown in the drawings here can be arranged and designed in various different configurations.

[0011] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0012] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features of the embodiments may be combined with each other.

[0013] It should be noted that similar reference numerals and letters denote similar items in the following drawings, and therefore, once an item is defined in one drawing, further definition and explanation thereof is not required in subsequent drawings.

[0014] In the description of the present invention, it should be noted that the terms "center", "upper", "lower", "left", "right", "vertical", "horizontal", "inside", "outside", etc. indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, or the positions or positional relationships in which the product of the invention is usually placed when in use, or the positions or positional relationships commonly understood by those skilled in the art, which are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", etc. are only used to distinguish the description, and cannot be understood as indicating or implying relative importance.

[0015] In the description of the present invention, it is also necessary to explain that, unless otherwise clearly specified and limited, the terms "set", "install", "connect", and "connect" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0016] The present invention discloses a method for repairing the size of the mating surface of the outer jacket of an aircraft engine combustion chamber, which restores the size of the worn surface by machining and thermal spraying, shortens the process to only 6 steps, and shortens the repair cycle; NiAl powder and NiCrW powder are thermally sprayed to form a coating on the mating surface of the outer jacket of the combustion chamber, thereby improving the performance of the outer jacket of the combustion chamber. Specifically, the repair method includes steps S01 to S06. It should be noted that the step identification in this scheme is only for the convenience of explaining the method, and does not constitute a limitation on the sequence. The sequence of each step shall be based on its language description and the sequence of each signal.

[0017] Step S01, placing the combustion chamber outer casing on the five-axis machining center platform for fixing and centering, adjusting the tool to align with the combustion chamber outer casing mating surface, and cutting the worn part of the mating surface flat until the mating surface size is larger than the minimum value required by the standard.

[0018] The structural diagram of the combustion chamber casing 1 is shown in FIG. Figure 1 As shown, the mating surfaces include an A mating surface 11 and a B mating surface 12 .

[0019] During cutting, the A mating surface 11 and the B mating surface 12 are aligned with the tool for cutting. During cutting, the processing size is 0.3 mm to 0.5 mm, and the single feed amount is 0.05 mm. Cut until the inner diameter of the A mating surface is less than or equal to 794.86 mm, and the inner diameter of the B mating surface is less than or equal to 849.77 mm.

[0020] Step S02: Clean and dry the mating surface after cutting.

[0021] In this step, acetone is used to clean the mating surface to ensure that there is no residual metal chips, oil stains, etc. on the processed parts. After cleaning, it can be placed at room temperature to dry naturally or wiped dry with a clean white cloth.

[0022] Step S03: After protecting the non-matching surface area of ​​the outer casing of the combustion chamber, perform sandblasting on the matching surface area until the matching surface area is uniformly gray and has a surface roughness of 2.0 μm to 4.8 μm.

[0023] This step only requires sandblasting treatment on the mating surface area, so it is necessary to first perform protective treatment on other areas except the mating surface, that is, non-mating surface areas. Specifically, a pressure-sensitive tape can be used to protect the non-mating surface area.

[0024] When sandblasting the mating surface area, use 120 mesh white corundum sand, control the compressed air pressure to 0.15 MPa ~ 0.35 MPa, the sandblasting distance to 100 mm ~ 150 mm, and the sandblasting angle to 75° ~ 90°, and sandblast until the surface of the part is uniformly gray.

[0025] The mating surfaces should be sandblasted. The qualified sandblasted surface should be a uniformly rough surface. No surface contamination such as rust, spots, dirt, scale, oil, fingerprints, etc. that may affect the coating quality is allowed. The surface roughness of the mating surface after sandblasting is 2.0μm to 4.8μm to ensure the spray quality of the spray layer during subsequent spraying.

[0026] Step S04, drying the NiAl powder and the NiCrW powder at a drying temperature of 40° C. to 80° C. for a drying time greater than 30 min.

[0027] NiAl powder and NiCrW powder are dried before spraying to improve the spraying quality.

[0028] Specifically, a clean powder drying box may be used or a powder barrel may be placed in a drying oven to dry the NiAl powder and the NiCrW powder.

[0029] Step S05, using plasma equipment to spray the bottom layer and the surface layer on the mating surface in sequence, wherein the bottom layer 13 is sprayed with NiAl powder for multiple times until the bottom layer thickness is 0.25 mm to 0.3 mm, and the surface layer 14 is sprayed with NiCrW powder for multiple times until the bottom layer thickness is 0.5 mm to 0.7 mm.

[0030] In this step, NiAl powder and NiCrW powder are used for the bottom layer and the surface layer, respectively. When spraying the NiAl powder of the bottom layer, the current is 550±10V, the voltage is 40±5A, the spraying distance is 100±10mm, and the spraying is performed 18 to 22 times until the thickness of the bottom layer is 0.25 mm to 0.3 mm.

[0031] When spraying the NiCrW powder on the surface layer, the current is 380±10V, the voltage is 35±5A, the spraying distance is 100±10mm, and the spraying is performed 18 to 22 times until the thickness of the bottom layer is 0.5 mm to 0.7 mm.

[0032] The bottom layer is formed by spraying NiAl powder, which serves as an intermediate bonding layer to firmly connect the substrate and the wear-resistant layer, thereby avoiding the surface layer directly bonding to the substrate and causing shedding failure due to low adhesion.

[0033] The surface layer is made of NiCrW powder, which is a wear-resistant coating. It effectively improves the wear resistance of the mating surface of the parts and reduces the probability of collision and wear damage during the use of the parts.

[0034] After spraying, visual inspection shows that the coating surface should be flat, dense, uniform in color, and free of defects such as cracks, delamination, peeling, and edge warping.

[0035] Step S06, machining the sprayed combustion chamber outer jacket mating surface until the diameter of the A mating surface is 793.86 mm to 799.86 mm and the diameter of the B mating surface is 852.77 mm to 854.77 mm.

[0036] During machining, the machining size is 0.25 mm ~ 0.7 mm, and the single feed amount is 0.05 mm to improve the repair quality.

[0037] The method of this scheme restores the size of the worn surface through machining and thermal spraying, shortens the modification cycle, and improves the performance of the coating through the study of current, voltage and spraying distance during the spraying process.

[0038] The method of this scheme removes the worn areas of the A and B mating surfaces while minimizing the damage to the substrate as much as possible, thereby preventing the parts from being deformed due to excessive damage to the substrate, while ensuring that the subsequent spraying thickness is not too thin or too thick, and can meet the use requirements under engine operating conditions.

[0039] The method of this scheme can repair the combustion chamber liner to meet the installation conditions. Compared with welding repair, spraying reduces the repair process, improves production efficiency, reduces the purchase funds of parts, and is conducive to the development of maintenance and support work.

[0040] Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for repairing the size of the outer cover of the combustion chamber of an aircraft engine, characterized in that: The following steps are involved: Place the combustion chamber outer casing on the five-axis machining center platform for fixation and centering, adjust the tool to align with the combustion chamber outer casing mating surface, and cut the worn area of ​​the mating surface flat until the mating surface size is larger than the minimum value required by the standard; Clean and dry the mating surfaces after cutting; After protecting the non-matching surface area of ​​the outer casing of the combustion chamber, the matching surface area is subjected to sandblasting treatment until the matching surface area is uniformly gray and the surface roughness is 2.0μm to 4.8μm; The NiAl powder and the NiCrW powder are dried at a temperature of 40°C to 80°C for a drying time of more than 30 min; The matching surface is sprayed with a plasma device in sequence for the bottom layer and the surface layer, wherein the bottom layer is sprayed with NiAl powder for multiple times until the bottom layer thickness is 0.25 mm to 0.3 mm, and the surface layer is sprayed with NiCrW powder for multiple times until the bottom layer thickness is 0.5 mm to 0.7 mm; The sprayed combustion chamber outer sleeve mating surface is machined until the diameter of the A mating surface is 793.86 mm to 799.86 mm and the diameter of the B mating surface is 852.77 mm to 854.77 mm.

2. A method for repairing the size of the outer surface of the combustion chamber of an aircraft engine according to claim 1, characterized in that: The worn area of ​​the mating surface is cut flat until the size of the mating surface is larger than the minimum value required by the standard: The worn parts of the mating surfaces are cut with a processing size of 0.3 mm to 0.5 mm and a single feed amount of 0.05 mm until the inner diameter of the A mating surface is less than or equal to 794.86 mm and the inner diameter of the B mating surface is less than or equal to 849.77 mm.

3. The method for repairing the size of the outer surface of the combustion chamber of an aircraft engine according to claim 1, characterized in that: The cleaning of the mating surface after cutting is as follows: Clean the mating surfaces with acetone.

4. A method for repairing the size of the outer surface of the combustion chamber of an aircraft engine according to claim 1, characterized in that: When the non-matching surface area of ​​the outer casing of the combustion chamber is protected and the matching surface area is sandblasted, 120 mesh white corundum sand is used, the compressed air pressure is controlled to be 0.15 MPa to 0.35 MPa, the sandblasting distance is 100 mm to 150 mm, and the sandblasting angle is 75° to 90°.

5. A method for repairing the size of the outer surface of the combustion chamber of an aircraft engine according to claim 1, characterized in that: The bottom layer is sprayed with NiAl powder for multiple times until the bottom layer thickness is 0.25 mm to 0.3 mm, including: The NiAl powder was sprayed 18 to 22 times in sequence at a current of 550±10V, a voltage of 40±5A, and a spraying distance of 100±10mm to form a base layer with a thickness of 0.25 mm to 0.3 mm.

6. A method for repairing the size of the outer surface of the combustion chamber of an aircraft engine according to claim 1, characterized in that: The surface layer is sprayed with NiCrW powder for multiple times until the bottom layer thickness is 0.5 mm to 0.7 mm, including: The NiCrW powder was sprayed 18 to 22 times in sequence with a current of 380±10V, a voltage of 35±5A and a spraying distance of 100±10mm to form a surface layer with a thickness of 0.5 mm to 0.7 mm.

7. A method for repairing the size of the outer surface of the combustion chamber of an aircraft engine according to claim 1, characterized in that: When machining the sprayed combustion chamber outer sleeve matching surface, the machining size is 0.25 mm to 0.7 mm, and the single feed amount is 0.05 mm.

Citation Information

Patent Citations

  • Thermal spraying remanufacturing method for damaged end surface of aero-engine accessory gearbox housing

    CN102877017A

  • Aeroengine case seam allowance size repairing method

    CN105401113A

  • Aero-engine titanium alloy part seam allowance size repairing method

    CN109338271A

  • Preparation method of shaft sleeve protection coating resisting corrosion and wear of molten metal

    CN109898046A

  • Size correcting method for aeroengine high-temperature alloy disc shaft abrasion

    CN111020449A