Resin composition, preparation method thereof, layer-adding adhesive film and application
Through the combination of cross-linked polymer resin, epoxy resin and inorganic fillers, the problem of high dielectric loss of the build-up adhesive film is solved, low dielectric loss and good mechanical properties are achieved, and the signal transmission efficiency is improved.
Patent Information
- Application Number
- CN202310452626.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-17
- Publication Date
- 2024-10-22
AI Technical Summary
The dielectric loss of the build-up adhesive film prepared from the existing resin composition material is relatively high, resulting in signal transmission delay and power loss, which affects its application in high-end semiconductor packaging carrier boards.
A combination of cross-linked polymer resin, epoxy resin, curing agent and inorganic filler is used to form a low dielectric loss resin composition through cross-linking reaction, reducing or eliminating the need to add high dielectric loss thermoplastic polymer resin, improving the Film-forming properties and mechanical properties of resin.
It achieves ultra-low dielectric loss, good lamination properties and dimensional stability of the build-up adhesive film, avoids signal transmission delay and power loss, and improves signal transmission efficiency.
Smart Images

Figure CN118812969A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of polymer materials, and in particular relates to a resin composition and a preparation method thereof, a build-up adhesive film and applications thereof. Background Art
[0002] Electronic packaging is an indispensable process after the production of integrated circuit chips, and it is a bridge from device to system. The packaging production link has a great impact on the quality and competitiveness of microelectronic products. Chip packaging is a process that uses film technology and micro-machining technology to arrange, paste, fix and connect chips and other elements on a frame or substrate, lead out the wiring terminals and fix them through plastic insulating medium to form an overall structure. Electronic packaging engineering is to connect and assemble elements such as substrates, chip packages and discrete devices according to the requirements of electronic complete machines, achieve certain electrical and physical properties, and transform them into complete devices or equipment in the form of complete machines or systems.
[0003] IC package substrate is a type of functional copper-clad board that emerged with the development of BGA (ball grid array) packaging technology. It can provide physical support and circuit connectivity for IC chips. It is an intermediate product connecting chips and circuit boards. It expands the number of chip pins per unit area, which is conducive to improving chip performance and reducing the manufacturing cost of IC packaging. IC package substrate is also a key material for new packaging forms such as CSP (chip scale package) and FC-BGA (Flip Chip Ball Grid Array). As one of the key core insulating dielectric materials for packaging substrates, the dielectric loss of the build-up film material has a crucial impact on the entire insertion loss of the board. The technical key and development bottleneck of the build-up film material lies in the resin composition material used to prepare the build-up film. In order to meet the technical development requirements of miniaturization, high density and high frequency, the resin composition material used in the build-up film must have many requirements such as low dielectric constant and low dielectric loss. The development of a build-up film material with lower dielectric loss is the core path to reduce signal transmission loss and has great value.
[0004] At present, the resin composition material for preparing the build-up film is usually a combination of an epoxy thermosetting system formula and a free radical polymerization type low molecular weight resin by some method, and the low dielectric loss characteristics of the free radical polymerization type resin are used to reduce the dielectric loss of the entire formula system. However, the introduction of free radical polymerization resin on the basis of the epoxy system has limited reduction in the dielectric tangent value (Df). This is because: on the one hand, the dielectric loss of the free radical polymerization type low molecular weight resin itself is not low enough, and the dielectric loss of the film material is not significantly reduced; on the other hand, this technology inevitably requires additional addition of thermoplastic polymer resin as a film-forming agent to make the film material prepared by the resin formula have a certain flexibility, but the dielectric loss of these additionally added thermoplastic polymer resins is relatively high, which is not conducive to reducing the dielectric loss of the build-up film material. Therefore, the dielectric tangent value (Df) of the build-up film prepared by the existing resin composition is still large, and the build-up film material still has the problem of insufficient dielectric performance. However, the dielectric loss of the build-up film is large, which easily causes transmission delay for voltage signals (i.e., RC delay effect), thereby causing adverse effects such as signal transmission delay power loss, which seriously affects its application in high-end semiconductor packaging substrates. Therefore, it is particularly important to develop a resin composition with low dielectric loss and a build-up film. Summary of the invention
[0005] The purpose of the present application is to provide a resin composition and a preparation method thereof, a build-up adhesive film, a packaging carrier, and an electronic device, aiming to solve the problem of high dielectric loss of the build-up adhesive film prepared from existing resin composition materials.
[0006] In order to achieve the above application purpose, the technical solution adopted in this application is as follows:
[0007] The first aspect of the present application provides a resin composition, which comprises components: a cross-linked polymer resin, an epoxy resin, a curing agent and an inorganic filler; wherein the cross-linked polymer resin comprises at least one of the following chemical structural formulas I:
[0008] Formula I; substituents R1 to R9 are independently selected from one of hydrogen atom, alkyl, alkoxy, ester group or aromatic group, R10 is selected from one of hydrogen atom, benzocyclobutene, alkyl, alkoxy, ester group and aromatic group, n is a positive integer of 4 to 1000, m is a positive integer of 0 to 1000, and n+m is a positive integer not less than 5.
[0009] In the resin composition provided by the embodiment of the present application, the cross-linked polymer resin is a resin formed by copolymerization of divinylbenzene and its derivatives with olefins and their derivatives, and the resin of the specific chemical structure has a relatively low overall molecular structure polarity, and polar groups are not produced after cross-linking, so that the product after the resin is cured has ultra-low loss characteristics, and the dielectric loss of the product after the resin composition is cured can be significantly reduced. And this type of resin contains functional groups such as reactive double bonds, which can react under cross-linking conditions to form a cross-linked network, thereby improving the cured film-forming properties of the resin composition. At the same time, it has a higher molecular weight, so that the resin composition has good film-forming properties, reducing or even without the need to add a thermoplastic polymer resin with high dielectric loss as a film-forming agent in the resin composition, so as to better ensure that the product after the resin composition is cured has ultra-low dielectric loss. In addition, epoxy resin and curing agent ensure the degumming performance and toughness of the product after the resin composition is cured with low dielectric loss, and inorganic fillers ensure the mechanical properties and dimensional stability of the resin composition and its cured product with low dielectric loss. Therefore, the resin composition has excellent curing film-forming performance through the joint action of various raw material components. The layered adhesive film formed after film formation has good lamination and debonding properties. The product of the layered adhesive film after curing has ultra-low dielectric loss, excellent dimensional stability, and suitable mechanical properties. It is particularly suitable as an insulating dielectric material for a carrier board. Its ultra-low dielectric loss characteristics can effectively avoid the adverse effects of voltage signal transmission delay and signal transmission delay power loss caused by insufficient dielectric performance, thereby improving the migration and transmission efficiency of the signal.
[0010] As a possible implementation of the resin composition of the present application, the R1 to R9 are independently selected from a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, an ester group having 1 to 10 carbon atoms, and an aromatic group having 6 to 12 carbon atoms;
[0011] As a possible implementation of the resin composition of the present application, the R10 is selected from a hydrogen atom, benzocyclobutene, an alkyl group with 1 to 10 carbon atoms, an alkoxy group with 1 to 10 carbon atoms, an ester group with 1 to 10 carbon atoms, and an aromatic group with 6 to 12 carbon atoms.
[0012] In this case, by selecting and matching the substituents R1 to R10 in the chemical structure I of the cross-linked polymer resin, the cross-linked polymer resin can contain functional groups such as double bonds and benzocyclobutene, which is more conducive to improving the curing and film-forming properties of the resin. It is also conducive to reducing the polarity of the resin and its cross-linked product, and achieving low dielectric loss of the cured product.
[0013] As a possible implementation of the resin composition of the present application, the cross-linked polymer resin includes benzocyclobutene resin and / or divinylbenzene resin; wherein the chemical structure of the benzocyclobutene resin is Formula I-1; the chemical structural formula of the divinylbenzene resin is Formula I-2 In this case, the benzocyclobutene resin and the divinylbenzene resin contain double bonds and / or functional groups such as benzocyclobutene, which can react under crosslinking conditions to form a crosslinked network structure, and have a better curing film-forming effect.
[0014] As a possible implementation method of the resin composition of the present application, the benzocyclobutene resin is selected from In this case, the benzocyclobutene resins of these specific structures contain double bonds and functional groups such as benzocyclobutene, which can react under crosslinking conditions to form a crosslinked network structure and have a good curing film-forming effect.
[0015] As a possible implementation method of the resin composition of the present application, the divinylbenzene resin is selected from At least one of the following, wherein a is a positive integer of 4 to 1000, b is a positive integer of 0 to 100, c is a positive integer of 0 to 1000, and d is a positive integer of 0 to 1000. In this case, the divinylbenzene resins of these specific structures contain multiple double bonds and have good curing film-forming effects under crosslinking conditions.
[0016] As a possible implementation of the resin composition of the present application, the weight average molecular weight of the cross-linked polymer resin is 1000 to 1000000. In this case, the cross-linked polymer resin has a relatively high molecular weight, and the high molecular weight resin is conducive to winding with other small molecular weight components during film formation, so that the layered film formed after the resin film formation has a certain flexibility and is not easy to break when the film is used.
[0017] As a possible implementation of the resin composition of the present application, the weight average molecular weight of the cross-linked polymer resin is 2000 to 100000. The cross-linked polymer resin within this weight average molecular weight range can better improve the film-forming performance of the resin composition, ensure the lamination of the build-up film formed after film formation, and reduce the dielectric loss of the product after the resin composition is cured.
[0018] As a possible implementation of the resin composition of the present application, in the resin composition, the mass ratio of the cross-linked polymer resin, the epoxy resin and the curing agent is (20-90): (5-60): (5-60). In this case, in the resin composition, the cross-linked polymer resin, the epoxy resin and the curing agent are non-volatile components, and the formula ratio of the three components simultaneously ensures the high film-forming performance of the resin composition, the good lamination and debonding properties of the build-up film after film formation, and the low dielectric loss after curing.
[0019] As a possible implementation of the resin composition of the present application, in the resin composition, the mass ratio of the total mass of the cross-linked polymer resin, the epoxy resin and the curing agent to the mass ratio of the inorganic filler is 1:(1-9). In this case, the content of the inorganic filler in the resin composition fully ensures the mechanical properties such as toughness and dimensional stability of the product after the resin composition is cured.
[0020] As a possible implementation of the resin composition of the present application, the curing agent includes at least one of phenols, cyanates, benzoxazines, carbodiimides, and active esters. These curing agents can make the resin in the resin composition better cross-linked and cured to form a film material.
[0021] As a possible implementation of the resin composition of the present application, the curing agent is selected from at least one of phenols, cyanates, and active esters modified with at least one functional group of a double bond or a benzocyclobutenyl group. In this case, the curing agent such as phenols, cyanates, and active esters may further contain at least one functional group of a double bond or a benzocyclobutenyl group, and while curing the epoxy resin, it may also react with the cross-linking resin, thereby being more conducive to improving the film-forming performance of the resin composition.
[0022] As a possible implementation of the resin composition of the present application, the average particle size of the inorganic filler is 0.01 to 10 μm. In this case, the inorganic filler is beneficial to improving the mechanical strength and other properties of the product after the resin composition is cured.
[0023] As a possible implementation of the resin composition of the present application, the surface of the inorganic filler is treated with at least one coupling agent selected from aminosilanes, epoxysilanes, double-bond silanes, mercaptosilanes, silanes, and titanates. In this case, by treating the surface of the inorganic filler, the surface is changed from hydrophilic to hydrophobic or has a functional group that can react with the resin, thereby improving the compatibility and bonding strength of the inorganic filler with the resin.
[0024] As a possible implementation of the resin composition of the present application, the inorganic filler includes at least one of silicon dioxide, aluminum oxide, glass, cordierite, silicon oxide, barium sulfate, barium carbonate, talc, clay, mica powder, zinc oxide, hydrotalcite, boehmite, aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, magnesium oxide, boron nitride, aluminum nitride, manganese nitride, aluminum borate, strontium carbonate, strontium titanate, calcium titanate, magnesium titanate, bismuth titanate, titanium oxide, zirconium oxide, barium titanate, barium zirconate, barium zirconate, calcium zirconate, zirconium phosphate, and zirconium tungstate phosphate. These inorganic fillers are added to the resin composition to improve the mechanical properties, dimensional stability and other properties of the product after the resin composition is cured.
[0025] As a possible implementation of the resin composition of the present application, the inorganic filler is selected from at least one of amorphous silica, fused silica, crystalline silica, synthetic silica, hollow silica, and spherical silica. In this case, silica has good dielectric properties, a relatively low thermal expansion coefficient, high filling properties and other comprehensive properties, and can reduce the thermal expansion coefficient of the product after the resin composition is cured, improve dimensional stability, increase strength and other properties.
[0026] As a possible implementation of the resin composition of the present application, the resin composition further comprises at least one of a curing accelerator, an initiator, a thermoplastic resin, and an auxiliary agent, which can further improve the physical and chemical properties of the slurry of the resin composition and its cured product.
[0027] As a possible implementation of the resin composition of the present application, the mass ratio of the total mass of the cross-linked polymer resin, the epoxy resin and the curing agent to the mass ratio of the curing accelerator is 100:(0.01~5); under this ratio, the amount of curing accelerator added to the resin composition can better promote the curing reaction between resins, shorten the curing time, and reduce the curing temperature.
[0028] As a possible implementation method of the resin composition of the present application, the mass ratio of the total mass of the cross-linked polymer resin, the epoxy resin and the curing agent to the mass ratio of the initiator is 100: (0.05-5); under this ratio, adding an initiator to the resin composition can effectively promote free radical polymerization and copolymerization reactions in the resin composition, thereby improving the curing and film-forming effect of the resin composition.
[0029] As a possible implementation of the resin composition of the present application, the mass ratio of the total mass of the cross-linked polymer resin, the epoxy resin and the curing agent to the thermoplastic resin is 100:(0.5~40); under this ratio, the thermoplastic resin added to the resin composition can effectively improve the toughness, impact resistance and other properties of the product of the resin composition after curing.
[0030] As a possible implementation of the resin composition of the present application, the mass ratio of the total mass of the cross-linked polymer resin, the epoxy resin and the curing agent to the mass ratio of the auxiliary agent is 100:(0-20). Under this ratio, adding the auxiliary agent to the resin composition can effectively improve the leveling, viscosity, film-forming, coloring, flame retardancy and other properties of the resin composition.
[0031] As a possible implementation method of the resin composition of the present application, the curing accelerator includes at least one of an amine curing accelerator, a phosphorus curing accelerator, an imidazole curing accelerator, a guanidine curing accelerator, and a metal curing accelerator; these types of curing accelerators can better promote the curing reaction between resins, shorten the curing time, and reduce the curing temperature.
[0032] As a possible implementation method of the resin composition of the present application, the initiator includes at least one of 1,1-di-tert-butyl cyclohexene peroxide, diisopropylbenzene peroxide, tert-butyl isopropylbenzene peroxide, di-tert-butyl peroxide, diisopropylbenzene hydroperoxide, isopropylbenzene hydroperoxide, and tert-butyl hydroperoxide; these initiators used can effectively promote free radical polymerization and copolymerization reactions in the resin composition, and improve the curing and film-forming effect of the resin composition.
[0033] As a possible implementation of the resin composition of the present application, the thermoplastic resin includes at least one of phenoxy resin, polyvinyl acetal resin, polyolefin resin, polyimide resin, polyamide-imide resin, polyetherimide resin, polysulfone resin, polyethersulfone resin, polyphenylene ether resin, polycarbonate resin, polyetheretherketone resin, polyester resin, styrene-butadiene copolymer, hydrogenated styrene-butadiene copolymer, polybutadiene, and hydrogenated polybutadiene; these thermoplastic resins used can effectively improve the toughness, impact resistance and other properties of the product of the resin composition after curing.
[0034] As a possible implementation of the resin composition of the present application, the auxiliary agent includes at least one of a flame retardant, an organic filler, a thickener, a defoamer, a leveling agent, and a colorant, which can further improve the physical and chemical properties of the slurry of the resin composition and its cured product.
[0035] As a possible implementation of the resin composition of the present application, the resin composition further comprises a solvent, which can be an ether compound, an alcohol compound, a ketone compound or other organic solvent commonly used in the art to dissolve resin.
[0036] In a second aspect, the present application provides a method for preparing a resin composition, comprising the following steps:
[0037] A cross-linked polymer resin, an epoxy resin, a curing agent and an inorganic filler are prepared into a mixed slurry to obtain a resin composition; wherein the cross-linked polymer resin comprises at least one of the following chemical structural formulas I:
[0038] Formula I; substituents R1 to R9 are independently selected from one of hydrogen atom, alkyl, alkoxy, ester group or aromatic group, R10 is selected from one of hydrogen atom, benzocyclobutene, alkyl, alkoxy, ester group and aromatic group, n is a positive integer of 4 to 1000, m is a positive integer of 0 to 1000, and n+m is a positive integer not less than 5.
[0039] The preparation method of the resin combination provided by the embodiment of the present application, the preparation process is simple, and is suitable for industrial large-scale production and application. In the prepared resin combination, the resin formed by copolymerization of divinylbenzene and its derivatives and olefins and their derivatives shown in the chemical structural formula I is included, and the overall polarity of the molecular structure of this type of resin is relatively low, and no polar group is produced after the functional group is cross-linked, so that the product after the resin is cured has ultra-low loss characteristics. And the molecular weight is higher, so there is good film-forming property, and it is possible to reduce or even do not need to add thermoplastic polymer resin with high dielectric loss as film-forming agent in the resin combination. Therefore, the prepared resin combination has excellent curing film-forming performance, and the cured product has ultra-low dielectric loss and suitable mechanical properties, and is particularly suitable for insulating dielectric materials used as carrier plates.
[0040] As a possible implementation of the method for preparing the resin composition of the present application, after the cross-linked polymer resin, the epoxy resin, and the curing agent are prepared into solutions, they are mixed with the inorganic filler to obtain the resin composition with low dielectric loss. Under this mixing condition, it can be fully ensured that each component in the resin composition is uniformly and stably dispersed in the system.
[0041] As a possible implementation method of the method for preparing the resin composition of the present application, the cross-linked polymer resin is selected from benzocyclobutene resin and / or divinylbenzene resin; wherein the chemical structure of the benzocyclobutene resin is Formula I-1; the chemical structural formula of the divinylbenzene resin is Formula I-2. In this case, the benzocyclobutene resin contains double bonds and functional groups such as benzocyclobutene, which can react under crosslinking conditions to form a crosslinked network structure, and has a better curing film-forming effect; the divinylbenzene resin contains olefin functional groups, which can react under crosslinking conditions to form a crosslinked network structure, and also has a good film-forming effect.
[0042] As a possible implementation of the method for preparing the resin composition of the present application, in the resin composition, the mass ratio of the cross-linked polymer resin, the epoxy resin and the curing agent is (20-90): (5-60): (5-60); in this case, the formula ratio of the three components simultaneously ensures the high film-forming performance of the resin composition, as well as the good lamination and debonding properties of the build-up film formed after the resin composition is formed, and the low dielectric loss of the product after the build-up film is cured.
[0043] As a possible implementation of the method for preparing the resin composition of the present application, the mass ratio of the total mass of the cross-linked polymer resin, the epoxy resin and the curing agent to the mass ratio of the inorganic filler is 1:(1-9). The content of the inorganic filler fully ensures the mechanical properties such as toughness of the product after the resin composition is cured, as well as the properties such as dimensional stability and low dielectric loss.
[0044] In a third aspect, the present application provides a build-up adhesive film, which is made of the above-mentioned resin composition, or the resin composition prepared by the above-mentioned method.
[0045] The layer-building adhesive film provided by the present application is made of the above-mentioned resin composition with low dielectric loss, and the resin composition with low dielectric loss has excellent curing film-forming performance, and the layer-building adhesive film formed after film formation has good lamination and degumming properties, and the film material has ultra-low dielectric loss, suitable mechanical properties and excellent dimensional stability after curing. The ultra-low loss characteristics of the low dielectric loss layer-building adhesive film can effectively avoid the adverse effects such as voltage signal transmission delay and signal transmission delay power loss caused by insufficient dielectric performance, thereby improving the migration transmission efficiency of the signal. The layer-building adhesive film has better application prospects on packaging substrates such as flip chip ball grid array (FC-BGA for short) substrates and ultra-high density UHD boards.
[0046] As a possible implementation of the build-up film of the present application, the dielectric loss of the build-up film after curing is not higher than 0.003, and the thermal expansion coefficient is not higher than 25ppm / °C. In this case, the build-up film has ultra-low dielectric loss and low thermal expansion coefficient, and the dimensional stability of the build-up film is good.
[0047] In a fourth aspect, the present application provides a packaging carrier, wherein the packaging carrier comprises the above-mentioned build-up adhesive film.
[0048] The packaging carrier provided in the present application includes the above-mentioned build-up layer adhesive film. After curing, the build-up layer adhesive film has ultra-low dielectric loss, good film dimensional stability, and suitable mechanical properties. Therefore, it can effectively reduce the influence of the dielectric loss of the interlayer dielectric material on the insertion loss of the carrier, reduce signal transmission loss, and improve signal transmission efficiency.
[0049] In a fifth aspect, the present application provides an electronic device, wherein the electronic device includes the above-mentioned packaging carrier.
[0050] The electronic device provided in the present application includes the packaging carrier board with high signal transmission efficiency, thereby improving the working efficiency of the electronic device.
[0051] The above description is only an overview of the technical solution of the present application. In order to more clearly understand the technical means of the present application, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are listed below. BRIEF DESCRIPTION OF THE DRAWINGS
[0052] Figure 1 It is a schematic flow chart of a method for preparing a resin composition provided in an embodiment of the present application. DETAILED DESCRIPTION
[0053] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application more clearly understood, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.
[0054] In this application, the term "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural. The character " / " generally indicates that the associated objects are in an "or" relationship.
[0055] In this application, "at least one" means one or more, and "plurality" means two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.
[0056] It should be understood that in the various embodiments of the present application, the size of the serial numbers of the above-mentioned processes does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.
[0057] The terms used in the embodiments of the present application are only for the purpose of describing specific embodiments, and are not intended to limit the present application. The singular forms "a", "said" and "the" used in the embodiments of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.
[0058] The term "dielectric loss" refers to the phenomenon that the dielectric itself heats up due to the consumption of part of the electric energy in the alternating electric field. The reason is that the dielectric contains carriers that can conduct electricity. Under the action of the external electric field, a conductive current is generated, which consumes part of the electric energy and converts it into heat energy. Dielectric loss is one of the indicators of the quality of insulating materials (such as insulating oil). The energy lost by the dielectric under the action of a constant electric field is related to the current passing through the inside. After the electric field is added, the current and loss inside the dielectric are as follows: ① The current caused by the geometric capacitance charging of the sample is a displacement current or a capacitive current, and this part of the current does not consume energy; ② The current caused by the establishment of various dielectric polarizations is related to polarization relaxation, etc., and the loss caused is polarization loss; ③ The current caused by the conductivity or leakage conduction of the dielectric is related to the free charge, and the loss caused is conductivity loss. Therefore, energy loss is related to the relaxation polarization, ion deformation and vibration, and conductivity inside the dielectric.
[0059] The term "Df" is an abbreviation for "Dielectric dissipation factor", which stands for dielectric loss tangent, also known as dielectric loss tangent, which refers to the energy consumed by the dielectric to convert electrical energy into heat energy (in the form of heat) per unit volume per unit time. It is a physical quantity that characterizes the dielectric loss of dielectric materials after an electric field is applied, expressed as tanδ, where δ is the dielectric loss angle. The dielectric loss angle is the angle between the current vector and the voltage vector flowing through the dielectric under an alternating electric field.
[0060] The term "CTE" is an abbreviation for "Coefficient of Thermal Expansion", which means the coefficient of thermal expansion. It refers to the expansion and contraction of an object due to temperature changes. The ability of CTE to change is expressed as the change in length value caused by a unit temperature change under constant pressure (p is constant), that is, the coefficient of thermal expansion. The coefficient of thermal expansion of each object is different. Generally, the unit of the coefficient of thermal expansion of metal is 1 / degree Celsius.
[0061] The term "SAP" is an abbreviation for "Semi-Additive Processes", which means semi-additive process, which refers to the process of electroplating patterns on thin copper foil (≤8um), removing the anti-plating dry film, and finally performing differential etching to obtain the required circuits. Because the base copper is very thin (≤8um), those areas that are not electroplated and thickened will be quickly removed in differential etching, and the remaining parts will be retained to form circuits.
[0062] The term "IC package substrate" refers to a key special base material used for IC card module packaging. It mainly protects the chip and serves as an interface between the IC chip and the outside world. It is in the form of a strip, usually golden yellow. The specific use process is as follows: First, the IC card chip is attached to the IC package substrate by a fully automatic placement machine, and then the contacts on the IC chip and the nodes on the IC package substrate are connected by a wire bonding machine to achieve circuit connectivity. Finally, the IC chip is protected by packaging materials to form an IC card module for later application. At present, there are several types of 6PIN, 8PIN, dual interface and contactless packaging frames.
[0063] At present, from the perspective of the development of the market situation, the focus of the printed circuit board market has shifted from computers to communications, especially to mobile terminals such as smartphones and tablets. Therefore, HDI boards (High Density Interconnector) for mobile terminals are the main point of growth for PCBs (printed circuit boards). Mobile terminals represented by smartphones drive HDI boards to be higher density and thinner. It is reported that in the future, there will be higher requirements for the line width / line spacing L / S (Line and Space), the Ra value (average roughness) of the insulation layer, and the adhesion of PCB boards. With the vigorous development of new integrated circuits such as BGA (ballgrid array) and CSP (chip scale package), higher requirements are put forward for new packaging substrates. As one of the most advanced printed circuit boards (PCBs), IC packaging substrates, like any kind of HDI and rigid-flex PCBs, have made rapid progress in popularization and application, and are currently widely used in the upgrading of telecommunications and electronic products. IC packaging substrates are substrates used to package bare IC (integrated circuit) chips.
[0064] The build-up film is one of the key core materials in the flip chip ball grid array (FC-BGA) substrate with a multi-layer structure, ultra-high density UHD board, etc., especially prepared by the semi-additive manufacturing process (SAP processing technology). As one of the key core insulating dielectric materials for the substrate, the dielectric loss of the build-up film has a crucial impact on the entire insertion loss of the substrate. If the dielectric properties of the build-up film are insufficient, it is easy to form a transmission delay for the voltage signal (i.e., RC delay effect), which in turn causes adverse effects such as signal transmission delay power loss, seriously affecting its application in high-end semiconductor packaging substrates. The technical key and development bottleneck of the build-up film material lies in the resin composition material used to prepare the build-up film. At present, the resin composition material for preparing the build-up film usually combines the epoxy thermosetting system formula with the free radical polymerization type low molecular weight resin by certain methods, and uses the low dielectric loss characteristics of the free radical polymerization type resin to reduce the dielectric loss of the entire formula system. However, since the dielectric loss of the free radical polymerizable low molecular weight resin itself is not low enough, and it is inevitable to add a thermoplastic polymer resin with higher dielectric loss as a film-forming agent, the introduction of the free radical polymerizable resin on the basis of the epoxy system has limited reduction in the dielectric tangent value (Df), and the dielectric tangent value (Df) of the build-up film prepared by the resin composition is still relatively large.
[0065] In order to alleviate the problem of high dielectric loss of the product after curing of the resin composition for preparing the build-up film, the study found that adding a cross-linkable resin with ultra-low dielectric loss to the epoxy resin system can greatly reduce the dielectric loss of the resin composition material and obtain an ultra-low dielectric loss (<0.003) build-up film. In addition, since this type of cross-linked polymer resin has a high molecular weight, the resin composition has good film-forming properties, reducing or even eliminating the need to add additional thermoplastic polymer resins with high dielectric loss as film-forming agents to the resin composition, thereby further ensuring that the resin composition and the build-up film prepared therefrom have ultra-low dielectric loss. This makes the build-up film have better application prospects on packaging substrates such as flip chip ball grid array (FC-BGA) substrates and ultra-high density UHD boards.
[0066] For the convenience of explanation, the following embodiments of the present application are described by taking a resin composition with low dielectric loss and a preparation method thereof, a build-up adhesive film and applications as examples.
[0067] In a first aspect, an embodiment of the present application provides a resin composition, the resin composition comprising components: a cross-linked polymer resin, an epoxy resin, a curing agent, and an inorganic filler; wherein the cross-linked polymer resin comprises at least one of the following chemical structural formulas I:
[0068] Formula I; substituents R1 to R9 are independently selected from one of hydrogen atom, alkyl, alkoxy, ester group or aromatic group, R10 is selected from one of hydrogen atom, benzocyclobutene, alkyl, alkoxy, ester group and aromatic group, n is a positive integer of 4 to 1000, m is a positive integer of 0 to 1000, and n+m is a positive integer not less than 5.
[0069] In this way, the resin composition provided by the embodiment of the present application includes cross-linked polymer resin, epoxy resin, curing agent and inorganic filler, wherein, cross-linked polymer resin is a resin formed by copolymerization of divinylbenzene and its derivatives with olefins and their derivatives, as shown in chemical structural formula I, the resin of this specific chemical structure, on the one hand, contains functional groups such as reactive double bonds, and self-crosslinking reaction can occur under cross-linking conditions to form a cross-linked network, without the need to additionally add auxiliary agents such as initiators, so as to obtain a resin composition cured product with high cross-linking density. On the other hand, the overall polarity of the molecular structure of this type of resin is relatively low, and polar groups are not produced after cross-linking, so that the product after the resin is cured has ultra-low loss characteristics, and the dielectric loss of the product after the resin composition is significantly reduced. On the other hand, this type of cross-linked polymer resin has a higher molecular weight, so that the resin composition has good film-forming properties, reducing or even without the need to additionally add a thermoplastic polymer resin with high dielectric loss as a film-forming agent in the resin composition. Thus it is better ensured that the product after the resin composition is cured has ultra-low dielectric loss. In addition, epoxy resin and curing agent ensure the degumming performance of the product after curing of the resin composition with low dielectric loss, so as to be conducive to preparing a metal layer on the surface of the resin composition, and also to improve the toughness of the product after curing of the resin composition. Inorganic filler ensures the mechanical properties and dimensional stability of the product after curing of the resin composition with low dielectric loss. Therefore, the resin composition with low dielectric loss provided by the embodiment of the present application has excellent curing film-forming performance through the joint action of each raw material component, and the layered adhesive film formed after the film formation of the resin composition has good lamination and degumming, and the product after curing of the layered adhesive film has ultra-low dielectric loss, good dimensional stability and suitable mechanical properties. It is particularly suitable for insulating dielectric materials used as carriers, and its ultra-low dielectric loss characteristics can effectively avoid the adverse effects such as voltage signal transmission delay and signal transmission delay power loss caused by insufficient dielectric performance, thereby improving the migration transmission efficiency of signals.
[0070] The cross-linked polymer resin in the resin composition of the present application embodiment may contain only one specific structure of Chemical Formula I, or may contain two or more resins with different structures at the same time. In practical applications, a cross-linked polymer resin with suitable performance may be selected according to specific needs.
[0071] In some possible embodiments, the functional components in the resin composition only include cross-linked polymer resin, epoxy resin, curing agent and inorganic filler, that is, the functional components of the resin composition are composed of cross-linked polymer resin, epoxy resin, curing agent and inorganic filler. In this case, since the cross-linked polymer resin in the resin composition has excellent film-forming properties, there is no need to add an additional film-forming agent in the resin composition, thereby avoiding the introduction of a thermoplastic polymer resin with high dielectric loss as a film-forming agent in the resin composition.
[0072] In some possible embodiments, R1 to R9 in the chemical structural formula I are independently selected from a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, an ester group having 1 to 10 carbon atoms, and an aromatic group having 6 to 12 carbon atoms.
[0073] In some possible embodiments, R10 in the chemical structural formula I is selected from a hydrogen atom, a benzocyclobutene, an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, an ester group having 1 to 10 carbon atoms, and an aromatic group having 6 to 12 carbon atoms.
[0074] In this case, by selecting and matching the substituents R1 to R10 in the chemical structure I of the cross-linked polymer resin, not only can the cross-linked polymer resin present a variety of configurations, but also can contain functional groups such as double bonds and benzocyclobutene in the cross-linked polymer resin, which is more conducive to improving the curing film-forming performance of the resin. At the same time, it is also conducive to reducing the polarity of the resin and its cross-linked product, so that the cross-linked polymer resin has lower dielectric loss and better curing film-forming performance, thereby better improving the film-forming performance of the resin composition and reducing the dielectric loss of the product after the resin composition is cured.
[0075] In some possible embodiments, the cross-linked polymer resin includes benzocyclobutene resin and / or divinylbenzene resin; wherein the chemical structure of the benzocyclobutene resin is Formula I-1; The chemical structural formula of divinylbenzene resin is Formula I-2. In this case, the benzocyclobutene resin contains double bonds and functional groups such as benzocyclobutene, which can react under crosslinking conditions to form a crosslinked network structure, and has a better curing film-forming effect. Wherein, the divinylbenzene resin includes divinylbenzene resin and divinylbenzene derivative resin. The divinylbenzene resin contains olefin functional groups, which can react under crosslinking conditions to form a crosslinked network structure, and also has a better film-forming effect.
[0076] In some possible embodiments, the benzocyclobutene resin is selected from In this case, the benzocyclobutene resins of these specific structures contain double bonds and functional groups such as benzocyclobutene, which can react under crosslinking conditions to form a crosslinked network structure and have a good curing film-forming effect.
[0077] In some possible embodiments, the divinylbenzene resin is selected from At least one of the following, wherein a is a positive integer of 4 to 1000, b is a positive integer of 0 to 100, c is a positive integer of 0 to 1000, and d is a positive integer of 0 to 1000. In this case, the divinylbenzene resins of these specific structures contain multiple double bonds and have good curing film-forming effects under crosslinking conditions.
[0078] In some possible embodiments, the weight average molecular weight of the cross-linked polymer resin is 1000 to 1000000. In this case, the cross-linked polymer resin has a relatively high molecular weight, and the high molecular weight resin is conducive to winding other small molecular weight components during film formation, so that the layered adhesive film formed after the resin film is formed has a certain flexibility, and it is not easy to break when the film material is used. Therefore, the cross-linked polymer resin with a weight average molecular weight of 1000 to 1000000 makes the resin composition have good film-forming properties, which can effectively reduce or even eliminate the need to add additional thermoplastic polymer resins with high dielectric loss as film-forming agents in the resin composition, thereby better ensuring that the product after the resin composition is cured has ultra-low dielectric loss. For example, the weight average molecular weight of the cross-linked polymer resin may be 1000-2000, 2000-3000, 3000-4000, 4000-5000, 5000-6000, 6000-7000, 7000-8000, 8000-10000, 10000-15000, 15000-20000, 20000-30000, 30000-40000, 40000-50000, 50000-60000, 60000-70000, 70000-80000. ~80000, 90000~100000, 100000~200000, 200000~300000, 400000~500000, 500000~600000, 700000~800000, 900000~1000000, 1000~10000, 10000~1000000, 10000~1000000, 2000~20000, 5000~50000, 60000~60000, 80000~800000, etc.
[0079] In some possible implementations, the weight average molecular weight of the cross-linked polymer resin is 2000 to 100000. The cross-linked polymer resin within this weight average molecular weight range can better improve the film-forming properties of the resin composition, ensure the lamination of the build-up film after film formation, and reduce the dielectric loss of the product after the resin composition is cured.
[0080] In some possible embodiments, the cross-linked polymer resin including at least one of the chemical structural formula I in the resin composition of the embodiment of the present application can be synthesized by methods known in the art, or directly obtained by commercial purchase. The specific effects that can be achieved by cross-linked polymer resins with different acquisition sources and chemical structural formulas in the present application are slightly different, but they can all play a role in reducing the dielectric loss of the resin composition and its cured product, improving the film-forming performance, and achieving the core performance of the technical solution of the embodiment of the present application.
[0081] In some possible embodiments, in the resin composition, the mass ratio of the cross-linked polymer resin, the epoxy resin and the curing agent is (20-90): (5-60): (5-60). In this case, in the resin composition, the cross-linked polymer resin, the epoxy resin and the curing agent are non-volatile components, and the formula ratio of the three components simultaneously ensures the high film-forming performance of the resin composition, as well as the good lamination and degumming properties of the added layer film formed after the resin composition is formed, and the low dielectric loss of the added layer film after curing. Among them, the ratio of the cross-linked polymer resin and the epoxy resin is beneficial to reducing the low dielectric loss of the product after the resin composition is cured, and is also beneficial to the degumming process of the added layer film. The degumming process increases the surface roughness of the film layer, which is beneficial to the subsequent combination with the metal plating layer. The content of the curing agent fully ensures that the epoxy resin in the resin composition can be cross-linked and cured, and avoids the introduction of substances containing polar groups when the content is too high, resulting in an increase in the dielectric loss of the product after the resin composition is cured.
[0082] In some possible implementations, cross-linked polymer resin, epoxy resin and curing agent are used as non-volatile components, and the mass percentage of cross-linked polymer resin in the non-volatile component is 20-90%, and examples thereof are 20-30%, 30-40%, 40-50%, 50-60%, 60-70%, 70-80%, 80-90%, 30-80%, 40-70%, 50-60%, etc. The mass percentage of epoxy resin in the non-volatile component is 5-60%, and examples thereof are 5-10%, 10-20%, 20-30%, 30-40%, 40-50%, 50-60%, 10-50%, 20-40%, 30-50%, etc. The mass percentage of the curing agent in the non-volatile component is 5-60%, exemplified by 5-10%, 10-20%, 20-30%, 30-40%, 40-50%, 50-60%, 10-50%, 20-40%, 30-50%, etc.
[0083] In some possible embodiments, in the resin composition, the mass ratio of the total mass of the cross-linked polymer resin, the epoxy resin and the curing agent to the inorganic filler is 1: (1-9). In this case, the content of the inorganic filler in the resin composition fully ensures the mechanical properties such as toughness of the product after the resin composition is cured, as well as properties such as dimensional stability. Exemplarily, in the resin composition, the mass ratio of the total mass of the cross-linked polymer resin, the epoxy resin and the curing agent to the inorganic filler can be 1: (1-2), 1: (2-3), 1: (3-4), 1: (4-5), 1: (5-6), 1: (6-9), etc.
[0084] In some possible embodiments, the epoxy resin molecule contains more than two epoxy groups, which is a polycondensation product of epichlorohydrin and bisphenol A or polyol. Due to the chemical activity of the epoxy group, a variety of compounds containing active hydrogen can be used to open the ring, and the cross-linking is cured to form a network structure, so it is a thermosetting resin. The epoxy resin of the embodiment of the present application can be an epoxy resin of any chemical structure well known in the art, which can be used alone or in combination with two or more epoxy resins. The specific effects that epoxy resins of different structures can achieve in this application are slightly different, but they can all achieve the core performance of the present application scheme. Exemplary, epoxy resins include glycidyl ether epoxy resins, glycidyl ester epoxy resins, glycidyl amine epoxy resins, alicyclic epoxy resins, aliphatic epoxy resins, etc.
[0085] The present application embodiment does not particularly limit the curing agent, as long as it is a substance or resin that can cure epoxy resin, it can be used as a curing agent. In some possible embodiments, the curing agent includes at least one of phenols, cyanates, benzoxazines, carbodiimides, and active esters. Among them, phenolic curing agents have excellent compatibility, corrosion resistance and other characteristics, are specially made long carbon chain resin polymers, and the reactive group is a phenol group, which is very compatible with epoxy resin. The curing mechanism of phenolic curing agents for epoxy resin mainly includes: etherification reaction of phenolic hydroxyl and epoxy group, etherification reaction of secondary hydroxyl and epoxy group, etc. Cyanate curing agents are resins containing -OC≡N cyanate functional groups, and their main components are cyanate monomers or prepolymers. This type of cyanate curing agent can undergo cross-linking reactions with substances containing active hydrogen groups such as polyesters and polyethers to form high molecular polymers, thereby achieving the curing and strengthening of resin compositions with low dielectric loss. Exemplary, cyanate curing agents include: bisphenol A cyanate, bisphenol F cyanate, phenolic cyanate, dicyclopentadiene cyanate, partially prepolymerized bisphenol A cyanate, etc. Benzoxazine curing agent is a special thermosetting compound. The characteristic of this type of ring-opening polymerization reaction is that there is almost no release of low molecular weight substances during the curing process. Active ester curing agents contain two or more ester groups with high activity, which can react with epoxy resin. The grid structure formed after the reaction does not contain secondary alcohol hydroxyl groups makes its cured product have low dielectric loss and water absorption. Carbodiimide curing agent is a cross-linking agent product with very high cross-linking efficiency, with high reactivity and excellent cross-linking performance, and the contained carbodiimide functional group can react with the group in epoxy resin.
[0086] In certain embodiments, the curing agent includes a variety of phenols, cyanates, benzoxazines, carbodiimides, and active esters, and through the compounding of a variety of curing agents, the resin in the composition can be cross-linked and cured to form a film material. In certain embodiments, the curing agent includes at least one of phenols, cyanates, and active ester resins. In this case, these curing agents not only have a better curing effect on epoxy resins, but also these curing agents easily contain a group cross-linked with a cross-linked polymer resin, which is conducive to improving the cured film-forming performance of the resin combination, and reducing the dielectric loss of the product after the resin combination is cured.
[0087] In some possible implementations, the curing agent is selected from at least one of phenols, cyanates, and active esters modified with at least one functional group containing a double bond or a benzocyclobutene group. In this case, the functional groups contained in the curing agent can react with the cross-linked polymer resin, and while curing the epoxy resin, it can also cross-link with the cross-linked resin, thereby being more conducive to improving the film-forming properties of the resin composition.
[0088] In some possible embodiments, the average particle size of the inorganic filler is 0.01 to 10 μm. In this case, the inorganic filler is beneficial to improve the mechanical strength and other properties of the product after the resin composition is cured. Exemplarily, the average particle size of the inorganic filler can be 0.01 to 0.1 μm, 0.1 to 0.5 μm, 0.5 to 1 μm, 1 to 1.5 μm, 1.5 to 2 μm, 2 to 3 μm, 3 to 4 μm, 4 to 5 μm, 5 to 6 μm, 6 to 7 μm, 7 to 8 μm, 8 to 9 μm, 9 to 10 μm, etc.
[0089] In some possible embodiments, the average particle size of the inorganic filler is 0.05 to 5 μm, and further, the average particle size of the inorganic filler is 0.1 to 2 μm. In this case, the inorganic filler used in the resin composition of the embodiment of the present application has a smaller particle size, and the filler with a small particle size is beneficial to improving the surface flatness and smoothness of the product after the resin composition is cured.
[0090] In some possible embodiments, the surface of the inorganic filler is treated with at least one coupling agent in aminosilanes, epoxysilanes, silanes containing double bonds, mercaptosilanes, silanes, and titanates. In this case, by surface treating the inorganic filler, its surface is changed from hydrophilic to hydrophobic or with a functional group that can react with the resin, thereby improving the compatibility and bonding force of the inorganic filler with the resin. At least one coupling agent in the aminosilanes, epoxysilanes, silanes containing double bonds, mercaptosilanes, silanes, and titanates used is a surface treatment agent of a class of polymer compounds, which has the function of forming a chemical bond between the surface of the inorganic filler and the resin, and plays a bridging role in the resin-based composite material of the composition. In addition, treating the surface of the inorganic filler with a coupling agent can also improve the wettability between the filler and the resin, forming a mechanical micro-buffer, greatly enhancing the bonding between the filler and the resin interface, preventing the intrusion of moisture or other impurities, reducing or even eliminating the weak interface layer, effectively transmitting stress, improving the bonding force between the interfaces, and significantly improving the comprehensive performance of the product after the resin composition is cured. In some specific embodiments, the surface of the inorganic filler is treated with two or more coupling agents selected from aminosilanes, epoxysilanes, double-bond silanes, mercaptosilanes, silanes, and titanates to better promote the compatibility between the inorganic filler and the resin.
[0091] In some possible embodiments, the inorganic filler includes at least one of silicon dioxide, aluminum oxide, glass, cordierite, silicon oxide, barium sulfate, barium carbonate, talc, clay, mica powder, zinc oxide, hydrotalcite, boehmite, aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, magnesium oxide, boron nitride, aluminum nitride, manganese nitride, aluminum borate, strontium carbonate, strontium titanate, calcium titanate, magnesium titanate, bismuth titanate, titanium oxide, zirconium oxide, barium titanate, barium zirconate, barium zirconate, calcium zirconate, zirconium phosphate, and zirconium tungstate phosphate. These inorganic fillers are added to the resin composition to improve the mechanical properties, dimensional stability and other properties of the product after the resin composition is cured.
[0092] In some possible embodiments, the inorganic filler is selected from at least one of amorphous silica, fused silica, crystalline silica, synthetic silica, hollow silica, and spherical silica. In this case, silica is selected as the inorganic filler, and silica has the comprehensive properties such as good dielectric properties, relatively low thermal expansion coefficient, high filling properties, can reduce the thermal expansion coefficient of the cured product of the resin combination, improve dimensional stability, increase strength, thereby reducing the shrinkage after the resin combination is cured, and also can significantly improve the mechanical properties, thermal stability and volume resistivity of the material, reduce costs, etc. In a further embodiment, the inorganic filler selects spherical silica. The shape of silica has a certain influence on the filling effect, and spherical silica has higher bulk density and uniform stress distribution, therefore can increase the fluidity of the resin combination system, reduce the viscosity of the system.
[0093] In some specific embodiments, the inorganic filler in the resin composition is selected from at least one of silica, aluminum oxide, glass, cordierite, silicon oxide, barium sulfate, barium carbonate, talc, clay, mica powder, zinc oxide, hydrotalcite, boehmite, aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, magnesium oxide, boron nitride, aluminum nitride, manganese nitride, aluminum borate, strontium carbonate, strontium titanate, calcium titanate, magnesium titanate, bismuth titanate, titanium oxide, zirconium oxide, barium titanate, barium zirconate, barium zirconate, calcium zirconate, zirconium phosphate, and zirconium tungstate phosphate, having an average particle size of 0.01 to 10 μm and a surface treated with at least one coupling agent selected from aminosilanes, epoxysilanes, double bond-containing silanes, mercaptosilanes, silanes, and titanates.
[0094] In some possible embodiments, the resin composition also includes at least one of a curing accelerator, an initiator, a thermoplastic resin, and an auxiliary agent. Among them, the main function of the curing accelerator is to promote the curing reaction between the epoxy resin and the curing agent, shorten the curing time or reduce the curing temperature. The curing accelerator added to the resin composition in the embodiment of the present application has a significant catalytic curing effect; and has good compatibility with other components in the resin composition system; it will not have an adverse effect on the curing system and has good chemical stability and low price, easy to obtain, etc. Among them, the initiator is easily decomposed by heat to produce free radicals (i.e., primary free radicals), which can promote free radical polymerization and copolymerization reactions in the resin composition and improve the curing film-forming effect of the resin composition. Thermoplastic resins have the properties of softening by heat and hardening by cooling, and do not react chemically. No matter how many times the heating and cooling are repeated, this property can be maintained. Thermoplastic resins have the following significant characteristics in mechanical properties: ① It has a significant mechanical relaxation phenomenon; ② Under the action of external forces, the ability to deform is large, that is, when the strain rate is not large, it can have a considerable elongation at break; ③ Good impact resistance. Therefore, adding thermoplastic resin to the resin composition is beneficial to improving the toughness, impact resistance and other properties of the cured product of the resin composition. In addition, auxiliary additives can further improve the physicochemical properties of the slurry of the resin composition and its cured product.
[0095] In some possible implementations, the mass ratio of the total mass of the cross-linked polymer resin, epoxy resin and curing agent to the mass ratio of the curing accelerator is 100:(0.01-5). Under this ratio, the amount of curing accelerator added to the resin composition can better promote the curing reaction between the resins, shorten the curing time, and reduce the curing temperature. Exemplarily, the mass ratio of the total mass of the cross-linked polymer resin, epoxy resin and curing agent to the mass ratio of the curing accelerator can be 100: (0.01-0.05), 100: (0.05-0.1), 100: (0.1-0.2), 100: (0.2-0.5), 100: (0.5-0.8), 100: (0.8-1), 100: (1-1.5), 100: (1.5-2), 100: (2-2.5), 100: (2.5-3), 100: (3-3.5), 100: (3.5-4), 100: (4-4.5), 100: (4.5-5), etc.
[0096] In some possible embodiments, the curing accelerator includes at least one of an amine curing accelerator, a phosphorus curing accelerator, an imidazole curing accelerator, a guanidine curing accelerator, and a metal curing accelerator; these types of curing accelerators can better promote the curing reaction between the epoxy resin and the curing agent, shorten the curing time, and reduce the curing temperature.
[0097] In some possible implementations, the mass ratio of the total mass of the cross-linked polymer resin, epoxy resin and curing agent to the mass ratio of the initiator is 100:(0.05-5). Under this ratio, adding an initiator to the resin composition can effectively promote free radical polymerization and copolymerization reactions in the resin composition, and improve the curing film-forming effect of the resin composition. Exemplarily, the mass ratio of the total mass of the cross-linked polymer resin, epoxy resin and curing agent to the mass ratio of the initiator can be 100: (0.01-0.05), 100: (0.05-0.1), 100: (0.1-0.2), 100: (0.2-0.5), 100: (0.5-0.8), 100: (0.8-1), 100: (1-1.5), 100: (1.5-2), 100: (2-2.5), 100: (2.5-3), 100: (3-3.5), 100: (3.5-4), 100: (4-4.5), 100: (4.5-5), etc.
[0098] In some possible embodiments, the initiator includes at least one of 1,1-di-tert-butyl cyclohexyl peroxide, diisopropylbenzene peroxide, tert-butyl isopropylbenzene peroxide, di-tert-butyl peroxide, diisopropylbenzene hydroperoxide, isopropylbenzene hydroperoxide, and tert-butyl hydroperoxide; these initiators used can effectively promote free radical polymerization and copolymerization reactions in the resin composition, and improve the curing and film-forming effect of the resin composition.
[0099] In some possible embodiments, the mass ratio of the total mass of the cross-linked polymer resin, the epoxy resin and the curing agent to the thermoplastic resin is 100: (0.5-40). Under this ratio, the thermoplastic resin added to the resin composition can effectively improve the toughness, impact resistance and other properties of the product after the resin composition is cured. Exemplarily, the mass ratio of the total mass of the cross-linked polymer resin, the epoxy resin and the curing agent to the thermoplastic resin can be 100: (0.5-1), 100: (1-3), 100: (3-5), 100: (5-8), 100: (8-10), 100: (10-15), 100: (15-20), 100: (20-23), 100: (23-25), 100: (25-30), 100: (30-35), 100: (35-38), 100: (38-40), etc.
[0100] In some possible embodiments, the thermoplastic resin includes at least one of phenoxy resin, polyvinyl acetal resin, polyolefin resin, polyimide resin, polyamide-imide resin, polyetherimide resin, polysulfone resin, polyethersulfone resin, polyphenylene ether resin, polycarbonate resin, polyetheretherketone resin, polyester resin, styrene-butadiene copolymer, hydrogenated styrene-butadiene copolymer, polybutadiene, and hydrogenated polybutadiene; these thermoplastic resins used can effectively improve the toughness, impact resistance and other properties of the product after the resin composition is cured.
[0101] In some possible embodiments, the mass ratio of the total mass of the cross-linked polymer resin, epoxy resin and curing agent to the mass ratio of the auxiliary agent is 100: (0-20). Under this ratio, the addition of auxiliary agents to the resin composition can effectively improve the leveling, viscosity, film-forming, coloring, flame retardancy and other properties of the resin composition. Exemplarily, the mass ratio of the total mass of the cross-linked polymer resin, epoxy resin and curing agent to the mass ratio of the auxiliary agent can be 100: (0-1), 100: (1-3), 100: (3-5), 100: (5-8), 100: (8-10), 100: (10-13), 100: (13-15), 100: (15-18), 100: (18-20), etc.
[0102] In some possible implementations, the auxiliary agent includes at least one of a flame retardant, an organic filler, a thickener, a defoamer, a leveling agent, and a colorant. In the resin composition of the present application example, the type and amount of the auxiliary agent can be reasonably selected and added according to the actual application requirements, without specific limitation.
[0103] Among them, the flame retardant can improve the flame retardant properties of the resin composition and its cured product. Exemplarily, the flame retardant includes organic flame retardant and inorganic flame retardant, halogen flame retardant (organic chloride and organic bromide) and non-halogen. Organic flame retardants are represented by bromine, phosphorus nitrogen, nitrogen and red phosphorus and compounds, while inorganic flame retardants are mainly antimony trioxide, magnesium hydroxide, aluminum hydroxide, silicon and other flame retardant systems.
[0104] Organic fillers are made of natural plants and animals and artificially synthesized organic materials, such as regenerated cellulose, synthetic resins, etc., which can further improve the mechanical properties of the resin composition.
[0105] The thickener can increase the viscosity of the resin composition system, so that the system maintains a uniform and stable suspension state or an emulsion state, which is beneficial for the subsequent preparation of the resin composition into a film material with uniform film thickness. In some embodiments, the thickener includes one or more of alkaline earth metal oxides, alkaline earth metal hydroxides, isocyanate compounds, and alcohols; illustratively, the thickener includes one or more of magnesium oxide, calcium oxide, barium oxide, magnesium hydroxide, calcium hydroxide, barium hydroxide, toluene diisocyanate (TDI), polyethylene glycol, and polypropylene glycol.
[0106] The defoamer added to the resin composition system does not affect the basic properties of the system, that is, it does not react with the defoamed system; at the same time, it has strong defoaming power, small dosage, low surface tension, good balance with the surface, good heat resistance, good diffusivity and permeability, chemical stability, strong oxidation resistance, good gas solubility and permeability, low solubility in foaming solutions, no physiological activity, high safety, etc., and can effectively reduce or even eliminate bubbles generated by the resin composition during preparation, transportation, processing, etc. In some embodiments, the defoamer includes an organosilicon or polyether defoamer, and illustratively, the defoamer includes polydimethylsiloxane, methyltrimethoxysilane, polyoxypropylene oxyethylene glycerol ether, etc.
[0107] The leveling agent can promote the resin composition to form a flat, smooth and uniform coating film during the curing film-forming process. It can effectively reduce the surface tension of the coating liquid and improve its leveling and uniformity. It improves the permeability of the resin composition, reduces the possibility of spots and scars during deposition, and makes the film formation uniform and natural. Exemplarily, the leveling agent is selected from at least one of acrylate homopolymers, acrylate oligomers, acrylate copolymers, silicone-modified acrylate polymers, and polysiloxanes; further, the leveling agent is selected from at least one of polyethyl acrylate, polybutyl acrylate, poly-2-ethylhexyl acrylate, ethyl acrylate and butyl acrylate copolymers, and silicone-modified acrylate polymers.
[0108] Colorant can change the color of resin combination and its cured product.By adding inorganic pigment and organic pigment to resin combination to color, resin combination is better satisfied with higher tinting strength and brilliance, good transparency, hiding power, dispersibility, weatherability, thermal stability, chemical stability, electrical performance and environmental performance and other requirements.In certain embodiments, colorant includes organic colorant and inorganic colorant, wherein, inorganic colorant heat resistance, weatherability, mobility are superior, and low price.Exemplary, inorganic colorant mainly includes the following categories: metal oxide, such as: titanium dioxide, chromium trioxide, iron oxide, zinc oxide, antimony oxide, etc.; carbon black; metal sulfide, such as: cadmium sulfide, mercuric sulfide, etc.; chromate, such as: chrome yellow, chrome orange, etc.; molybdate, such as: molybdenum red, etc.; other pigments such as ultramarine, iron blue, manganese pigment, cobalt pigment and bismuth vanadate. Organic colorants have a wide variety of types, bright colors, high tinting power and excellent application performance. According to their different structural types, they mainly include: insoluble azo pigments, lake pigments, phthalocyanine pigments, quinoxaline pigments, pyrrolopyrrole dione pigments, dioxazine pigments, isophthalic acid pigments, and some such as carbazole, pyrene, quinophthalone, anthracene pigments, benzimidazolaldehyde pigments, etc.
[0109] In some possible embodiments, the resin composition also includes a solvent, and the solvent may be an organic solvent for dissolving resins commonly used in the art such as ether compounds, alcohol compounds and other ketone compounds. In some specific embodiments, the resin composition also includes at least one solvent in acetone, butanone, methanol, methyl ether, ethylene glycol methyl ether, toluene, and xylene. The present application embodiment does not specifically limit the content of the solvent in the resin composition, as long as the components in the resin composition can form a uniformly dispersed and stable slurry, and it is conducive to subsequent film forming treatment. In practical applications, under the premise of ensuring that each component is fully and evenly dissolved and dispersed, the amount of solvent can be added according to different film forming processes to make the resin composition have a slurry viscosity suitable for the film forming process.
[0110] The resin composition provided in the above embodiments of the present application can be prepared by the following embodiment method.
[0111] Second, as attached Figure 1 As shown, the present application provides a method for preparing a resin composition, comprising the following steps:
[0112] S10. A cross-linked polymer resin, an epoxy resin, a curing agent and an inorganic filler are prepared into a mixed slurry to obtain a resin composition; wherein the cross-linked polymer resin comprises at least one of the following chemical formulas I:
[0113] Formula I; substituents R1 to R9 are independently selected from one of hydrogen atom, alkyl, alkoxy, ester group or aromatic group, R10 is selected from one of hydrogen atom, benzocyclobutene, alkyl, alkoxy, ester group and aromatic group, n is a positive integer of 4 to 1000, m is a positive integer of 0 to 1000, and n+m is a positive integer not less than 5.
[0114] The preparation method of the resin composition provided by the embodiment of the present application, cross-linked polymer resin, epoxy resin, curing agent and inorganic filler are made into mixed slurry, and a resin composition with low dielectric loss is obtained, and the preparation process is simple, and it is suitable for industrial large-scale production and application. In the resin composition with low dielectric loss prepared, the resin formed by copolymerization of divinylbenzene and its derivatives and olefins and their derivatives shown in the chemical structural formula I is included, and the overall polarity of the molecular structure of this type of resin is relatively low, and polar groups are not produced after cross-linking, so that the product after the resin is cured has ultra-low loss characteristics. And containing functional groups such as reactive double bonds, the molecular weight is relatively high, and thus there is a good curing film-forming performance, which can reduce or even do not need to add thermoplastic polymer resins with high dielectric loss as film-forming agents in the resin composition. Therefore, the prepared resin composition has excellent curing film-forming performance, and the cured product has ultra-low dielectric loss and suitable mechanical properties, and is particularly suitable for insulating dielectric materials used as carriers.
[0115] In some possible embodiments, after cross-linked polymer resin, epoxy resin and curing agent are respectively configured into solution, mixed treatment is carried out with inorganic filler to obtain a resin composition with low dielectric loss. In this case, cross-linked polymer resin is dissolved in a solvent and pre-configured into a solution, epoxy resin is dissolved and dispersed in a solvent and pre-configured into a solution, and curing agent is also dissolved in a solvent and pre-configured into a solution, and then each raw material component dissolved in advance is mixed and processed, so that each raw material component is fully and evenly mixed and dispersed, and after forming a uniformly dispersed and stable solution system, inorganic filler is added for mixed treatment, which is conducive to making the inorganic filler fully and evenly dispersed in the resin composition system, preventing filler from aggregating and depositing. Under this mixing condition, it is possible to fully ensure that each component in the resin composition is uniformly and stably dispersed in the system. In some possible embodiments, the solvent can be an organic solvent for dissolving resins commonly used in other fields such as ether compounds, alcohol compounds and other ketone compounds. In some specific embodiments, the solvent can be at least one of acetone, butanone, methanol, methyl ether, ethylene glycol methyl ether, toluene and xylene.
[0116] In some possible embodiments, the cross-linked polymer resin is selected from benzocyclobutene resin and / or divinylbenzene resin; wherein the chemical structure of the benzocyclobutene resin is Formula I-1; The chemical structural formula of divinylbenzene resin is Formula I-2. In this case, the benzocyclobutene resin contains double bonds and functional groups such as benzocyclobutene, which can react under crosslinking conditions to form a crosslinked network structure, and has a better curing film-forming effect; the divinylbenzene resin includes divinylbenzene resin and divinylbenzene derivative resin, and the divinylbenzene resin contains olefin functional groups, which can react under crosslinking conditions to form a crosslinked network structure, and also has a good film-forming effect.
[0117] In one possible embodiment, the cross-linked polymer resin is selected from
[0118] At least one of the following, wherein a is a positive integer of 4 to 1000, b is a positive integer of 0 to 100, c is a positive integer of 0 to 1000, and d is a positive integer of 0 to 1000. The benzocyclobutene resins of these specific structures simultaneously contain double bonds and / or functional groups such as benzocyclobutene, and can react under crosslinking conditions to form a crosslinked network structure, and have a good curing film-forming effect.
[0119] In some possible implementations, the weight average molecular weight of the cross-linked polymer resin is 1000 to 1000000. Further, the weight average molecular weight of the cross-linked polymer resin is 2000 to 100000. The cross-linked polymer resin within this weight average molecular weight range can better reduce the dielectric loss of the product after the resin composition is cured and improve the film-forming performance of the resin composition.
[0120] In some possible embodiments, in the resin composition, the mass ratio of the cross-linked polymer resin, the epoxy resin and the curing agent is (20-90): (5-60): (5-60); in this case, in the resin composition, the cross-linked polymer resin, the epoxy resin and the curing agent are non-volatile components, and the formula ratio of the three components simultaneously ensures the high film-forming performance of the resin composition, as well as the good lamination and debonding properties of the build-up film formed after the resin composition is formed, and the low dielectric loss of the product after the build-up film is cured. In addition, the mass ratio of the total mass of the cross-linked polymer resin, the epoxy resin and the curing agent to the inorganic filler is 1: (1-9). The content of the inorganic filler fully ensures the mechanical properties such as toughness of the product after the resin composition is cured, as well as properties such as low dielectric loss.
[0121] In a third aspect, the present application provides a build-up adhesive film, which is made of the above-mentioned resin composition, or the resin composition prepared by the above-mentioned method.
[0122] The layer-building adhesive film provided in the embodiment of the present application is made of the above-mentioned resin composition with low dielectric loss. The resin composition has excellent curing film-forming performance. The layer-building adhesive film prepared by the resin composition has ultra-low dielectric loss, and the film material has suitable mechanical properties and excellent dimensional stability. After the film material is cured, it has ultra-low dielectric loss and excellent dimensional stability. The ultra-low dielectric loss characteristics of the low dielectric loss layer-building adhesive film can effectively avoid the adverse effects such as voltage signal transmission delay and signal transmission delay power loss caused by insufficient dielectric performance, thereby improving the migration transmission efficiency of the signal. The layer-building adhesive film has better application prospects on packaging substrates such as flip chip ball grid array (FC-BGA for short) substrates and ultra-high density UHD boards.
[0123] In some possible implementations, the dielectric loss of the build-up film after curing is not higher than 0.003, and the thermal expansion coefficient is not higher than 25ppm / °C. In this case, the build-up film has ultra-low dielectric loss and low thermal expansion coefficient, and the build-up film has good dimensional stability, making the build-up film particularly suitable as an insulating dielectric material for a carrier board, significantly reducing the effect of dielectric loss on board insertion loss, reducing signal transmission loss, and improving signal transmission efficiency.
[0124] The embodiment of the present application does not specifically limit the method of using a resin composition with low dielectric loss to make a build-up film, and the film material can be made by any method in the art. In some possible embodiments, the steps of using a resin composition with low dielectric loss to make a build-up film include but are not limited to: coating the resin composition with low dielectric loss on a substrate to form a wet film, pre-baking at a temperature of 80 to 120° C. to volatilize and remove the solvent, and obtaining a build-up film.
[0125] In a fourth aspect, the present application provides a packaging carrier, wherein the packaging carrier comprises the above-mentioned build-up adhesive film.
[0126] The packaging carrier provided in the embodiment of the present application includes the above-mentioned build-up layer adhesive film. The build-up layer adhesive film has ultra-low dielectric loss after curing, and the film material has good dimensional stability and suitable mechanical properties. Therefore, it can effectively reduce the influence of dielectric loss on the insertion loss of the board, reduce signal transmission loss, and improve signal transmission efficiency.
[0127] In a fifth aspect, the present application provides an electronic device, wherein the electronic device includes the above-mentioned packaging carrier.
[0128] The electronic device provided in the embodiment of the present application includes the packaging carrier with high signal transmission efficiency, thereby improving the working efficiency of the electronic device.
[0129] Example
[0130] The following is explained in conjunction with specific embodiments. The embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If no specific techniques or conditions are indicated in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. If the manufacturer of the reagents or instruments is not indicated, they are all conventional products that can be obtained commercially.
[0131] The benzocyclobutene resin (BCB resin) used in the following examples of this application is It is prepared by the following steps (it can also be prepared according to other known methods in the art or directly purchased commercially in actual application):
[0132] 1. Add benzocyclobutene monosubstituted divinylbenzene monomer into a 50ml single-necked bottle. (0.075 mol), styrene monomer (0.025 mol) and covered with a rubber stopper.
[0133] 2. After vacuuming and passing nitrogen for 3 times, inject toluene and perform thermal polymerization at 100°C. After stirring for 10 hours, cool to room temperature to terminate the reaction. Then, precipitate with methanol and repeat for 3 times to obtain a white powder, namely benzocyclobutene resin (BCB resin).
[0134] Example 1
[0135] The present application embodiment provides a resin composition with low dielectric loss, the preparation of which comprises the steps of:
[0136] 1. Heat and stir 25 parts of naphthol epoxy resin (NC7000L manufactured by Nippon Kayaku Co., Ltd., epoxy equivalent 230 g / mol), 25 parts of bisphenol F epoxy resin (YNF-170 manufactured by Laiwu Runda Co., Ltd., epoxy equivalent 154 g / mol) and 75 parts of vinyl active ester (DFE619 manufactured by Dongcai Technology Co., Ltd., epoxy equivalent 232 g / mol) in 200 parts of butanone solvent until completely dissolved to obtain a mixed solution.
[0137] 2. After the mixed solution is cooled to room temperature, 108 parts of BCB resin (weight average molecular weight Mw: 3-7w, toluene solution with a solid content of 50%), 34.5 parts of hydrogenated styrene-butadiene copolymer (SEBS, toluene solution with a solid content of 65%), 28 parts of hydrogenated polybutadiene (BI-3000 manufactured by Japan Soda Co., Ltd., toluene solution with a solid content of 80%), 65 parts of 1,1-di-tert-butyl cyclohexyl peroxide (PH-C, toluene solution with a solid content of 2%) and 50 parts of dimethylaminopyridine (DMAP, toluene solution with a solid content of 1%) are added to the mixed solution and stirred evenly.
[0138] 3. Finally, add 523.6 parts of spherical silica surface-treated with an epoxy-based coupling agent and disperse evenly with a high-speed rotary mixer to obtain a resin composition with low dielectric loss.
[0139] Example 2
[0140] The present application embodiment provides a resin composition with low dielectric loss, the preparation of which comprises the steps of:
[0141] 1. Heat and stir 25 parts of naphthol epoxy resin (NC7000L manufactured by Nippon Kayaku Co., Ltd., epoxy equivalent 230 g / mol), 25 parts of bisphenol F epoxy resin (YNF-170 manufactured by Laiwu Runda Co., Ltd., epoxy equivalent 154 g / mol) and 75 parts of vinyl active ester (DFE619 manufactured by Dongcai Technology Co., Ltd., epoxy equivalent 232 g / mol) in 200 parts of butanone solvent until completely dissolved to obtain a mixed solution.
[0142] 2. After the mixed solution is cooled to room temperature, 251 parts of BCB resin (weight average molecular weight Mw: 3-7w, toluene solution with a solid content of 50%), 48 parts of hydrogenated styrene-butadiene copolymer (SEBS, toluene solution with a solid content of 65%), 39 parts of hydrogenated polybutadiene (BI-3000 manufactured by Japan Soda Co., Ltd., toluene solution with a solid content of 80%), 100 parts of 1,1-di-tert-butyl cyclohexyl peroxide (PH-C, toluene solution with a solid content of 2%) and 50 parts of dimethylaminopyridine (DMAP, toluene solution with a solid content of 1%) are added to the mixed solution and stirred evenly.
[0143] 3. Finally, add 717.5 parts of spherical silica surface-treated with an epoxy-based coupling agent and disperse evenly with a high-speed rotary mixer to obtain a resin composition with low dielectric loss.
[0144] Example 3
[0145] The present application embodiment provides a resin composition with low dielectric loss, the preparation of which comprises the steps of:
[0146] 1. Heat and stir 25 parts of naphthol epoxy resin (NC7000L manufactured by Nippon Kayaku Co., Ltd., epoxy equivalent 230 g / mol), 25 parts of bisphenol F epoxy resin (YNF-170 manufactured by Laiwu Runda Co., Ltd., epoxy equivalent 154 g / mol) and 75 parts of vinyl active ester (DFE619 manufactured by Dongcai Technology Co., Ltd., epoxy equivalent 232 g / mol) in 200 parts of butanone solvent until completely dissolved to obtain a mixed solution.
[0147] 2. After the mixed solution is cooled to room temperature, 585 parts of BCB resin (weight average molecular weight Mw: 3-7w, toluene solution with a solid content of 50%), 80 parts of hydrogenated styrene-butadiene copolymer (SEBS, toluene solution with a solid content of 65%), 65 parts of hydrogenated polybutadiene (BI-3000 manufactured by Japan Soda Co., Ltd., toluene solution with a solid content of 80%), 184 parts of 1,1-di-tert-butyl cyclohexyl peroxide (PH-C, toluene solution with a solid content of 2%) and 50 parts of dimethylaminopyridine (DMAP, toluene solution with a solid content of 1%) are added to the mixed solution and stirred evenly.
[0148] 3. Finally, add 1168.3 parts of spherical silica surface-treated with an epoxy-based coupling agent and disperse evenly with a high-speed rotary mixer to obtain a resin composition with low dielectric loss.
[0149] Example 4
[0150] The present application embodiment provides a resin composition with low dielectric loss, the preparation of which comprises the steps of:
[0151] 1. Heat and stir 25 parts of naphthol epoxy resin (NC7000L manufactured by Nippon Kayaku Co., Ltd., epoxy equivalent 230 g / mol), 25 parts of bisphenol F epoxy resin (YNF-170 manufactured by Laiwu Runda Co., Ltd., epoxy equivalent 154 g / mol) and 75 parts of vinyl active ester (DFE619 manufactured by Dongcai Technology Co., Ltd., epoxy equivalent 232 g / mol) in 200 parts of butanone solvent until completely dissolved to obtain a mixed solution.
[0152] 2. After the mixed solution is cooled to room temperature, 585 parts of BCB resin (weight average molecular weight Mw: 3-7w, toluene solution with a solid content of 50%), 184 parts of 1,1-di-tert-butyl cyclohexyl peroxide (PH-C, toluene solution with a solid content of 2%) and 50 parts of dimethylaminopyridine (DMAP, toluene solution with a solid content of 1%) are added to the mixed solution and stirred evenly.
[0153] 3. Finally, add 975.3 parts of spherical silica surface-treated with an epoxy-based coupling agent and disperse evenly with a high-speed rotary mixer to obtain a resin composition with low dielectric loss.
[0154] Example 5
[0155] The present application embodiment provides a resin composition with low dielectric loss, the preparation of which comprises the steps of:
[0156] 1. Heat and stir 15 parts of bisphenol F epoxy resin (YNF-170 manufactured by Laiwu Runda Company, epoxy equivalent 154 g / mol) and 27 parts of vinyl active ester (DFE619 manufactured by Dongcai Technology Company, epoxy equivalent 232 g / mol) in 100 parts of butanone solvent until completely dissolved to obtain a mixed solution.
[0157] 2. After the mixed solution is cooled to room temperature, 197 parts of BCB resin (weight average molecular weight Mw: 3-7w, toluene solution with a solid content of 50%), 27 parts of hydrogenated styrene-butadiene copolymer (SEBS, toluene solution with a solid content of 65%), 22 parts of hydrogenated polybutadiene (toluene solution with a solid content of 80%), 63 parts of diisopropylbenzene peroxide (DCP, toluene solution with a solid content of 2%) and 15 parts of dimethylaminopyridine (toluene solution with a solid content of 1%) are added to the solution and stirred evenly.
[0158] 3. Finally, add 409.5 parts of spherical silica surface-treated with an epoxy-based coupling agent and disperse evenly with a high-speed rotary mixer to obtain a resin composition with low dielectric loss.
[0159] Example 6
[0160] The present application embodiment provides a resin composition with low dielectric loss, the preparation of which comprises the steps of:
[0161] 1. Heat and stir 15 parts of bisphenol F epoxy resin (YNF-170 manufactured by Laiwu Runda Company, epoxy equivalent 154 g / mol) and 27 parts of vinyl active ester (DFE619 manufactured by Dongcai Technology Company, epoxy equivalent 232 g / mol) in 100 parts of butanone solvent until completely dissolved to obtain a mixed solution.
[0162] 2. After the mixed solution is cooled to room temperature, 197 parts of divinylbenzene resin (ODV manufactured by NSCM, a toluene solution with a solid content of 50%), 27 parts of hydrogenated styrene-butadiene copolymer (SEBS, a toluene solution with a solid content of 65%), 22 parts of hydrogenated polybutadiene (a toluene solution with a solid content of 80%), 63 parts of diisopropylbenzene peroxide (DCP, a toluene solution with a solid content of 2%) and 15 parts of dimethylaminopyridine (a toluene solution with a solid content of 1%) are added to the solution and stirred evenly.
[0163] 3. Finally, add 409.5 parts of spherical silica surface-treated with an epoxy-based coupling agent and disperse evenly with a high-speed rotary mixer to obtain a resin composition with low dielectric loss.
[0164] Example 7
[0165] The present application embodiment provides a resin composition with low dielectric loss, the preparation of which comprises the steps of:
[0166] 1. Heat and stir 15 parts of bisphenol F epoxy resin (YNF-170 manufactured by Laiwu Runda Company, epoxy equivalent 154 g / mol) and 27 parts of vinyl active ester (DFE619 manufactured by Dongcai Technology Company, epoxy equivalent 232 g / mol) in 100 parts of butanone solvent until completely dissolved to obtain a mixed solution.
[0167] 2. After the mixed solution is cooled to room temperature, 98.5 parts of BCB resin (weight average molecular weight Mw: 3-7w, toluene solution with a solid content of 50%) and 98.5 parts of divinylbenzene resin (ODV manufactured by NSCM, toluene solution with a solid content of 50%), 27 parts of hydrogenated styrene-butadiene copolymer (SEBS, toluene solution with a solid content of 65%), 22 parts of hydrogenated polybutadiene (toluene solution with a solid content of 80%), 63 parts of diisopropylbenzene peroxide (DCP, toluene solution with a solid content of 2%) and 15 parts of dimethylaminopyridine (toluene solution with a solid content of 1%) are added to the solution and stirred evenly.
[0168] 3. Finally, add 409.5 parts of spherical silica surface-treated with an epoxy-based coupling agent and disperse evenly with a high-speed rotary mixer to obtain a resin composition with low dielectric loss.
[0169] Example 8
[0170] The present application embodiment provides a resin composition with low dielectric loss, the preparation of which comprises the steps of:
[0171] 1. Heat and stir 25 parts of naphthol epoxy resin (NC7000L manufactured by Nippon Kayaku Co., Ltd., epoxy equivalent 230 g / mol), 25 parts of bisphenol F epoxy resin (YNF-170 manufactured by Laiwu Runda Co., Ltd., epoxy equivalent 154 g / mol) and 75 parts of vinyl active ester (DFE619 manufactured by Dongcai Technology Co., Ltd., epoxy equivalent 232 g / mol) in 200 parts of butanone solvent until completely dissolved to obtain a mixed solution.
[0172] 2. After the mixed solution is cooled to room temperature, 28 parts of BCB resin (weight average molecular weight Mw: 3-7w, toluene solution with a solid content of 50%), 27 parts of hydrogenated styrene-butadiene copolymer (SEBS, toluene solution with a solid content of 65%), 22 parts of hydrogenated polybutadiene (BI-3000 manufactured by Japan Soda Co., Ltd., toluene solution with a solid content of 80%), 45 parts of 1,1-di-tert-butyl cyclohexyl peroxide (PH-C, toluene solution with a solid content of 2%) and 50 parts of dimethylaminopyridine (DMAP, toluene solution with a solid content of 1%) are added to the mixed solution and stirred evenly.
[0173] 3. Finally, add 416.5 parts of spherical silica surface-treated with an epoxy-based coupling agent and disperse evenly with a high-speed rotary mixer to obtain a resin composition with low dielectric loss.
[0174] Comparative Example 1
[0175] This comparative example provides a resin composition with low dielectric loss, the preparation of which comprises the steps of:
[0176] 1. Heat and stir 25 parts of naphthol epoxy resin (NC7000L manufactured by Nippon Kayaku Co., Ltd., epoxy equivalent 230 g / mol), 25 parts of bisphenol F epoxy resin (YNF-170 manufactured by Laiwu Runda Co., Ltd., epoxy equivalent 154 g / mol) and 112 parts of active ester (DFE617 manufactured by Dongcai Technology Co., Ltd., epoxy equivalent 223 g / mol, butanone solution with a solid content of 65%) in 100 parts of butanone solvent until completely dissolved to obtain a mixed solution.
[0177] 2. After the mixed solution is cooled to room temperature, 21 parts of phenoxy resin (manufactured by Shengquan Technology Co., Ltd., a propylene glycol monomethyl ether solution with a solid content of 30%) and 50 parts of dimethylaminopyridine (a toluene solution with a solid content of 1%) are added to the solution and stirred evenly.
[0178] 3. Finally, add 301 parts of spherical silica surface-treated with an epoxy-based coupling agent and disperse evenly with a high-speed rotary mixer to obtain a resin composition with low dielectric loss.
[0179] In order to verify the progressiveness of the embodiments of the present application, the low dielectric loss resin composition prepared in Examples 1 to 8 and Comparative Example 1 was evenly coated on the release surface of the release film (PET, 50 μm thick) using a coating device, and the coating thickness was set based on the thickness of 50 μm after the film was cured. The coated film was then pre-baked at 100°C for 3 minutes to remove the solvent to obtain a build-up film. The build-up film was then cured under vacuum at 150°C / 30min+200°C / 90min to obtain a cured build-up film for testing the performance of the film. The following performance tests were carried out on each embodiment and comparative example:
[0180] 1. Dielectric loss tangent (Df) determination method: Take a sample of 80*80mm of the cured build-up film, and measure the dielectric loss tangent of the sample by the resonant cavity perturbation method at a measurement frequency of 10GHz and a measurement temperature of 23℃. Measure 3 samples and calculate the average value. Df≤0.002 is judged as excellent; 0.002≤Df≤0.003 is judged as qualified; Df>0.003 is judged as unqualified.
[0181] 2. Determination method of coefficient of thermal expansion (CTE): Use thermomechanical analyzer TMA equipment to measure in the temperature range of 20-260℃ at a heating rate of 10℃ / min, take the second heating curve as the CTE value line, and take the CTE in the range of 25-150℃ as the evaluation value.
[0182] 3. Evaluation of lamination: The resin composition layer of the semi-cured film obtained above is joined to the inner substrate (the "inner substrate" mainly refers to a glass epoxy substrate, a metal substrate, a polyester substrate, a polyimide substrate, a BT resin substrate, a thermosetting polyphenylene ether substrate, etc., which is a circuit substrate with a conductor layer (circuit) formed on one or both sides of the substrate by pattern processing), and then the two are bonded together by heating and pressing to obtain an evaluation substrate. There is no special limitation on the equipment for heating and pressing, such as a commonly used vacuum laminator on the market. In the vacuum lamination method, the heating and pressing temperature is preferably in the range of 70°C to 150°C, the pressure is preferably in the range of 0.5MPa to 1.50MPa, and the heating and pressing time is preferably in the range of 30 seconds to 500 seconds. The lamination of the evaluation substrate after lamination is analyzed to check whether the gaps between the inner substrate circuits are completely filled with the composition in the semi-cured film material and there are no voids. If so, the semi-cured film is judged to have met the lamination standards. If there are voids, it is judged to be unqualified.
[0183] 4. Evaluation of degumming property: The substrate obtained for lamination evaluation is cured at 100-200°C for 15-90 minutes, then immersed in an expansion liquid (alkaline solution) at 30-80°C for 2-20 minutes, then immersed in an oxidant solution (alkaline potassium permanganate solution) at 50-90°C for 10-30 minutes, and finally immersed in a neutralizing solution at 40-80°C for 5-20 minutes to obtain a sample for degumming property evaluation. Judgment standard: The surface of the prepared degumming property evaluation sample is characterized by arithmetic average roughness (Ra), and Ra≤200nm is judged as qualified, and Ra>200nm is judged as unqualified.
[0184] The test results are shown in Table 1 below:
[0185] Table 1
[0186]
[0187]
[0188] Note 1: In the table, “◎” represents excellent, “○” represents good, and “×” represents unqualified.
[0189] Note 2: The amount of each component in the table is the actual amount of non-volatile components remaining after deducting the volatile solvent.
[0190] It can be seen from the above test results that by comparing Examples 1 to 8 of the present application with Comparative Example 1, it can be seen that when a cross-linked polymer resin (A) component is added to the resin composition, the dielectric loss tangent Df of the build-up film after curing can be greatly reduced. In particular, after the proportion of A / (A+B+C) exceeds 30%, ultra-low dielectric loss (Df<0.003) can be achieved. By comparing Examples 1 to 7 and Example 8, it can be seen that when the content of component (A) in the resin composition is low, the effect of improving the dielectric loss performance of the resin composition and the build-up film after curing is not significant enough. When component (A) is not added to the resin composition of Comparative Example 1, the build-up film prepared by the resin composition exhibits the worst dielectric loss performance after curing, and the thermal expansion coefficient is high, and the dimensional stability of the build-up film is relatively poor.
[0191] At the same time, the build-up film prepared by the resin composition of the embodiment of the present application also has good dimensional stability after curing, and the coefficient of thermal expansion CTE ≤ 25ppm / ℃. In addition, because the resin composition contains epoxy resin (B) and curing agent (C) components, the resin composition prepared by the embodiment of the present application and the build-up film prepared therefrom also have good lamination properties. After being laminated and bonded with the inner substrate, the build-up film has a good filling effect on the gaps between the lines on the surface of the inner substrate, and the bonding is tight and the stability is good. In addition, it also has good degumming performance. The surface roughness of the build-up film after degumming is beneficial to the subsequent metallization film layer and the application of the film material.
[0192] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them; although the present application has been described in detail with reference to the aforementioned embodiments, those of ordinary skill in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents; and these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present application, and they should all be included in the scope of the claims and specification of the present application. In particular, as long as there is no structural conflict, the various technical features mentioned in each embodiment can be combined in any way. The scope of protection of the present application is not limited to the specific embodiments disclosed herein, but includes all technical solutions that fall within the scope of the claims. Therefore, the scope of protection of the present application shall be based on the scope of protection of the claims.
Claims
1. A resin composition, characterized in that The resin composition comprises components: a cross-linked polymer resin, an epoxy resin, a curing agent and an inorganic filler; wherein the cross-linked polymer resin comprises at least one of the following chemical structural formulas I: The substituents R1 to R9 are independently selected from one of hydrogen atom, alkyl, alkoxy, ester group or aromatic group, R10 is selected from one of hydrogen atom, benzocyclobutene, alkyl, alkoxy, ester group and aromatic group, n is a positive integer of 4 to 1000, m is a positive integer of 0 to 1000, and n+m is a positive integer not less than 5.
2. The resin composition according to claim 1, characterized in that R1 to R9 are independently selected from a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, an ester group having 1 to 10 carbon atoms, and an aromatic group having 6 to 12 carbon atoms; and / or, The R10 is selected from a hydrogen atom, benzocyclobutene, an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, an ester group having 1 to 10 carbon atoms, and an aromatic group having 6 to 12 carbon atoms.
3. The resin composition according to claim 2, characterized in that The cross-linked polymer resin includes benzocyclobutene resin and / or divinylbenzene resin; wherein the chemical structure of the benzocyclobutene resin is The chemical structural formula of the divinylbenzene resin is 4. The resin composition according to claim 3, characterized in that The benzocyclobutene resin is selected from At least one of .
5. The resin composition according to claim 3, characterized in that The divinylbenzene resin is selected from At least one of the following, wherein a is a positive integer from 4 to 1000, b is a positive integer from 0 to 100, c is a positive integer from 0 to 1000, and d is a positive integer from 0 to 1000.
6. The resin composition according to any one of claims 1 to 5, characterized in that The weight average molecular weight of the cross-linked polymer resin is 1,000 to 1,000,000.
7. The resin composition according to claim 6, characterized in that The weight average molecular weight of the cross-linked polymer resin is 2,000 to 100,000.
8. The resin composition according to any one of claims 1 to 5 or 7, characterized in that In the resin composition, the mass ratio of the cross-linked polymer resin, the epoxy resin and the curing agent is (20-90): (5-60): (5-60).
9. The resin composition according to claim 8, characterized in that In the resin composition, the mass ratio of the total mass of the cross-linked polymer resin, the epoxy resin and the curing agent to the mass ratio of the inorganic filler is 1:(1-9).
10. The resin composition according to any one of claims 1 to 5, 7 or 9, characterized in that The curing agent includes at least one of phenols, cyanates, benzoxazines, carbodiimides, and active esters.
11. The resin composition according to claim 10, characterized in that The curing agent is selected from at least one of phenols, cyanates and active esters modified with at least one functional group including a double bond and a benzocyclobutene group.
12. The resin composition according to any one of claims 1 to 5, 7, 9 or 11, characterized in that The average particle size of the inorganic filler is 0.01 to 10 μm.
13. The resin composition according to claim 12, characterized in that The surface of the inorganic filler is treated with at least one coupling agent selected from the group consisting of aminosilanes, epoxysilanes, double-bond silanes, mercaptosilanes, silanes, and titanates.
14. The resin composition according to claim 13, characterized in that The inorganic filler includes at least one of silicon dioxide, aluminum oxide, glass, cordierite, silicon oxide, barium sulfate, barium carbonate, talc, clay, mica powder, zinc oxide, hydrotalcite, boehmite, aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, magnesium oxide, boron nitride, aluminum nitride, manganese nitride, aluminum borate, strontium carbonate, strontium titanate, calcium titanate, magnesium titanate, bismuth titanate, titanium oxide, zirconium oxide, barium titanate, barium zirconate, barium zirconate, calcium zirconate, zirconium phosphate, and zirconium tungstate phosphate.
15. The resin composition according to claim 14, characterized in that The inorganic filler is selected from at least one of amorphous silica, fused silica, crystalline silica, synthetic silica, hollow silica and spherical silica.
16. The resin composition according to any one of claims 1 to 5, 7, 9, 11, 13 to 15, characterized in that The resin composition further comprises at least one of a curing accelerator, an initiator, a thermoplastic resin and an auxiliary agent.
17. The resin composition according to claim 16, characterized in that The mass ratio of the total mass of the cross-linked polymer resin, the epoxy resin and the curing agent to the mass ratio of the curing accelerator is 100:(0.01-5); and / or, The mass ratio of the total mass of the cross-linked polymer resin, the epoxy resin and the curing agent to the mass ratio of the initiator is 100:(0.05-5); and / or, The mass ratio of the total mass of the cross-linked polymer resin, the epoxy resin and the curing agent to the mass ratio of the thermoplastic resin is 100:(0.5-40); and / or, The mass ratio of the total mass of the cross-linked polymer resin, the epoxy resin and the curing agent to the mass ratio of the auxiliary agent is 100:(0-20).
18. The resin composition according to claim 16, characterized in that The curing accelerator includes at least one of an amine curing accelerator, a phosphorus curing accelerator, an imidazole curing accelerator, a guanidine curing accelerator, and a metal curing accelerator; and / or, The initiator comprises at least one of 1,1-di-tert-butyl cyclohexyl peroxide, diisopropylbenzene peroxide, tert-butyl cumene peroxide, di-tert-butyl peroxide, diisopropylbenzene hydroperoxide, cumene hydroperoxide, and tert-butyl hydroperoxide; and / or, The thermoplastic resin includes at least one of phenoxy resin, polyvinyl acetal resin, polyolefin resin, polyimide resin, polyamide-imide resin, polyetherimide resin, polysulfone resin, polyethersulfone resin, polyphenylene ether resin, polycarbonate resin, polyetheretherketone resin, polyester resin, styrene-butadiene copolymer, hydrogenated styrene-butadiene copolymer, polybutadiene, and hydrogenated polybutadiene; and / or, The auxiliary agent includes at least one of a flame retardant, an organic filler, a thickener, a defoamer, a leveling agent, and a colorant.
19. The resin composition according to any one of claims 1 to 5, 7, 9, 11, 13 to 15, 17 to 18, characterized in that The resin composition further comprises a solvent.
20. A method for preparing a resin composition, characterized in that: The following steps are involved: A cross-linked polymer resin, an epoxy resin, a curing agent and an inorganic filler are prepared into a mixed slurry to obtain a resin composition; wherein the cross-linked polymer resin comprises at least one of the following chemical structural formulas I: The substituents R1 to R9 are independently selected from one of hydrogen atom, alkyl, alkoxy, ester group or aromatic group, R10 is selected from one of hydrogen atom, benzocyclobutene, alkyl, alkoxy, ester group and aromatic group, n is a positive integer of 4 to 1000, m is a positive integer of 0 to 1000, and n+m is a positive integer not less than 5.
21. The method for preparing a resin composition according to claim 20, wherein: The cross-linked polymer resin, the epoxy resin and the curing agent are respectively prepared into solutions, and then mixed with the inorganic filler to obtain the resin composition.
22. The method for preparing a resin composition according to claim 20 or 21, characterized in that: The cross-linked polymer resin is selected from benzocyclobutene resin and / or divinylbenzene resin; wherein the chemical structural formula of the benzocyclobutene resin is The chemical structural formula of the divinylbenzene resin is 23. The method for preparing a resin composition according to claim 22, wherein: In the resin composition, the mass ratio of the cross-linked polymer resin, the epoxy resin and the curing agent is (20-90): (5-60): (5-60); The mass ratio of the total mass of the cross-linked polymer resin, the epoxy resin and the curing agent to the mass ratio of the inorganic filler is 1:(1-9).
24. A build-up adhesive film, characterized in that: The build-up adhesive film is made of the resin composition according to any one of claims 1 to 19, or a resin composition prepared by the method according to any one of claims 20 to 23.
25. The build-up adhesive film according to claim 24, characterized in that: The dielectric loss of the build-up adhesive film after curing is not higher than 0.003, and the thermal expansion coefficient is not higher than 25 ppm / °C.
26. A packaging carrier, characterized in that: The packaging carrier includes the build-up adhesive film as described in claims 24 to 25.
27. An electronic device, characterized in that: The electronic device comprises the packaging carrier as claimed in claim 26.
Citation Information
Patent Citations
Low-dielectric-loss high-heat-conductivity resin composition and preparation method thereof, and prepreg and laminated board prepared from resin composition
CN105585808A
Terminal-modified soluble polyfunctional vinyl aromatic copolymer, and curable resin composition and optical waveguide produced using same
CN107108782A
Benzocyclobutene monomer, benzocyclobutene resin, preparation of benzocyclobutene resin, low-dielectric material and application of low-dielectric material
CN114736096A
Semiconductor package, core layer material, buildup layer material, and sealing resin composition
US20100032826A1
Cited By
Low-CTE layer-adding film and preparation method and application thereof
CN119350950A