Modified polyamide composite film and preparation process thereof
By designing and preparing modified polyamide composite films, the problem of uneven strength and elongation at break of aluminum-plastic films during lithium battery molding was solved, achieving high strength and uniformity and improving the stamping performance of lithium battery aluminum-plastic films.
Patent Information
- Application Number
- CN202410565561.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-08
- Publication Date
- 2024-10-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The uniformity of strength and elongation at break of existing aluminum-plastic films is difficult to meet the requirements of different models in the lithium battery molding process, affecting the stamping depth and quality of aluminum-plastic films.
A modified polyamide composite film structure, comprising a first layer, a second layer, and a third layer, is formed by co-extrusion, rapid cooling molding, and multiple stretching through specific raw material composition and process flow, resulting in a high-strength and uniform film structure.
It improves the 360° tensile strength and elongation at break of aluminum-plastic film, enhances the deep-drawing performance of aluminum-plastic film for lithium batteries, and meets the molding requirements of different types of lithium batteries.
Smart Images

Figure CN118810179A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of composite films, in particular to a modified polyamide composite film and a preparation process thereof. Background Art
[0002] At present, the outer layer of the general aluminum-plastic film is a polyamide film (also known as biaxially oriented nylon film or nylon film or BOPA film) or a polyester film (also known as biaxially oriented polyester film or BOPET film), or a composite film of the two. In the usual aluminum-plastic film preparation process, the aluminum foil and the outer film are composited using traditional adhesives.
[0003] According to different lithium battery models, the aluminum-plastic film is stamped into the size of the matching battery model through the molding machine mold. During the stamping process, we found that the strength and elongation at break (commonly known as toughness) of the outer layer of the aluminum-plastic film and the uniformity of its strength and elongation at break play a very critical role in the molding depth. Summary of the invention
[0004] Therefore, in order to solve the above-mentioned shortcomings, the present invention provides a modified polyamide composite film and a preparation process.
[0005] The present invention is implemented by constructing a modified polyamide composite film and a preparation process, comprising a film, the total thickness of the film is 15-30 μm, and the film comprises a first layer, a second layer, and a third layer;
[0006] The first layer is 2-4 μm thick and is in contact with the aluminum foil.
[0007] The first layer is composed of PA6 chips, with a relative viscosity of 3.0-3.2;
[0008] The second layer is a core layer, and the second layer is a combination of PA6 slices and long carbon chain polyamide, a copolymer of long carbon chain polyamide and polyamide 6, or both;
[0009] The third layer is composed of PA6 slices, open anti-adhesive lubricant masterbatch, anti-adhesive agent and lubricant in the masterbatch.
[0010] Preferably, the mass ratio of the second layer is 80-95% of PA6 slices, and one of the long carbon chain polyamide, the copolymer of long carbon chain polyamide and polyamide 6, or the combination of the two accounts for 20-5% of the total mass of the second layer;
[0011] The relative viscosity of PA6 chips is 3.4-4.0;
[0012] The long carbon chain polyamide is at least one of PA11, PA12, PA510, PA512, PA610, PA612, PA1010, PA1012, and PA1212.
[0013] Preferably, the third layer has a thickness of 3-6 μm and is the outermost surface, which is a smooth surface;
[0014] The mass ratio of the third layer is: PA6 slice 90-99%, its relative viscosity is 3.0-3.2, open anti-adhesion lubricant masterbatch 10-1%, the mass percentage of anti-adhesion agent in the masterbatch is 4-6%, and the mass percentage of lubricant is 4-6%.
[0015] A process for preparing a modified polyamide composite film, characterized in that:
[0016] The steps include:
[0017] Step S1: After various raw materials of each layer are mixed uniformly according to the formula, they are cleanly metered and added, and co-extruded through respective extruders, metering pumps, disc filters, melt pipes, distributors and T-die heads to obtain continuous sheet melt;
[0018] Step S2: the continuous sheet melt is rapidly cooled and formed by a chilled roller having a surface temperature of 18-25°C;
[0019] Step S3: Then, longitudinal stretching is performed. Before longitudinal stretching, the sheet is preheated by two pairs of rollers at a temperature of 40-50°C, and the first longitudinal stretching is performed under the condition that the stretching roller temperature is 50-60°C, and then both surfaces are immediately quenched by a pair of quenching rollers at a temperature of 18-25°C;
[0020] Step 4: Then, preheat the rollers at a temperature of 50-60°C for a second time, and perform longitudinal stretching for a second time under the condition that the stretching roller temperature is 50-60°C;
[0021] Step S5: Then immediately perform a second rapid cooling on both surfaces on a pair of rapid cooling rollers at a temperature of 18-25°C, the first longitudinal stretching multiple is 1.8-2.4, the second longitudinal stretching multiple is 1.4-2, and the total number of digits is 2.5-3.5;
[0022] Step S6: After longitudinal stretching, the film is then stretched transversely, with the transverse stretching multiple being 2.5-3.5 times, the transverse relaxation ratio being 7-13%, and the production speed being 80-160 m / min.
[0023] The extruder, metering pump, disc filter, melt pipe, distributor and T-die in step S1 are set at a temperature of 215-300°C.
[0024] The present invention has the following advantages: The present invention provides a modified polyamide composite film and a preparation process by improvement, which has the following improvements compared with the same type of equipment:
[0025] The present invention discloses a modified polyamide composite film and a preparation process thereof. The polyamide composite film has been tested to have a tensile strength in all directions of 360° that can be controlled at (280±10%) MPa, and a breaking length rate in all directions of 360° that can be controlled at (130±10%)%. The modified polyamide composite film is used to replace a conventional outer polyamide film or polyester film or a composite film of the two-1, and the aluminum-plastic film for lithium batteries produced by conventional processes can greatly improve the deep-drawing performance of the aluminum-plastic film. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 : Schematic diagram of aluminum-plastic film for lithium batteries;
[0027] Figure 2 : Schematic diagram of the structure of modified polyamide composite film;
[0028] Figure 3 : The test results of the embodiments of the present invention are compared with the typical values of conventional aluminum-plastic films, and different process conditions are listed in each embodiment. DETAILED DESCRIPTION
[0029] The following will be combined Figure 3 The present invention is described in detail, and the technical solutions in the embodiments of the present invention are made clear. The complete description is obvious. The described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0030] It should be noted that when a component is referred to as being "fixed to" another component, it may be directly on the other component or there may also be a component centered. When a component is considered to be "connected to" another component, it may be directly connected to the other component or there may also be a component centered. When a component is considered to be "set on" another component, it may be directly set on the other component or there may also be a component centered. The terms "vertical", "horizontal", "left", "right" and similar expressions used herein are for illustrative purposes only.
[0031] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0032] Embodiment 1;
[0033] A modified polyamide composite film and preparation process of the present invention, the total thickness of the aluminum-plastic film is 113um, the total thickness of the film is 20μm, and the film includes a first layer, a second layer, and a third layer;
[0034] The first layer is 2 μm thick and is in contact with the aluminum foil.
[0035] The first layer is composed of PA6 chips with a relative viscosity of 3;
[0036] The second layer is a core layer, and the second layer is a combination of PA6 slices and long carbon chain polyamide, a copolymer of long carbon chain polyamide and polyamide 6, or both;
[0037] The mass ratio of the second layer: PA6 slices 82%, one of the long carbon chain polyamide, the copolymer of long carbon chain polyamide and polyamide 6 or the combination of the two accounts for 18% of the total mass of the second layer;
[0038] The relative viscosity of PA6 slices is 3.5;
[0039] The long carbon chain polyamide is at least one of PA11, PA12, PA510, PA512, PA610, PA612, PA1010, PA1012, and PA1212.
[0040] The third layer is composed of PA6 slices and open anti-adhesion lubricant masterbatch.
[0041] The third layer is 3 μm thick and has a smooth outer surface.
[0042] The mass ratio of the third layer: PA6 slices 90-99%, its relative viscosity is 3, open anti-adhesive lubricant masterbatch 10-1%, the mass percentage of anti-adhesive in the masterbatch is 4-6%, and the mass percentage of lubricant is 4-6%;
[0043] Step 1: After the above raw materials are mixed evenly, they are cleanly metered and added, and co-extruded through their respective extruders, metering pumps, disc filters, melt pipes, distributors and T-die heads to obtain a continuous sheet melt;
[0044] Step S2: the continuous sheet melt is rapidly cooled and formed by a chilled roller having a surface temperature of 18-25°C;
[0045] Step S3: Then, longitudinal stretching is performed. Before longitudinal stretching, the sheet is preheated by two pairs of rollers at a temperature of 40-50°C, and the first longitudinal stretching is performed under the condition that the stretching roller temperature is 50-60°C, and then both surfaces are immediately quenched by a pair of quenching rollers at a temperature of 18-25°C;
[0046] Step 4: Then, preheat the rollers at a temperature of 50-60°C for a second time, and perform longitudinal stretching for a second time under the condition that the stretching roller temperature is 50-60°C;
[0047] Step S5: Then immediately perform a second quenching on both surfaces on a pair of quenching rollers at a temperature of 18-25°C, the first longitudinal stretching multiple is 1.8, and the second longitudinal stretching multiple is 1.4;
[0048] Step S6: After longitudinal stretching, the film is then stretched transversely, with the transverse stretching multiple being 2.5-3.5 times, the transverse relaxation ratio being 8%, and the production speed being 80-160 m / min;
[0049] And the test results of BOPA composite film show that the tensile strength of BOPA film is 275-295Mpa in all directions of 360°, and the elongation at break is 130%.
[0050] Embodiment 2:
[0051] The total thickness of the aluminum-plastic film is 113um, and the total thickness of the film is 25μm. The film includes the first layer, the second layer, and the third layer;
[0052] The first layer is 3 μm thick and is in contact with the aluminum foil.
[0053] The first layer is composed of PA6 chips, which has a relative viscosity of 3.1;
[0054] The second layer is a core layer, and the second layer is a combination of PA6 slices and long carbon chain polyamide, a copolymer of long carbon chain polyamide and polyamide 6, or both;
[0055] The mass ratio of the second layer is: PA6 slices 87%, and one of the long carbon chain polyamide, the copolymer of long carbon chain polyamide and polyamide 6 or the combination of the two accounts for 13% of the total mass of the second layer;
[0056] The relative viscosity of PA6 chips is 3.7;
[0057] The long carbon chain polyamide is at least one of PA11, PA12, PA510, PA512, PA610, PA612, PA1010, PA1012, and PA1212.
[0058] The third layer is composed of PA6 slices and open anti-adhesion lubricant masterbatch.
[0059] The third layer is 4 μm thick and has a smooth outer surface.
[0060] The mass ratio of the third layer: PA6 slices 90-99%, its relative viscosity is 3.1, open anti-adhesive lubricant masterbatch 10-1%, the mass percentage of anti-adhesive in the masterbatch is 4-6%, and the mass percentage of lubricant is 4-6%;
[0061] Step 1: After the above raw materials are mixed evenly, they are cleanly metered and added, and co-extruded through their respective extruders, metering pumps, disc filters, melt pipes, distributors and T-die heads to obtain a continuous sheet melt;
[0062] Step S2: the continuous sheet melt is rapidly cooled and formed by a chilled roller having a surface temperature of 18-25°C;
[0063] Step S3: Then, longitudinal stretching is performed. Before longitudinal stretching, the sheet is preheated by two pairs of rollers at a temperature of 40-50°C, and the first longitudinal stretching is performed under the condition that the stretching roller temperature is 50-60°C, and then both surfaces are immediately quenched by a pair of quenching rollers at a temperature of 18-25°C;
[0064] Step 4: Then, preheat the rollers at a temperature of 50-60°C for a second time, and perform longitudinal stretching for a second time under the condition that the stretching roller temperature is 50-60°C;
[0065] Step S5: Then immediately perform a second quenching on both surfaces on a pair of quenching rollers at a temperature of 18-25°C, the first longitudinal stretching multiple is 1.9, and the second longitudinal stretching multiple is 1.4;
[0066] Step S6: After longitudinal stretching, the film is then stretched transversely, with the transverse stretching multiple being 2.5-3.5 times, the transverse relaxation ratio being 9%, and the production speed being 80-160 m / min.
[0067] And the test results of BOPA composite film show that the tensile strength of BOPA film is 270-301Mpa in all directions of 360°, and the elongation at break is 131%.
[0068] Embodiment three;
[0069] The total thickness of the aluminum-plastic film is 113um, and the total thickness of the film is 30μm. The film includes the first layer, the second layer, and the third layer;
[0070] The first layer is 4 μm thick and is in contact with the aluminum foil.
[0071] The first layer is composed of PA6 chips, which has a relative viscosity of 3.2;
[0072] The second layer is a core layer, and the second layer is a combination of PA6 slices and long carbon chain polyamide, a copolymer of long carbon chain polyamide and polyamide 6, or both;
[0073] The mass ratio of the second layer: PA6 slices 92%, one of the long carbon chain polyamide, the copolymer of long carbon chain polyamide and polyamide 6, or the combination of the two accounts for 8% of the total mass of the second layer;
[0074] The relative viscosity of PA6 chips is 3.9;
[0075] The long carbon chain polyamide is at least one of PA11, PA12, PA510, PA512, PA610, PA612, PA1010, PA1012, and PA1212.
[0076] The third layer is composed of PA6 slices and open anti-adhesion lubricant masterbatch.
[0077] The third layer is 5 μm thick and has a smooth outer surface.
[0078] The mass ratio of the third layer: PA6 slices 90-99%, its relative viscosity is 3.2, open anti-adhesive lubricant masterbatch 10-1%, the mass percentage of anti-adhesive in the masterbatch is 4-6%, and the mass percentage of lubricant is 4-6%;
[0079] Step 1: After the above raw materials are mixed evenly, they are cleanly metered and added, and co-extruded through their respective extruders, metering pumps, disc filters, melt pipes, distributors and T-die heads to obtain a continuous sheet melt;
[0080] Step S2: the continuous sheet melt is rapidly cooled and formed by a chilled roller having a surface temperature of 18-25°C;
[0081] Step S3: Then, longitudinal stretching is performed. Before longitudinal stretching, the sheet is preheated by two pairs of rollers at a temperature of 40-50°C, and the first longitudinal stretching is performed under the condition that the stretching roller temperature is 50-60°C, and then both surfaces are immediately quenched by a pair of quenching rollers at a temperature of 18-25°C;
[0082] Step 4: Then, preheat the rollers at a temperature of 50-60°C for a second time, and perform longitudinal stretching for a second time under the condition that the stretching roller temperature is 50-60°C;
[0083] Step S5: Then immediately perform a second rapid cooling on both surfaces on a pair of rapid cooling rollers at a temperature of 18-25°C, the first longitudinal stretching multiple is 2.0, and the second longitudinal stretching multiple is 1.4;
[0084] Step S6: After longitudinal stretching, the film is then subjected to transverse stretching, the transverse stretching multiple is 2.5-3.5 times, the transverse relaxation ratio is 10%, and the production speed is 80-160 m / min.
[0085] And the test results of BOPA composite film show that the tensile strength of BOPA film is 260-305Mpa in all directions of 360°, and the elongation at break is 135%.
[0086] Embodiment 4:
[0087] The total thickness of the aluminum-plastic film is 113um, and the total thickness of the film is 20μm. The film includes the first layer, the second layer, and the third layer;
[0088] The first layer is 4 μm thick and is in contact with the aluminum foil.
[0089] The first layer is composed of PA6 chips with a relative viscosity of 3;
[0090] The second layer is a core layer, and the second layer is a combination of PA6 slices and long carbon chain polyamide, a copolymer of long carbon chain polyamide and polyamide 6, or both;
[0091] The mass ratio of the second layer is: PA6 slices 87%, and one of the long carbon chain polyamide, the copolymer of long carbon chain polyamide and polyamide 6 or the combination of the two accounts for 13% of the total mass of the second layer;
[0092] The relative viscosity of PA6 slices is 3.5;
[0093] The long carbon chain polyamide is at least one of PA11, PA12, PA510, PA512, PA610, PA612, PA1010, PA1012, and PA1212.
[0094] The third layer is composed of PA6 slices and open anti-adhesion lubricant masterbatch.
[0095] The third layer is 3 μm thick and has a smooth outer surface.
[0096] The mass ratio of the third layer: PA6 slices 90-99%, its relative viscosity is 3, open anti-adhesive lubricant masterbatch 10-1%, the mass percentage of anti-adhesive in the masterbatch is 4-6%, and the mass percentage of lubricant is 4-6%;
[0097] Step 1: After the above raw materials are mixed evenly, they are cleanly metered and added, and co-extruded through their respective extruders, metering pumps, disc filters, melt pipes, distributors and T-die heads to obtain a continuous sheet melt;
[0098] Step S2: the continuous sheet melt is rapidly cooled and formed by a chilled roller having a surface temperature of 18-25°C;
[0099] Step S3: Then, longitudinal stretching is performed. Before longitudinal stretching, the sheet is preheated by two pairs of rollers at a temperature of 40-50°C, and the first longitudinal stretching is performed under the condition that the stretching roller temperature is 50-60°C, and then both surfaces are immediately quenched by a pair of quenching rollers at a temperature of 18-25°C;
[0100] Step 4: Then, preheat the rollers at a temperature of 50-60°C for a second time, and perform longitudinal stretching for a second time under the condition that the stretching roller temperature is 50-60°C;
[0101] Step S5: Then immediately perform a second quenching on both surfaces on a pair of quenching rollers at a temperature of 18-25°C, the first longitudinal stretching multiple is 2.0, and the second longitudinal stretching multiple is 1.5;
[0102] Step S6: After longitudinal stretching, the film is then stretched transversely, with the transverse stretching multiple being 2.5-3.5 times, the transverse relaxation ratio being 11%, and the production speed being 80-160 m / min.
[0103] And the test results of BOPA composite film show that the tensile strength of BOPA film is 259-307Mpa in all directions of 360°, and the elongation at break is 125%.
[0104] Embodiment five;
[0105] The total thickness of the aluminum-plastic film is 113um, and the total thickness of the film is 25μm. The film includes the first layer, the second layer, and the third layer;
[0106] The first layer is 3 μm thick and is in contact with the aluminum foil.
[0107] The first layer is composed of PA6 chips, which has a relative viscosity of 3.1;
[0108] The second layer is a core layer, and the second layer is a combination of PA6 slices and long carbon chain polyamide, a copolymer of long carbon chain polyamide and polyamide 6, or both;
[0109] The mass ratio of the second layer: PA6 slices 82%, one of the long carbon chain polyamide, the copolymer of long carbon chain polyamide and polyamide 6 or the combination of the two accounts for 18% of the total mass of the second layer;
[0110] The relative viscosity of PA6 chips is 3.7;
[0111] The long carbon chain polyamide is at least one of PA11, PA12, PA510, PA512, PA610, PA612, PA1010, PA1012, and PA1212.
[0112] The third layer is composed of PA6 slices and open anti-adhesion lubricant masterbatch.
[0113] The third layer is 4 μm thick and has a smooth outer surface.
[0114] The mass ratio of the third layer: PA6 slices 90-99%, its relative viscosity is 3.1, open anti-adhesive lubricant masterbatch 10-1%, the mass percentage of anti-adhesive in the masterbatch is 4-6%, and the mass percentage of lubricant is 4-6%;
[0115] Step 1: After the above raw materials are mixed evenly, they are cleanly metered and added, and co-extruded through their respective extruders, metering pumps, disc filters, melt pipes, distributors and T-die heads to obtain a continuous sheet melt;
[0116] Step S2: the continuous sheet melt is rapidly cooled and formed by a chilled roller having a surface temperature of 18-25°C;
[0117] Step S3: Then, longitudinal stretching is performed. Before longitudinal stretching, the sheet is preheated by two pairs of rollers at a temperature of 40-50°C, and the first longitudinal stretching is performed under the condition that the stretching roller temperature is 50-60°C, and then both surfaces are immediately quenched by a pair of quenching rollers at a temperature of 18-25°C;
[0118] Step 4: Then, preheat the rollers at a temperature of 50-60°C for a second time, and perform longitudinal stretching for a second time under the condition that the stretching roller temperature is 50-60°C;
[0119] Step S5: Then immediately perform a second quenching on both surfaces on a pair of quenching rollers at a temperature of 18-25°C, the first longitudinal stretching multiple is 2.0, and the second longitudinal stretching multiple is 1.3;
[0120] Step S6: After longitudinal stretching, the film is then stretched transversely, with the transverse stretching multiple being 2.5-3.5 times, the transverse relaxation ratio being 12%, and the production speed being 80-160 m / min.
[0121] And the test results of BOPA composite film show that the tensile strength of BOPA film is 268-300Mpa in all directions of 360°, and the elongation at break is 120%.
[0122] Embodiment six;
[0123] The total thickness of the aluminum-plastic film is 113um, and the total thickness of the film is 30μm. The film includes the first layer, the second layer, and the third layer;
[0124] The first layer is 2 μm thick and is in contact with the aluminum foil.
[0125] The first layer is composed of PA6 chips, which has a relative viscosity of 3.2;
[0126] The second layer is a core layer, and the second layer is a combination of PA6 slices and long carbon chain polyamide, a copolymer of long carbon chain polyamide and polyamide 6, or both;
[0127] The mass ratio of the second layer: PA6 slices 92%, one of the long carbon chain polyamide, the copolymer of long carbon chain polyamide and polyamide 6, or the combination of the two accounts for 8% of the total mass of the second layer;
[0128] The relative viscosity of PA6 chips is 3.9;
[0129] The long carbon chain polyamide is at least one of PA11, PA12, PA510, PA512, PA610, PA612, PA1010, PA1012, and PA1212.
[0130] The third layer is composed of PA6 slices and open anti-adhesion lubricant masterbatch.
[0131] The third layer is 5 μm thick and has a smooth outer surface.
[0132] The mass ratio of the third layer: PA6 slices 90-99%, its relative viscosity is 3.2, open anti-adhesive lubricant masterbatch 10-1%, the mass percentage of anti-adhesive in the masterbatch is 4-6%, and the mass percentage of lubricant is 4-6%;
[0133] Step 1: After the above raw materials are mixed evenly, they are cleanly metered and added, and co-extruded through their respective extruders, metering pumps, disc filters, melt pipes, distributors and T-die heads to obtain a continuous sheet melt;
[0134] Step S2: the continuous sheet melt is rapidly cooled and formed by a chilled roller having a surface temperature of 18-25°C;
[0135] Step S3: Then, longitudinal stretching is performed. Before longitudinal stretching, the sheet is preheated by two pairs of rollers at a temperature of 40-50°C, and the first longitudinal stretching is performed under the condition that the stretching roller temperature is 50-60°C, and then both surfaces are immediately quenched by a pair of quenching rollers at a temperature of 18-25°C;
[0136] Step 4: Then, preheat the rollers at a temperature of 50-60°C for a second time, and perform longitudinal stretching for a second time under the condition that the stretching roller temperature is 50-60°C;
[0137] Step S5: Then immediately perform a second quenching on both surfaces on a pair of quenching rollers at a temperature of 18-25°C, the first longitudinal stretching multiple is 1.9, and the second longitudinal stretching multiple is 1.5;
[0138] Step S6: After longitudinal stretching, the film is then subjected to transverse stretching, the transverse stretching multiple is 2.5-3.5 times, the transverse relaxation ratio is 13%, and the production speed is 80-160 m / min.
[0139] The test results of BOPA composite film show that the tensile strength of BOPA film is 285-297Mpa in all directions of 360° and the elongation at break is 119%.
[0140] Embodiment seven;
[0141] The total thickness of the aluminum-plastic film is 113um, and the total thickness of the film is 20μm. The film includes the first layer, the second layer, and the third layer;
[0142] The first layer is 3 μm thick and is in contact with the aluminum foil.
[0143] The first layer is composed of PA6 chips with a relative viscosity of 3;
[0144] The second layer is a core layer, and the second layer is a combination of PA6 slices and long carbon chain polyamide, a copolymer of long carbon chain polyamide and polyamide 6, or both;
[0145] The mass ratio of the second layer: PA6 slices 92%, one of the long carbon chain polyamide, the copolymer of long carbon chain polyamide and polyamide 6, or the combination of the two accounts for 8% of the total mass of the second layer;
[0146] The relative viscosity of PA6 chips is 3.9;
[0147] The long carbon chain polyamide is at least one of PA11, PA12, PA510, PA512, PA610, PA612, PA1010, PA1012, and PA1212.
[0148] The third layer is composed of PA6 slices and open anti-adhesion lubricant masterbatch.
[0149] The third layer is 3 μm thick and has a smooth outer surface.
[0150] The mass ratio of the third layer: PA6 slices 90-99%, its relative viscosity is 3, open anti-adhesive lubricant masterbatch 10-1%, the mass percentage of anti-adhesive in the masterbatch is 4-6%, and the mass percentage of lubricant is 4-6%;
[0151] Step 1: After the above raw materials are mixed evenly, they are cleanly metered and added, and co-extruded through their respective extruders, metering pumps, disc filters, melt pipes, distributors and T-die heads to obtain a continuous sheet melt;
[0152] Step S2: the continuous sheet melt is rapidly cooled and formed by a chilled roller having a surface temperature of 18-25°C;
[0153] Step S3: Then, longitudinal stretching is performed. Before longitudinal stretching, the sheet is preheated by two pairs of rollers at a temperature of 40-50°C, and the first longitudinal stretching is performed under the condition that the stretching roller temperature is 50-60°C, and then both surfaces are immediately quenched by a pair of quenching rollers at a temperature of 18-25°C;
[0154] Step 4: Then, preheat the rollers at a temperature of 50-60°C for a second time, and perform longitudinal stretching for a second time under the condition that the stretching roller temperature is 50-60°C;
[0155] Step S5: Then immediately perform a second quenching on both surfaces on a pair of quenching rollers at a temperature of 18-25°C, the first longitudinal stretching multiple is 1.8, and the second longitudinal stretching multiple is 1.4;
[0156] Step S6: After longitudinal stretching, the film is then subjected to transverse stretching, the transverse stretching multiple is 2.5-3.5 times, the transverse relaxation ratio is 13%, and the production speed is 80-160 m / min.
[0157] And the test results of BOPA composite film show that the tensile strength of BOPA film is 296-305Mpa in all directions of 360°, and the elongation at break is 124%.
[0158] Embodiment eight;
[0159] The total thickness of the aluminum-plastic film is 113um, and the total thickness of the film is 25μm. The film includes the first layer, the second layer, and the third layer;
[0160] The first layer is 2 μm thick and is in contact with the aluminum foil.
[0161] The first layer is composed of PA6 chips, which has a relative viscosity of 3.1;
[0162] The second layer is a core layer, and the second layer is a combination of PA6 slices and long carbon chain polyamide, a copolymer of long carbon chain polyamide and polyamide 6, or both;
[0163] The mass ratio of the second layer: PA6 slices 82%, one of the long carbon chain polyamide, the copolymer of long carbon chain polyamide and polyamide 6 or the combination of the two accounts for 18% of the total mass of the second layer;
[0164] The relative viscosity of PA6 chips is 3.7;
[0165] The long carbon chain polyamide is at least one of PA11, PA12, PA510, PA512, PA610, PA612, PA1010, PA1012, and PA1212.
[0166] The third layer is composed of PA6 slices and open anti-adhesion lubricant masterbatch.
[0167] The third layer is 4 μm thick and has a smooth outer surface.
[0168] The mass ratio of the third layer: PA6 slices 90-99%, its relative viscosity is 3.1, open anti-adhesive lubricant masterbatch 10-1%, the mass percentage of anti-adhesive in the masterbatch is 4-6%, and the mass percentage of lubricant is 4-6%;
[0169] Step 1: After the above raw materials are mixed evenly, they are cleanly metered and added, and co-extruded through their respective extruders, metering pumps, disc filters, melt pipes, distributors and T-die heads to obtain a continuous sheet melt;
[0170] Step S2: the continuous sheet melt is rapidly cooled and formed by a chilled roller having a surface temperature of 18-25°C;
[0171] Step S3: Then, longitudinal stretching is performed. Before longitudinal stretching, the sheet is preheated by two pairs of rollers at a temperature of 40-50°C, and the first longitudinal stretching is performed under the condition that the stretching roller temperature is 50-60°C, and then both surfaces are immediately quenched by a pair of quenching rollers at a temperature of 18-25°C;
[0172] Step 4: Then, preheat the rollers at a temperature of 50-60°C for a second time, and perform longitudinal stretching for a second time under the condition that the stretching roller temperature is 50-60°C;
[0173] Step S5: Then immediately perform a second quenching on both surfaces on a pair of quenching rollers at a temperature of 18-25°C, the first longitudinal stretching multiple is 1.9, and the second longitudinal stretching multiple is 1.4;
[0174] Step S6: After longitudinal stretching, the film is then stretched transversely, with the transverse stretching multiple being 2.5-3.5 times, the transverse relaxation ratio being 12%, and the production speed being 80-160 m / min.
[0175] And the test results of BOPA composite film show that the tensile strength of BOPA film is 267-287Mpa in all directions of 360°, and the elongation at break is 123%.
[0176] Embodiment 9:
[0177] The total thickness of the aluminum-plastic film is 113um, and the total thickness of the film is 30μm. The film includes the first layer, the second layer, and the third layer;
[0178] The first layer is 4 μm thick and is in contact with the aluminum foil.
[0179] The first layer is composed of PA6 chips, which has a relative viscosity of 3.2;
[0180] The second layer is a core layer, and the second layer is a combination of PA6 slices and long carbon chain polyamide, a copolymer of long carbon chain polyamide and polyamide 6, or both;
[0181] The mass ratio of the second layer is: PA6 slices 87%, and one of the long carbon chain polyamide, the copolymer of long carbon chain polyamide and polyamide 6 or the combination of the two accounts for 13% of the total mass of the second layer;
[0182] The relative viscosity of PA6 slices is 3.5;
[0183] The long carbon chain polyamide is at least one of PA11, PA12, PA510, PA512, PA610, PA612, PA1010, PA1012, and PA1212.
[0184] The third layer is composed of PA6 slices and open anti-adhesion lubricant masterbatch.
[0185] The third layer is 5 μm thick and has a smooth outer surface.
[0186] The mass ratio of the third layer: PA6 slices 90-99%, its relative viscosity is 3.2, open anti-adhesive lubricant masterbatch 10-1%, the mass percentage of anti-adhesive in the masterbatch is 4-6%, and the mass percentage of lubricant is 4-6%;
[0187] Step 1: After the above raw materials are mixed evenly, they are cleanly metered and added, and co-extruded through their respective extruders, metering pumps, disc filters, melt pipes, distributors and T-die heads to obtain a continuous sheet melt;
[0188] Step S2: the continuous sheet melt is rapidly cooled and formed by a chilled roller having a surface temperature of 18-25°C;
[0189] Step S3: Then, longitudinal stretching is performed. Before longitudinal stretching, the sheet is preheated by two pairs of rollers at a temperature of 40-50°C, and the first longitudinal stretching is performed under the condition that the stretching roller temperature is 50-60°C, and then both surfaces are immediately quenched by a pair of quenching rollers at a temperature of 18-25°C;
[0190] Step 4: Then, preheat the rollers at a temperature of 50-60°C for a second time, and perform longitudinal stretching for a second time under the condition that the stretching roller temperature is 50-60°C;
[0191] Step S5: Then immediately perform a second rapid cooling on both surfaces on a pair of rapid cooling rollers at a temperature of 18-25°C, the first longitudinal stretching multiple is 2.0, and the second longitudinal stretching multiple is 1.4;
[0192] Step S6: After longitudinal stretching, the film is then stretched transversely, with the transverse stretching multiple being 2.5-3.5 times, the transverse relaxation ratio being 11%, and the production speed being 80-160 m / min.
[0193] And the test results of BOPA composite film show that the tensile strength of BOPA film is 267-298Mpa in all directions of 360°, and the elongation at break is 135%.
[0194] Embodiment ten;
[0195] The total thickness of the aluminum-plastic film is 113um, and the total thickness of the film is 20μm. The film includes the first layer, the second layer, and the third layer;
[0196] The first layer is 2 μm thick and is in contact with the aluminum foil.
[0197] The first layer is composed of PA6 chips with a relative viscosity of 3;
[0198] The second layer is a core layer, and the second layer is a combination of PA6 slices and long carbon chain polyamide, a copolymer of long carbon chain polyamide and polyamide 6, or both;
[0199] The mass ratio of the second layer: PA6 slices 82%, one of the long carbon chain polyamide, the copolymer of long carbon chain polyamide and polyamide 6 or the combination of the two accounts for 18% of the total mass of the second layer;
[0200] The relative viscosity of PA6 slices is 3.5;
[0201] The long carbon chain polyamide is at least one of PA11, PA12, PA510, PA512, PA610, PA612, PA1010, PA1012, and PA1212.
[0202] The third layer is composed of PA6 slices and open anti-adhesion lubricant masterbatch.
[0203] The third layer is 5 μm thick and has a smooth outer surface.
[0204] The mass ratio of the third layer: PA6 slices 90-99%, its relative viscosity is 3, open anti-adhesive lubricant masterbatch 10-1%, the mass percentage of anti-adhesive in the masterbatch is 4-6%, and the mass percentage of lubricant is 4-6%;
[0205] Step 1: After the above raw materials are mixed evenly, they are cleanly metered and added, and co-extruded through their respective extruders, metering pumps, disc filters, melt pipes, distributors and T-die heads to obtain a continuous sheet melt;
[0206] Step S2: the continuous sheet melt is rapidly cooled and formed by a chilled roller having a surface temperature of 18-25°C;
[0207] Step S3: Then, longitudinal stretching is performed. Before longitudinal stretching, the sheet is preheated by two pairs of rollers at a temperature of 40-50°C, and the first longitudinal stretching is performed under the condition that the stretching roller temperature is 50-60°C, and then both surfaces are immediately quenched by a pair of quenching rollers at a temperature of 18-25°C;
[0208] Step 4: Then, preheat the rollers at a temperature of 50-60°C for a second time, and perform longitudinal stretching for a second time under the condition that the stretching roller temperature is 50-60°C;
[0209] Step S5: Then immediately perform a second quenching on both surfaces on a pair of quenching rollers at a temperature of 18-25°C, the first longitudinal stretching multiple is 2.0, and the second longitudinal stretching multiple is 1.5;
[0210] Step S6: After longitudinal stretching, the film is then subjected to transverse stretching, the transverse stretching multiple is 2.5-3.5 times, the transverse relaxation ratio is 10%, and the production speed is 80-160 m / min.
[0211] And the test results of BOPA composite film show that the tensile strength of BOPA film is 264-301Mpa in all directions of 360°, and the elongation at break is 139%.
[0212] Embodiment eleven;
[0213] The total thickness of the aluminum-plastic film is 113um, and the total thickness of the film is 25μm. The film includes the first layer, the second layer, and the third layer;
[0214] The first layer is 3 μm thick and is in contact with the aluminum foil.
[0215] The first layer is composed of PA6 chips, which has a relative viscosity of 3.1;
[0216] The second layer is a core layer, and the second layer is a combination of PA6 slices and long carbon chain polyamide, a copolymer of long carbon chain polyamide and polyamide 6, or both;
[0217] The mass ratio of the second layer: PA6 slices 92%, one of the long carbon chain polyamide, the copolymer of long carbon chain polyamide and polyamide 6, or the combination of the two accounts for 8% of the total mass of the second layer;
[0218] The relative viscosity of PA6 chips is 3.9;
[0219] The long carbon chain polyamide is at least one of PA11, PA12, PA510, PA512, PA610, PA612, PA1010, PA1012, and PA1212.
[0220] The third layer is composed of PA6 slices and open anti-adhesion lubricant masterbatch.
[0221] The third layer is 4 μm thick and has a smooth outer surface.
[0222] The mass ratio of the third layer: PA6 slices 90-99%, its relative viscosity is 3.1, open anti-adhesive lubricant masterbatch 10-1%, the mass percentage of anti-adhesive in the masterbatch is 4-6%, and the mass percentage of lubricant is 4-6%;
[0223] Step 1: After the above raw materials are mixed evenly, they are cleanly metered and added, and co-extruded through their respective extruders, metering pumps, disc filters, melt pipes, distributors and T-die heads to obtain a continuous sheet melt;
[0224] Step S2: the continuous sheet melt is rapidly cooled and formed by a chilled roller having a surface temperature of 18-25°C;
[0225] Step S3: Then, longitudinal stretching is performed. Before longitudinal stretching, the sheet is preheated by two pairs of rollers at a temperature of 40-50°C, and the first longitudinal stretching is performed under the condition that the stretching roller temperature is 50-60°C, and then both surfaces are immediately quenched by a pair of quenching rollers at a temperature of 18-25°C;
[0226] Step 4: Then, preheat the rollers at a temperature of 50-60°C for a second time, and perform longitudinal stretching for a second time under the condition that the stretching roller temperature is 50-60°C;
[0227] Step S5: Then immediately perform a second quenching on both surfaces on a pair of quenching rollers at a temperature of 18-25°C, the first longitudinal stretching multiple is 2.0, and the second longitudinal stretching multiple is 1.3;
[0228] Step S6: After longitudinal stretching, the film is then stretched transversely, with the transverse stretching multiple being 2.5-3.5 times, the transverse relaxation ratio being 9%, and the production speed being 80-160 m / min.
[0229] And the test results of BOPA composite film show that the tensile strength of BOPA film is 261-302Mpa in all directions of 360°, and the elongation at break is 140%.
[0230] Embodiment 12:
[0231] The total thickness of the aluminum-plastic film is 113um, and the total thickness of the film is 30μm. The film includes the first layer, the second layer, and the third layer;
[0232] The first layer is 4 μm thick and is in contact with the aluminum foil.
[0233] The first layer is composed of PA6 chips, which has a relative viscosity of 3.2;
[0234] The second layer is a core layer, and the second layer is a combination of PA6 slices and long carbon chain polyamide, a copolymer of long carbon chain polyamide and polyamide 6, or both;
[0235] The mass ratio of the second layer is: PA6 slices 87%, and one of the long carbon chain polyamide, the copolymer of long carbon chain polyamide and polyamide 6 or the combination of the two accounts for 13% of the total mass of the second layer;
[0236] The relative viscosity of PA6 chips is 3.7;
[0237] The long carbon chain polyamide is at least one of PA11, PA12, PA510, PA512, PA610, PA612, PA1010, PA1012, and PA1212.
[0238] The third layer is composed of PA6 slices and open anti-adhesion lubricant masterbatch.
[0239] The third layer is 3 μm thick and has a smooth outer surface.
[0240] The mass ratio of the third layer: PA6 slices 90-99%, its relative viscosity is 3.2, open anti-adhesive lubricant masterbatch 10-1%, the mass percentage of anti-adhesive in the masterbatch is 4-6%, and the mass percentage of lubricant is 4-6%;
[0241] Step 1: After the above raw materials are mixed evenly, they are cleanly metered and added, and co-extruded through their respective extruders, metering pumps, disc filters, melt pipes, distributors and T-die heads to obtain a continuous sheet melt;
[0242] Step S2: the continuous sheet melt is rapidly cooled and formed by a chilled roller having a surface temperature of 18-25°C;
[0243] Step S3: Then, longitudinal stretching is performed. Before longitudinal stretching, the sheet is preheated by two pairs of rollers at a temperature of 40-50°C, and the first longitudinal stretching is performed under the condition that the stretching roller temperature is 50-60°C, and then both surfaces are immediately quenched by a pair of quenching rollers at a temperature of 18-25°C;
[0244] Step 4: Then, preheat the rollers at a temperature of 50-60°C for a second time, and perform longitudinal stretching for a second time under the condition that the stretching roller temperature is 50-60°C;
[0245] Step S5: Then immediately perform a second quenching on both surfaces on a pair of quenching rollers at a temperature of 18-25°C, the first longitudinal stretching multiple is 1.9, and the second longitudinal stretching multiple is 1.5;
[0246] Step S6: After longitudinal stretching, the film is then subjected to transverse stretching, the transverse stretching multiple is 2.5-3.5 times, the transverse relaxation ratio is 8%, and the production speed is 80-160 m / min.
[0247] And the test results of BOPA composite film show that the tensile strength of BOPA film is 259-305Mpa in all directions of 360°, and the elongation at break is 127%.
[0248] The above shows and describes the basic principle, main features and advantages of the present invention, and the standard parts used in the present invention can be purchased from the market, and special-shaped parts can be customized according to the description in the specification and the drawings. The specific connection methods of each part adopt the conventional means such as mature bolts, rivets, welding, etc. in the prior art. The machinery, parts and equipment all adopt the conventional models in the prior art, and the circuit connection adopts the conventional connection method in the prior art, which will not be described in detail here.
[0249] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A modified polyamide composite film, the total thickness of which is 15-30 μm, the film comprising a first layer, a second layer, and a third layer; Features: The first layer is 2-4 μm thick and is a composite layer with aluminum foil; The first layer is composed of PA6 chips, with a relative viscosity of 3.0-3.2; The second layer is a core layer, and the second layer is a combination of PA6 slices and long carbon chain polyamide, a copolymer of long carbon chain polyamide and polyamide 6, or both; The third layer is composed of PA6 slices and open anti-adhesion lubricant masterbatch.
2. A modified polyamide composite film according to claim 1, characterized in that: Second layer quality ratio; PA6 slices 80-95%, one of long carbon chain polyamide, copolymer of long carbon chain polyamide and polyamide 6 or a combination of both accounts for 20-5% of the total mass of the second layer; The relative viscosity of PA6 chips is 3.4-4.0; The long carbon chain polyamide is at least one of PA11, PA12, PA510, PA512, PA610, PA612, PA1010, PA1012, and PA1212.
3. A modified polyamide composite film according to claim 2, characterized in that: The third layer is 3-6 μm thick and is the outermost surface, which is the smooth surface. The mass ratio of the third layer is: PA6 slice 90-99%, its relative viscosity is 3.0-3.2, open anti-adhesion lubricant masterbatch 10-1%, the mass percentage of anti-adhesion agent in the masterbatch is 4-6%, and the mass percentage of lubricant is 4-6%.
4. The process for preparing a modified polyamide composite film according to claim 3, characterized in that: The steps include: Step S1: After various raw materials of each layer are mixed uniformly according to the formula, they are cleanly metered and added, and co-extruded through respective extruders, metering pumps, disc filters, melt pipes, distributors and T-die heads to obtain continuous sheet melt; Step S2: the continuous sheet melt is rapidly cooled and formed by a chilled roller having a surface temperature of 18-25°C; Step S3: Then, longitudinal stretching is performed. Before longitudinal stretching, the sheet is preheated by two pairs of rollers at a temperature of 40-50°C, and the first longitudinal stretching is performed under the condition that the stretching roller temperature is 50-60°C, and then both surfaces are immediately quenched by a pair of quenching rollers at a temperature of 18-25°C; Step 4: Then, preheat the rollers at a temperature of 50-60°C for a second time, and perform longitudinal stretching for a second time under the condition that the stretching roller temperature is 50-60°C; Step S5: Then immediately perform a second quenching on both surfaces on a pair of quenching rollers at a temperature of 18-25°C, the first longitudinal stretching multiple is 1.8-2.4, the second longitudinal stretching multiple is 1.4-2, and the total longitudinal stretching multiple of the two longitudinal stretching multiples is 2.5-3.5; Step S6: After longitudinal stretching, the film is then stretched transversely, with the transverse stretching multiple being 2.5-3.5 times, the transverse relaxation ratio being 7-13%, and the production speed being 80-160 m / min.
5. The process for preparing a modified polyamide composite film according to claim 4, characterized in that: The extruder, metering pump, disc filter, melt pipe, distributor and T-die in step S1 are set at a temperature of 215-300°C.
Citation Information
Patent Citations
Stretched polyamide film
CN103402737A
Biaxial stretching polyamide film master batch and film as well as preparation method of polyamide film master batch and film
CN103554901A
BOPA heat conduction film and preparation method thereof
CN106379018A
Special nylon film for aluminum-plastic film and manufacture method thereof
CN107471801A
Polyamide laminated film for lithium ion secondary battery exterior