Polystyrene foam material and preparation method thereof
Through the use of specific particle size talcum powder and glass fiber compound and graphite carbon black additives, combined with the eccentric rotor volume pulsation deformation plasticizing transport device, the problem of low compressive strength of polystyrene foam materials is solved and a more airtight seal is achieved. The cellular structure and higher compressive strength of polystyrene foam improve its overall performance.
Patent Information
- Application Number
- CN202410889925.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-10-22
AI Technical Summary
The low compressive strength of existing polystyrene foam materials limits their use in certain applications.
Talc powder with a specific particle size and glass fiber of a specific length are used as a nucleating agent, combined with graphite and carbon black as processing aids, and melted and foamed through the eccentric rotor volume pulsating deformation plasticizing transport device to form a more durable product. Polystyrene foam with closed cell structure and increased compressive strength.
It improves the compressive strength and cell wall strength of polystyrene foam materials, while maintaining flame retardant properties, reducing apparent density, and enhancing the overall performance of the material.
Smart Images

Figure CN118812971A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the technical field of foaming materials, and in particular to a polystyrene foaming material and a preparation method thereof. Background Art
[0002] Polystyrene foam material is a rigid foam plastic board made of polystyrene resin as raw material, other raw materials and polymers, which is heated and mixed, and a foaming agent is injected at the same time, and then extruded and pressed to form. It has a perfect closed-cell honeycomb structure. The closed-cell honeycomb structure polystyrene foam material has the advantages of extremely low water absorption, low thermal conductivity, high compressive resistance, anti-aging, light weight, high strength, low water absorption, and convenient construction. It is widely used in building roof insulation, steel structure roof, building wall insulation, building ground insulation, square ground, ground frost heave control, central air conditioning ventilation ducts, etc. However, the existing polystyrene foam material has the disadvantage of low compression strength, which limits the application of polystyrene foam board in some aspects. Summary of the invention
[0003] The purpose of the present invention is to overcome the deficiencies of the prior art and provide a polystyrene foam material and a preparation method thereof.
[0004] To achieve the above object, the technical solution adopted by the present invention is:
[0005] In the first aspect, a polystyrene foam material is provided, comprising the following components in parts by weight: 99-101 parts of polystyrene, 5-10 parts of a nucleating agent, 15-22 parts of a flame retardant, 2-3 parts of a foaming agent, and 0.2-1 parts of a processing aid; the nucleating agent is glass fiber and talcum powder; the mass ratio of the glass fiber to the talcum powder is 2-4; the particle size D95 of the talcum powder is ≤6μm, and the average length of the glass fiber is 15-35μm.
[0006] In some embodiments, the polystyrene has a melt index of 2-5 g / 10 min under 200° C. and 5 kg test conditions.
[0007] In some embodiments, the processing aid includes graphite and carbon black.
[0008] In some embodiments, the mass ratio of the graphite to the carbon black is 1:1-2.
[0009] In some embodiments, the flame retardant is magnesium hydroxide.
[0010] In some embodiments, the particle size D90 of the magnesium hydroxide is ≤2.4 μm.
[0011] In some embodiments, the blowing agent is a combination of CO2, alcohol and HFO-1234ze.
[0012] In a second aspect, a method for preparing the polystyrene foam material is provided, comprising the following steps:
[0013] After the polystyrene, the nucleating agent and the processing aid are uniformly mixed, the flame retardant is added and mixed uniformly to obtain a premix;
[0014] The premix is added into an eccentric rotor volume pulsating deformation plasticizing and conveying device to melt the premix, and then a foaming agent is injected into the melt of the premix, and foaming and extrusion are performed through a heat exchanger, followed by shaping and cooling to obtain a polystyrene foam material.
[0015] In some embodiments, the melting temperature and the extrusion temperature are 170-200°C; and the temperature of the heat exchanger is 110-130°C.
[0016] Compared with the prior art, the beneficial effects of the present invention are as follows: the present invention uses talcum powder with a specific particle size and glass fiber with a specific length as a nucleating agent for a polystyrene foam material. On the one hand, the talcum powder increases the number of pores in the polystyrene foam material and makes the pore size of the polystyrene foam material within the range of 40-100 μm; on the other hand, the glass fiber reduces the damage of the pore wall, makes the pores of the polystyrene foam material have a more closed pore structure, and improves the strength of the pore wall at the same time. The two act synergistically, and on the basis of maintaining the flame retardant performance of the polystyrene foam material, the compressive strength of the polystyrene foam material is improved, and the apparent density of the polystyrene foam material is reduced. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 Schematic diagram of the distribution of nucleating agents in the pores of polystyrene foaming material;
[0018] Figure 2 Schematic diagram of preparing polystyrene foam material using an eccentric rotor volume pulsating deformation plasticizing and transporting device. DETAILED DESCRIPTION
[0019] In order to facilitate understanding of the present disclosure, the present disclosure will be described more fully below. However, the present disclosure can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present disclosure more thorough and comprehensive.
[0020] For simplicity, the present disclosure only explicitly discloses some numerical ranges. However, any lower limit can be combined with any upper limit to form an unclearly recorded range; and any lower limit can be combined with other lower limits to form an unclearly recorded range, and any upper limit can be combined with any other upper limit to form an unclearly recorded range. In addition, although not clearly recorded, each point or single value between the range endpoints is included in the range. Thus, each point or single value can be combined with any other point or single value as its own lower limit or upper limit or with other lower limits or upper limits to form an unclearly recorded range.
[0021] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present disclosure. The terms used herein in the specification of the present disclosure are only for the purpose of describing specific embodiments and are not intended to limit the present disclosure. It should be noted that, unless otherwise stated, the term "and / or" used herein includes any and all combinations of one or more related listed items, and "above" and "below" include the number, and the meaning of "multiple" in "one or more" is more than two.
[0022] The above application contents of the present disclosure are not intended to describe each disclosed embodiment or each implementation in the present disclosure. The following description more specifically illustrates exemplary embodiments. In many places throughout the application, guidance is provided by a series of embodiments, which can be used in various combinations. In each example, enumeration is only used as a representative group and should not be interpreted as exhaustive.
[0023] In a first aspect of the present disclosure, a polystyrene foam material is provided, comprising the following components in parts by weight: 99-101 parts of polystyrene, 5-10 parts of a nucleating agent, 15-22 parts of a flame retardant, 2-3 parts of a foaming agent, and 0.2-1 parts of a processing aid; the nucleating agent is glass fiber and talcum powder; the mass ratio of the glass fiber to the talcum powder is 2-4; the particle size D95 of the talcum powder is ≤6 μm, and the average length of the glass fiber is 15-35 μm.
[0024] Specifically, the weight proportion of the nucleating agent may be, but is not limited to, 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, or 10 parts.
[0025] Specifically, the weight proportion of the flame retardant may be, but is not limited to, 15 parts, 16 parts, 17 parts, 18 parts, 19 parts, 20 parts, 21 parts, or 22 parts.
[0026] Specifically, the weight proportion of the foaming agent may be, but is not limited to, 2 parts, 2.2 parts, 2.4 parts, 2.6 parts, 2.8 parts, or 3 parts.
[0027] Specifically, the weight portion of the processing aid may be, but is not limited to, 0.2 parts, 0.4 parts, 0.6 parts, 0.8 parts, or 1 part.
[0028] Specifically, the mass ratio of the glass fiber to talc powder can be, but is not limited to, 2, 2.2, 2.5, 2.7, 3, 3.3, 3.5, 3.8, or 4.
[0029] Specifically, the particle size D95 of the talc powder can be but is not limited to 6μm, 5.5μm, 5μm, 4.5μm, 4μm, 3.5μm, 3μm, 2.8μm, 2.6μm, 2.4μm, 2.2μm, 2μm, 1.5μm, 1μm; preferably 2.4-2.6μm.
[0030] Specifically, the average length of the glass fiber may be, but is not limited to, 15 μm, 17 μm, 20 μm, 23 μm, 25 μm, 28 μm, 30 μm, 33 μm, or 35 μm.
[0031] The present invention discloses a compound of talcum powder with a specific particle size and glass fiber with a specific length as a nucleating agent for a polystyrene foam material. On the one hand, the talcum powder increases the number of cells of the polystyrene foam material and makes the cell size of the polystyrene foam material within a range of 40-100 μm; on the other hand, the glass fiber reduces the damage of the cell wall, makes the cells of the polystyrene foam material have a more closed cell structure, and improves the strength of the cell wall at the same time. The two act synergistically, and on the basis of maintaining the flame retardant performance of the polystyrene foam material, the compressive strength of the polystyrene foam material is improved, and the apparent density of the polystyrene foam material is reduced.
[0032] like Figure 1 As shown, talcum powder has a layered structure, and glass fiber has a rod-like structure. Glass fiber and talcum powder are evenly distributed in the pores of polystyrene foam material. The particle size D95 of talcum powder will affect the compressive strength and apparent density of polystyrene foam material. If the particle size D95 of talcum powder is greater than 6 μm or the average length of glass fiber is greater than 35 μm, the compressive strength of polystyrene foam material will be significantly reduced, and the apparent density will be significantly increased. If the particle size D95 of talcum powder is too small or the average length of glass fiber is less than 15 μm, glass fiber is difficult to be evenly dispersed in polystyrene foam material, which will significantly reduce the compressive strength of polystyrene foam material and significantly increase the apparent density.
[0033] Specifically, the average diameter of the glass fiber is 5-8 μm.
[0034] In addition, the mass ratio of glass fiber and talcum powder is also one of the key factors affecting the compressive strength and apparent density of polystyrene foam materials. If the mass ratio of glass fiber and talcum powder is <2 or >4, the compressive strength of the polystyrene foam material will decrease significantly and the apparent density will increase significantly.
[0035] Specifically, the particle size D95 of talcum powder is obtained by testing with a Malvern 3000 laser particle size analyzer.
[0036] Specifically, the average length of the glass fiber is obtained by taking 1000 samples and testing them under a microscope and taking the average value.
[0037] The method for controlling the average length of the glass fiber disclosed herein is not limited; for example, the average length of the glass fiber can be controlled by ball milling, and the average length of the glass fiber can be adjusted to a desired range by controlling the parameters of the ball milling, such as the rotation speed and time.
[0038] Specifically, the rotation speed of the ball mill is 80-100 rpm; and the time of the ball mill is 30-60 min.
[0039] In some embodiments, the melt index of the polystyrene under the test conditions of 200° C. and 5 kg is 2-5 g / 10 min; for example, it can be but not limited to 2 g / 10 min, 3 g / 10 min, 4 g / 10 min, and 5 g / 10 min.
[0040] Specifically, the melt index of the polystyrene is tested according to ISO 1133:2005 standard.
[0041] The melt index within the above range can further improve the compressive strength of the polystyrene foam material and reduce the apparent density of the polystyrene foam material.
[0042] In some embodiments, the processing aid includes graphite and carbon black.
[0043] In the present disclosure, graphite and carbon black are used as processing aids, which can further improve the compressive strength of the polystyrene foam material on the one hand, and on the other hand, during the processing, the lubricating effect of graphite and the effect of carbon black on reducing thermal conductivity and thermal expansion ensure a smooth extrusion process and reduce the defective rate of the polystyrene foam material.
[0044] In some embodiments, the mass ratio of graphite to carbon black is 1:1-2, for example, but not limited to, 1:1, 1:1.2, 1:1.4, 1:1.6, 1:1.8, 1:2.
[0045] Selecting graphite and carbon black within the above mass ratio range can further improve the compressive strength and cell uniformity of the polystyrene foam material.
[0046] In some embodiments, the flame retardant is magnesium hydroxide.
[0047] In some embodiments, the particle size D90 of the magnesium hydroxide is ≤2.4 μm, for example, it can be but not limited to 2.4 μm, 2 μm, 1.6 μm, 1.3 μm, 1 μm, or 0.5 μm.
[0048] Specifically, the particle size D90 of magnesium hydroxide is obtained by testing with a Malvern 3000 laser particle size analyzer.
[0049] In some embodiments, the blowing agent is a combination of CO2, alcohol and HFO-1234ze.
[0050] In some embodiments, the mass ratio of CO2, alcohol and HFO-1234ze is CO2: alcohol: HFO-1234ze = 8-10:1-2:1-2, for example, but not limited to 8:2:1, 9:2:2, 10:1:2.
[0051] In a second aspect, a method for preparing the polystyrene foam material is provided, comprising the following steps:
[0052] After the polystyrene, the nucleating agent and the processing aid are uniformly mixed, the flame retardant is added and mixed uniformly to obtain a premix;
[0053] The premix is added into an eccentric rotor volume pulsating deformation plasticizing and conveying device to melt the premix, and then a foaming agent is injected into the melt of the premix, and foaming and extrusion are performed through a heat exchanger, followed by shaping and cooling to obtain a polystyrene foam material.
[0054] The eccentric rotor volume pulsating deformation plasticizing and transporting device used in the present disclosure is the eccentric rotor volume pulsating deformation plasticizing and transporting device described in CN104002447A.
[0055] The use of an eccentric rotor volume pulsating deformation plasticizing and conveying device for melt extrusion can make the flame retardant and nucleating agent more evenly dispersed in the polystyrene matrix, improving the uniformity of the pores and the compression strength of the polystyrene foam material. In addition, the use of an eccentric rotor volume pulsating deformation plasticizing and conveying device for tensile rheology and extrusion does not require secondary foaming of the resulting polystyrene foam material, reducing the number of processes and improving efficiency.
[0056] In some embodiments, the melting temperature is 170-200°C, for example, but not limited to 170°C, 175°C, 180°C, 185°C, 190°C, 195°C, 200°C; the temperature of the heat exchanger is 110-130°C, for example, but not limited to 110°C, 115°C, 120°C, 125°C, 130°C.
[0057] In some embodiments, the screw speed of the eccentric rotor volume pulsation deformation plasticizing and transporting device is 400-500 rpm, for example, it can be but not limited to 400 rpm, 420 rpm, 440 rpm, 460 rpm, 480 rpm, 500 rpm.
[0058] In some embodiments, the mixing speed is 300-600 rpm; the mixing time is 3-10 min.
[0059] The raw materials used in the embodiments and comparative examples are described below, but are not limited to these materials:
[0060] The glass fiber is homemade, and its preparation method is as follows: add commercially available glass fiber into a ball mill, and ball mill it at a rotation speed of 80-100 rpm for 30-60 minutes, and obtain glass fibers with different average lengths by controlling the rotation speed and time of ball milling.
[0061] Glass fiber 1: average length 15 μm;
[0062] Glass fiber 2: average length 25 μm;
[0063] Glass fiber 3: average length 35 μm;
[0064] Glass fiber 4: average length 45 μm;
[0065] Talc 1: D95 = 5 μm, commercially available;
[0066] Talc 2: D95 = 6 μm, commercially available;
[0067] Talc 3: D95 = 15 μm, commercially available;
[0068] Polystyrene: melt index is 3g / 10min at 200℃ and 5kg test conditions, brand: PS158K, manufacturer: BASF-YZ;
[0069] Magnesium hydroxide: D90 = 2.4 μm, commercially available.
[0070] Examples 1-9 and Comparative Examples 1-9
[0071] The components of the polystyrene foam materials described in Examples 1-9 and Comparative Examples 1-9 of the present disclosure are shown in Table 1 and Table 2.
[0072] The method for preparing the polystyrene foam material described in Examples 1-9 and Comparative Examples 1-8 comprises the following steps:
[0073] Add polystyrene, nucleating agent and processing aid into a high-speed mixer in proportion, mix at a speed of 500 rpm for 3 minutes, add flame retardant, and mix at a speed of 500 rpm for 8 minutes to obtain a premix;
[0074] like Figure 2 As shown, the obtained premix is added into an eccentric rotor volume pulsating deformation plasticizing and conveying device (8 temperature zones in total), and the premix is melted in the 1st temperature zone to the 4th temperature zone, the temperature of the 1st temperature zone to the 8th temperature zone is 180° C., and the speed of the screw is 400 rpm;
[0075] Then, in the fifth temperature zone, a blowing agent is injected into the melt of the premix, and in the fifth temperature zone to the eighth temperature zone, the blowing agent and the melt of the first premix are fused to form a gel for foaming. The gel is foamed by a heat exchanger at a temperature of 120° C. After being extruded through a die head, it is shaped and cooled to obtain a polystyrene foam material.
[0076] The flame retardant is magnesium hydroxide; the foaming agent is a composition of CO2, alcohol and HFO-1234ze, the mass ratio of CO2, alcohol and HFO-1234ze in Example 1 is CO2: alcohol: HFO-1234ze = 10:1:2, the mass ratio of CO2, alcohol and HFO-1234ze in Example 2 is CO2: alcohol: HFO-1234ze = 9:2:2, and the mass ratio of CO2, alcohol and HFO-1234ze in Examples 3-9 and Comparative Examples 1-9 is CO2: alcohol: HFO-1234ze = 8:2:1.
[0077] The preparation method of the polystyrene foam material in Comparative Example 9 is different from that in Example 3 only in that a twin-screw extruder is used to replace the eccentric rotor volume pulsation deformation plasticizing and conveying device, and the remaining steps and parameters are the same as those in Example 3.
[0078] Table 1
[0079]
[0080] Table 2
[0081]
[0082]
[0083] Performance Testing
[0084] The polystyrene foam materials obtained in each embodiment and comparative example were subjected to performance tests, and the test methods were as follows:
[0085] 1. Compression strength: tested in accordance with GB / T 8813-2008 standard;
[0086] 2. Apparent total density: tested in accordance with GB / T 6343-2009 standard, the test steps are as follows: prepare the sample after the polystyrene foam material is placed for 72 hours, and the obtained sample is placed at a temperature of 25°C and a humidity of 50% for 16 hours before testing;
[0087] 3. Flame retardant performance: tested according to UL94:1997 standard, the evaluation results are HBF, HF-1, HF-2, HF-1 is the best, HF-2 is the second, and HBF is the worst.
[0088] The test results are shown in Table 3.
[0089] Table 3
[0090]
[0091]
[0092] It can be seen from Table 3 that the compression strength of the polystyrene foam material disclosed in the present invention is 3.5-4.2 MPa, and the apparent density is 0.041-0.059 g / cm 3 , the flame retardant property is HF-1.
[0093] By comparing Examples 3-6 and Comparative Examples 7-8, it can be seen that the mass ratio of glass fiber to talcum powder affects the compressive strength and apparent density of the polystyrene foam material. When the mass ratio of glass fiber to talcum powder is <2 or >4, the compressive strength of the obtained polystyrene foam material decreases significantly and the apparent density increases significantly.
[0094] By comparing Example 3, Examples 7-8 and Comparative Example 6, it can be seen that the average length of the glass fiber is one of the factors affecting the compressive strength and apparent density of the polystyrene foam material. When the average length of the glass fiber is >35 μm, the compressive strength of the obtained polystyrene foam material decreases significantly and the apparent density increases significantly.
[0095] By comparing Example 3, Example 9 and Comparative Example 5, it can be seen that when the particle size D95 of talc powder is greater than 6 μm, the compressive strength of the obtained polystyrene foam material is significantly reduced and the apparent density is significantly increased.
[0096] It can be seen from Comparative Example 3 and Comparative Examples 1-4 that when at least one of talcum powder, glass fiber and flame retardant is missing, the compressive strength of the obtained polystyrene foam material is significantly reduced and the apparent density is significantly increased.
[0097] By comparing Example 3 and Comparative Example 9, it can be seen that, compared with the twin-screw extruder, the eccentric rotor volume pulsation deformation plasticizing and conveying device can improve the dispersion uniformity of each component, improve the compressive strength and flame retardant properties of the polystyrene foam material, and reduce the apparent density of the polystyrene foam material.
[0098] Finally, it should be noted that the above embodiments are used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A polystyrene foam material, characterized in that: The invention comprises the following components in parts by weight: 99-101 parts of polystyrene, 5-10 parts of nucleating agent, 15-22 parts of flame retardant, 2-3 parts of foaming agent and 0.2-1 parts of processing aid; the nucleating agent is glass fiber and talcum powder; the mass ratio of the glass fiber to the talcum powder is 2-4; the particle size D95 of the talcum powder is ≤6 μm, and the average length of the glass fiber is 15-35 μm.
2. The polystyrene foam material according to claim 1, characterized in that: The polystyrene has a melting index of 2-5 g / 10 min under the test conditions of 200° C. and 5 kg.
3. The polystyrene foam material according to claim 1, characterized in that: The processing aids include graphite and carbon black.
4. The polystyrene foam material according to claim 3, characterized in that: The mass ratio of the graphite to the carbon black is 1:1-2.
5. The polystyrene foam material according to claim 1, characterized in that: The flame retardant is magnesium hydroxide.
6. The polystyrene foam material according to claim 5, characterized in that: The particle size D90 of the magnesium hydroxide is ≤2.4 μm.
7. The polystyrene foam material according to claim 1, characterized in that: The foaming agent is a composition of CO2, alcohol and HFO-1234ze.
8. The polystyrene foam material according to claim 7, characterized in that: The mass ratio of CO2, alcohol and HFO-1234ze is CO2: alcohol: HFO-1234ze = 8-10: 1-2: 1-2.
9. A method for preparing a polystyrene foam material according to any one of claims 1 to 8, characterized in that: The following steps are involved: After the polystyrene, the nucleating agent and the processing aid are uniformly mixed, the flame retardant is added and mixed uniformly to obtain a premix; The premix is added into an eccentric rotor volume pulsating deformation plasticizing and conveying device to melt the premix, and then a foaming agent is injected into the melt of the premix, and foaming and extrusion are performed through a heat exchanger, followed by shaping and cooling to obtain a polystyrene foam material.
10. The preparation method according to claim 9, characterized in that: The melting temperature is 170-200°C; the temperature of the heat exchanger is 110-130°C.
Citation Information
Patent Citations
Eccentric rotor volume pulsation deformation plasticizing transport method and device
CN104002447A