Stretch blow molded article, toner bottle, method for producing stretch blow molded article, molded article, and pellet

By adding inorganic layered double hydroxide and zeolite in PET bottle recycling, combined with stretch blow molding technology, the problems of wax migration to the surface and poor forming in PET bottle recycling are solved, achieving high strength and image uniformity. Toner bottle.

CN118813005APending Publication Date: 2024-10-22CANON KK
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410469156.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-04-21
Filing Date
2024-04-18
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

In the existing PET bottle recycling process, material recycling causes the molecular weight of PET resin to decrease, resulting in rapid crystallization during stretch blow molding and poor molding. In toner bottles, wax migrates to the surface and causes chemical attack, resulting in uneven image density.

Method used

Using a combined material containing polyester, wax, and an inorganic layered double hydroxide and zeolite, and using stretch blow molding technology, the wax is prevented from migrating to the surface of the molded product and the deformation of the surface of the toner particles is suppressed.

Benefits of technology

It effectively prevents wax from migrating to the surface of the molded product, avoids toner deterioration, and improves the strength of the molded product and the uniformity of image formation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118813005A_ABST
    Figure CN118813005A_ABST
Patent Text Reader

Abstract

The invention relates to a stretch blow molded article, a toner bottle, a method for manufacturing the stretch blow molded article, a molded article, and pellets. A stretch blow molded article comprising: a polyester; wax; and at least one selected from the group consisting of inorganic layered double hydroxides and zeolites.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a stretch blow molded product, a toner bottle, and a method for producing the stretch blow molded product. In addition, the present disclosure relates to a molded product and a pellet. Background Art

[0002] For an electrophotographic image forming apparatus, a toner bottle for supplying toner and the like needs to have strength sufficient to prevent breakage even when dropped, etc. Therefore, a molded product obtained by injection stretch blow molding of polyethylene terephthalate (hereinafter may be referred to as "PET") as a polyester resin is also often used. For example, Japanese Patent Application Publication No. 2001-042626 discloses a toner bottle manufactured by stretch blow molding.

[0003] In recent years, from the viewpoint of environmental protection, recycling of beverage PET bottles as PET bottles has been widely carried out. Here, as a recycling method of PET, chemical recycling and material recycling are known, as described in paragraphs

[0008] and

[0009] of Japanese Patent Application Publication No. 2014-198422.

[0004] As disclosed in Japanese Patent Application Gazette No. 2000-169623, chemical recycling requires a multi-step (multistage) process, and for this purpose, decomposition equipment and purification treatment equipment become necessary, resulting in high recycling costs. In addition, the environmental load is also large. On the other hand, PET obtained by material recovery (hereinafter also referred to as "material recovery PET" or "MR-PET") can be hydrolyzed by absorbing moisture in the air by the PET resin and then heating for granulation, which can lead to a decrease in molecular weight. In addition, as the molecular weight of the PET resin decreases, the time required for crystallization is shortened (THE NIKKANKOGYO SHIMBUN, LTD., SATURATED POLYESTER RESIN HANDBOOK, YUGI KAZUO, first edition December 22, 1989, p. 224 to p. 225).

[0005] Thus, even when stretch blow molding is attempted using a preform formed of PET with a reduced molecular weight, PET rapidly crystallizes during the stretching process. Therefore, it is more likely to cause poor molding. As a method for compensating for the defects of material recycling, mechanical recycling that additionally includes the steps of repolymerization and intrinsic viscosity adjustment as described in paragraph

[0010] of Japanese Patent Application Publication No. 2014-198422 is known. Summary of the invention

[0006] Solid phase polymerization for repolymerizing PET with reduced molecular weight requires a large amount of heat energy and has a large environmental load. In addition, in material recycling, a step of cleaning the bottle is generally performed. However, the cleaning of the bottle can be performed multiple times using water, acid or alkali, etc., and in addition, a drying step is required. Therefore, the cleaning of the bottle also increases the environmental load.

[0007] From the viewpoint of reducing environmental load, the inventors simplified or omitted the cleaning of the toner bottle to be recycled, obtained MR-PET from the toner bottle still including the toner attached to the inside thereof, and manufactured the toner bottle using the MR-PET again. Then, the inventors found the following. When the toner is contained in the toner bottle thus obtained, the surface of the toner particles may be deformed at the contact point between the toner in the toner bottle and the inner surface of the toner bottle. The toner particles with the deformed surface may cause poor development, and the poor development may cause uneven image density in the electrophotographic image.

[0008] The present inventors speculate that the reason for deformation on the surface of the toner contained in the toner bottle formed using the MR-PET obtained from the toner bottle still having the toner attached thereto is as follows. That is, it is considered that the toner bottle mixes the wax contained in the toner. Then, it is considered that at least a part of the mixed wax exists on the surface inside the toner bottle. Then, it is considered that the contact between the toner contained in the toner bottle and the wax exposed on the inner side surface of the toner bottle deforms the surface of the toner particles. The deformation phenomenon of the surface of the toner particles due to the wax may be referred to as a chemical attack hereinafter.

[0009] At least one aspect of the present disclosure is intended to provide a stretch blow molded product that can prevent wax from migrating to the surface of the blow molded product under the premise that polyester including wax is used as a raw material. In addition, at least another aspect of the present disclosure is intended to provide a toner bottle that can prevent the toner contained from deteriorating. In addition, at least another aspect of the present disclosure is intended to provide a method for manufacturing a stretch blow molded product that can prevent wax from migrating to the surface of the blow molded product under the premise that polyester including wax is used as a raw material.

[0010] In addition, at least one aspect of the present disclosure is to provide a molded product that can prevent wax from migrating to the surface when polyester including wax is used as a raw material. In addition, at least one aspect of the present disclosure is to provide a pellet that helps to inhibit wax from migrating to the surface of a molded product.

[0011] At least one aspect provides a stretch blow molded article comprising:

[0012] Polyester;

[0013] wax; and

[0014] At least one selected from the group consisting of inorganic layered double hydroxides and zeolites.

[0015] At least one aspect provides a toner bottle comprising:

[0016] Polyester;

[0017] wax; and

[0018] At least one selected from the group consisting of inorganic layered double hydroxides and zeolites.

[0019] At least one aspect provides a method for manufacturing the stretch blow molded product, the method comprising:

[0020] a step of preparing a preform comprising polyester, wax, and at least one selected from the group consisting of an inorganic layered double hydroxide and a zeolite; and

[0021] A step of forming a stretch blow molded product by stretch blow molding the preform.

[0022] In addition, at least one aspect provides a molded article comprising:

[0023] Polyester;

[0024] wax; and

[0025] At least one selected from the group consisting of inorganic layered double hydroxides and zeolites.

[0026] In addition, at least one aspect provides a pellet comprising:

[0027] Polyester;

[0028] wax; and

[0029] At least one selected from the group consisting of inorganic layered double hydroxides and zeolites.

[0030] According to at least one aspect of the present disclosure, a stretch blow molded product can be obtained that can prevent wax from migrating to the surface of the blow molded product under the premise that polyester including wax is used as a raw material. In addition, according to at least one aspect of the present disclosure, a toner bottle can be obtained that can prevent the contained toner from deteriorating. In addition, according to at least one aspect of the present disclosure, a method for manufacturing a stretch blow molded product that can prevent wax from migrating to the surface of the blow molded product under the premise that polyester including wax is used as a raw material can be obtained. Further features of the present invention will become apparent from the description of the following exemplary embodiments with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 is a schematic diagram of an image forming apparatus;

[0032] Figure 2 is a schematic diagram showing a method of forming a preform;

[0033] Figure 3 is a schematic diagram showing a blow molding method;

[0034] Figure 4 It is a schematic diagram of one-step blow molding;

[0035] Figure 5 is a schematic diagram showing the migration of wax components; and

[0036] Figure 6 It is a schematic diagram of a blow molded bottle. DETAILED DESCRIPTION

[0037] Next, examples of embodiments for carrying out the present disclosure will be described in detail with reference to the accompanying drawings. In the present disclosure, unless otherwise specified, the descriptions "from XX to YY" and "XX to YY" indicating a numerical range indicate a numerical range including the lower limit and the upper limit of the range as endpoints. In the case of describing the numerical range in sections, the upper and lower limits of each numerical range can be arbitrarily combined.

[0038] As mentioned above, wax incorporated into recycled polyesters such as MR-PET is believed to cause chemical attack. Figure 5 As shown in FIG. 1 , during the molding process of the toner bottle when the temperature of the PET resin 201 becomes equal to or higher than the glass transition temperature, the wax 202 migrates to the surface of the bottle. Above the glass transition temperature of the PET resin 201, the thermal movement of the PET resin 201 becomes intense. Thus, the wax 202 migrates from the gaps in the PET resin 201 to the surface of the bottle.

[0039] Under such circumstances, the present inventors recognized the following. Even a stretch blow molded product from a raw material including recycled polyester derived from a toner bottle requires technical development to obtain a stretch blow molded product that is less likely to cause chemical attack to the toner in contact with its surface. As a result of the present inventors' continued research based on this recognition, they found the following stretch blow molded product that is less likely to cause chemical attack to the toner in contact with its surface.

[0040] That is, the stretch blow molded product according to at least one aspect of the present disclosure contains polyester, wax, and at least one selected from the group consisting of an inorganic layered double hydroxide and zeolite.

[0041] As a result of the research by the present inventors, they found the following: The presence of at least one selected from the group consisting of an inorganic layered double hydroxide and a zeolite in the polyester containing wax can prevent chemical attack.

[0042] The reason for this is considered to be as follows. At least one member selected from the group consisting of an inorganic layered double hydroxide and a zeolite (hereinafter also referred to as zeolite, etc.) adsorbs the wax, which suppresses the migration of the wax to the surface of the toner bottle. In particular, the toner tends to be charged by friction with other members. Therefore, it is considered that at least a portion of the toner remaining in the toner bottle is charged. Then, it is considered that the state in which the toner is charged is maintained even in the form of MR-PET, and it is considered that at least a portion of the wax included in the MR-PET is also charged. It is considered that the wax thus charged tends to be adsorbed by zeolite, etc.

[0043] During the use of a toner bottle in an electrophotographic image forming apparatus, the toner is subjected to friction. Therefore, the toner (including the wax included in the toner) is charged. The charged state of the toner is maintained even in the form of MR-PET, so the wax included in the MR-PET is generally charged. It is considered as follows. At least one selected from the group consisting of an inorganic layered double hydroxide and a zeolite (hereinafter also referred to as zeolite, etc.) adsorbs the charged wax, which can inhibit the wax from migrating to the bottle surface.

[0044] Therefore, the stretch blow molded product according to the present disclosure can be obtained by stretch blow molding of a preform as a molded product molded from a resin mixture containing polyester, wax, and at least one selected from the group consisting of an inorganic layered double hydroxide and zeolite.

[0045] Prefab

[0046] The preform for stretch blow molding preferably comprises the following (a), (b) and (c).

[0047] (a) Wax

[0048] (b) at least one selected from the group consisting of an inorganic layered double hydroxide and a zeolite, and

[0049] (c) Polyester

[0050] Zeolite and the like are covered by the skin layer of polyester when the preform of the bottle precursor is formed, and are less likely to precipitate to the surface of the bottle. This hinders the migration of adsorbed wax to the surface of the bottle. This effect tends to prevent chemical attack of the wax.

[0051] Polyester

[0052] There is no particular limitation on the polyester, and known polyester resins can be used. The polyester may be a thermoplastic polyester. The polyester preferably comprises at least one selected from the group consisting of polyethylene terephthalate and polyethylene naphthalate. The polyester more preferably comprises polyethylene terephthalate (PET). PET can be obtained by, for example, a condensation reaction or an ester exchange reaction between terephthalic acid or its ester-forming derivative and 1,2-ethylene glycol or its ester-forming derivative. In addition, the polyester may be a mixture with other resins. The polyester preferably comprises PET in an amount of 60 to 100% by mass, more preferably 80 to 100% by mass, and further preferably 90 to 100% by mass.

[0053] The polyester is, for example, recycled polyester. The polyester may be MR-PET, and may be virgin material PET whose molecular weight is not reduced. However, the polyester is MR-PET obtained by recycling a toner bottle so that the effect according to the present disclosure is significantly produced. Therefore, the polyester is preferably a material recycled polyester, and more preferably a material recycled PET.

[0054] The weight average molecular weight of the polyester is preferably 20,000 to 80,000, more preferably 35,000 to 45,000. For example, the measurement of the weight average molecular weight is performed using gel permeation chromatography (GPC).

[0055] Inorganic layered double hydroxide

[0056] The stretch blow molded product, molded product and pellets each contain at least one selected from the group consisting of inorganic layered double hydroxides and zeolites. Incidentally, the presence of inorganic layered double hydroxides and zeolites in the stretch blow molded product, molded product or pellets can be confirmed by measurement using micro FT-IR.

[0057] Examples of the inorganic layered double hydroxide may include kaolin and mica. Examples of more effective and readily available compounds include hydrotalcite compounds represented by the following general formula (1). The inorganic layered double hydroxide preferably contains a hydrotalcite compound.

[0058] General formula (1): M 2+ (1-X) M 3+ X (OH) 2 A n- (X / n) ·mH 2 O

[0059] (where 0 <X≤0.5,m≥0,M 2+ :such as Mg 2+ or Zn 2+ The divalent metal ion, M 3+ : Such as Al 3+ or Fe3+ The trivalent metal ion, A n- :such as CO 3 2- , Cl - or NO 3 - n-valent anion, wherein n is an integer greater than 1)

[0060] The hydrotalcite compound represented by the general formula (1) comprises a positively charged base layer [M 2+ (1-X) M 3+ X (OH) 2 ] X+ and the negatively charged middle layer [A n- (X / n) ·mH 2 O] X- The intercalation compound is a layered compound and can be considered to be an intercalation compound obtained by inserting an intermediate layer into a base layer. Generally, it is known that intercalation compounds exhibit specific chemical properties (reactivity). In the case of a hydrotalcite compound represented by the general formula (1), it is known that anions (A) present in the ionic intermediate layer n- ) and negative ions are easily replaced (anion exchange). Although the mechanism of anion exchange is still uncertain, it is speculated that the electrical interaction (attraction) between the basic layer and the negative ions, the size of the gaps in the middle layer (the thickness of the middle layer) and adsorption play a role in it.

[0061] In the general formula (1), preferably, the divalent metal ion M 2+ Mg 2+ , and the trivalent metal ion M 3+ It's Al 3+ In addition, the n-valent anion is preferably CO 3 2- or Cl - .

[0062] Based on the mass of the stretch blow molded product, molded product or pellet, the content of the inorganic layered double hydroxide is preferably 0.09 to 1.2 mass%, more preferably 0.1 to 1.0 mass%. When the content is 0.09 mass% or more, the wax can be more fully adsorbed, so that the wax becomes less likely to migrate to the bottle surface. When the content is 1.2 mass% or less, the inorganic layered double hydroxide is less likely to become the starting point of rupture when the preform is blown. By setting the mixing amount within the aforementioned range, it becomes easier to balance chemical attack suppression and blow molding.

[0063] Zeolite

[0064] Zeolites are hydrous aluminosilicates containing alkali metals or alkaline earth metals, and the hydrous aluminosilicates include a rigid anionic framework having regular channels (tubular pores) and cavities (hollows). There is no particular limitation, and natural or artificial (synthetic) zeolites can be used.

[0065] In addition, zeolites represented by the following composition are preferred.

[0066] (M I ,M II 1 / 2 ) m (Al m Si n O 2(m+n) )· x H 2 O,(n≥m)

[0067] M I :Li + ,Na + ,K + , etc., M II :Ca 2 +,Mg 2 +,Ba 2 +, etc.

[0068] M I Preferably Na + . M II Preferably Ca 2+ . m is preferably from 1 to 384. n is preferably from 0 to 27.

[0069] Zeolites include zeolites having various framework structures. That is, the framework structures of zeolites include LTA type, FER type, MWW type, MFI type, MOR type, LTL type, FAU type, BEA type, etc. certified by the International Zeolite Association. In the present disclosure, although zeolites with any framework structure can be used, the MFI type is preferred. The MFI type (ZSM-5) is a aluminosilicate zeolite having a framework structure in which five-membered ring units are connected in a chain, and the chemical formula of the unit lattice of the units is represented by [Na m Al m Si 96-m O 192 ·16H 2 O(0<m<27)].

[0070] Based on the mass of the stretch blow molded product (molded product or pellet), the content of zeolite is preferably 0.09 to 1.2 mass%, more preferably 0.1 to 1.0 mass%. When the content is 0.09 mass% or more, wax can be more fully adsorbed, making it less likely that wax will migrate to the surface of the bottle. When the content is 1.2 mass% or less, zeolite is less likely to become a starting point for cracking when the preform is blow molded. By setting the mixing amount within the aforementioned range, it becomes easier to balance chemical attack suppression and blow molding properties.

[0071] From the viewpoint of achieving both chemical attack suppression and blow moldability, the total content of the inorganic layered double hydroxide and zeolite is preferably 0.09 to 1.2 mass %, more preferably 0.1 to 1.0 mass %, based on the mass of the stretch blow molded product (molded product or pellet).

[0072] The content ratio of inorganic layered double hydroxide and zeolite in stretch blow molded products (molded products or pellets) can be measured in the following manner. After measuring the mass of the stretch blow molded products, the stretch blow molded products are placed in a container made of stainless steel, and then placed in an oven at 480°C for 1 hour to burn the resin of the blow molded products. Subsequently, ion exchange water is placed in a container made of stainless steel including residue. After sufficient stirring, filter through a nylon mesh with an opening size that prevents inorganic layered double hydroxide and zeolite from passing through. The opening size can be selected in consideration of the size of other materials other than inorganic layered double hydroxide and zeolite. After filtration, the moisture is removed by a 100°C oven and the mass is measured. The mass of the nylon mesh is subtracted therefrom. As a result, the content ratio can be measured. With this method, catalysts, carbon black, etc. included in the resin pass through the nylon mesh. Therefore, the content ratio of inorganic layered double hydroxide and zeolite can be accurately measured. When the inorganic layered double hydroxide and zeolite cannot be separated by filtration alone, the contents can be measured by further combining known means.

[0073] The number average particle size of the inorganic layered double hydroxide and zeolite is preferably 0.05 to 2.00 μm, more preferably 0.10 to 1.50 μm. A number average particle size of 0.05 μm or more results in good dispersibility in the resin. A number average particle size of 2.00 μm or less makes it difficult to form foreign matter during blow molding, which tends to suppress the breakage of the molded product.

[0074] wax

[0075] The wax includes the following waxes. Examples thereof may include aliphatic hydrocarbon waxes such as low molecular weight polyethylene, low molecular weight polypropylene, polyolefin copolymers, polyolefin waxes, microcrystalline waxes, paraffin waxes, and Fischer-Tropsch waxes; oxides of aliphatic hydrocarbon waxes such as polyethylene oxide waxes; or block copolymers thereof; plant waxes such as candelilla wax, carnauba wax, Japan wax, and jojoba wax; animal waxes such as beeswax, lanolin, and spermaceti; mineral waxes such as ozokerite, ceresin, and vaseline; waxes including aliphatic esters as main components such as montanic acid ester waxes and castor waxes; and those waxes obtained by deoxidizing part or all of aliphatic esters such as deoxidized carnauba waxes.

[0076] In addition, examples may include saturated straight-chain fatty acids such as palmitic acid, stearic acid, montanic acid, or long-chain alkyl carboxylic acids having a longer chain alkyl group; unsaturated fatty acids such as brassinoic acid, eleostearic acid, and stearidonic acid; saturated alcohols such as stearyl alcohol, arachidyl alcohol, behenyl alcohol, carnauba alcohol, hexacosanol, triacontanol, or alkyl alcohols having a longer chain alkyl group; polyols such as sorbitol; aliphatic amides such as linoleic acid amide, oleic acid amide, and lauric acid amide; saturated aliphatic bisamides such as methylene bisstearic acid amide, ethylene biscapric acid amide, ethylene bislauric acid amide, and hexamethylene bisstearic acid amide; unsaturated fatty acid amides, Such as ethylenebisoleamide, hexamethylenebisoleamide, N,N'-dioleyladipamide and N,N'-dioleylsebacamide; aromatic bisamides, such as meta-xylene bisstearamide and N,N'-distearylisophthalamide; fatty acid metal salts (those commonly referred to as metal soaps), such as calcium stearate, calcium laurate, zinc stearate and magnesium stearate; waxes obtained by grafting aliphatic hydrocarbon waxes with vinyl monomers such as styrene or acrylic acid; partial esterification products of fatty acids and polyols, such as monoglyceride of behenic acid; and methyl ester compounds having a hydroxyl group obtained by hydrogenating vegetable oils and fats.

[0077] In addition, it is preferred to use those waxes obtained by sharpening the molecular weight distribution of the wax using a pressurized sweating method, a solvent method, a recrystallization method, a vacuum distillation method, a supercritical gas extraction method or a melt crystallization method. Alternatively, it is also preferred to use those waxes obtained by removing low molecular weight solid fatty acids, low molecular weight solid alcohols, low molecular weight solid compounds and other impurities.

[0078] The presence of wax in the stretch blow molded product (molded product or pellet) can be confirmed by GPC-FTIR.

[0079] Specific examples of the wax may include VISKOL (registered trademark) 330-P, 550-P, 660-P, and TS-200 (manufactured by Sanyo Chemical Industries, Ltd.), Hi-WAX 400P, 200P, 100P, 410P, 420P, 320P, 220P, 210P, and 110P (MITSUI CHEMICAL Inc.), SASOL H1, H2, C80, C105, and C77 (Schumann Sasol Co.), HNP-1, HNP-3, HNP-9, HNP-10, HNP-11, and HNP-12 (NIPPON SEIRO CO., LTD.), UNILIN (registered trademark) 350, 425, 550, and 700, UNICID (registered trademark) 350, 425, 550, and 700 (TOYO PETROLITE CO.), Japan wax, beeswax, rice wax, candelilla wax and carnauba wax (available at CERARICA NODA CO., LTD.).

[0080] Based on the mass of the stretch blow molded product (molded product or pellet), examples of the content ratio of the wax in the stretch blow molded product (molded product or pellet) may include 0.001 to 0.100 mass%, 0.002 to 0.050 mass%, and 0.002 to 0.030 mass%. When the content ratio of the wax falls within the aforementioned range, the wax can be more reliably prevented from affecting the stretch blow molding property of the preform.

[0081] Incidentally, the quantification of the presence of wax in the PET resin can be obtained by measurement using, for example, pyrolysis GC / MS.

[0082] In the stretch blow molded product (molded product or pellet), the total content of the inorganic layered double hydroxide and the zeolite is preferably 400 to 5000 parts by mass, more preferably 450 to 4600 parts by mass, relative to 100 parts by mass of the wax.

[0083] The stretch blow molded product (molded product or pellet) may contain carbon black. For example, carbon black may be added to the stretch blow molded product for appearance reasons. Examples of the content (mixing amount) of carbon black in the stretch blow molded product (molded product or pellet) may include 0.01 to 0.20 mass % and 0.02 to 0.10 mass %.

[0084] Manufacturing of stretch blow molded products

[0085] Next, one aspect of a method for producing a stretch blow molded product such as a toner bottle by biaxial stretch blow molding will be described below. The method for producing the stretch blow molded product has a step of preparing a preform containing polyester, wax and at least one selected from the group consisting of an inorganic layered double hydroxide and a zeolite, and a molding step of stretch blow molding the preform and obtaining the stretch blow molded product.

[0086] First, an example of a method for producing pellets used as a material for a preform for biaxial stretch blow molding of a stretch blow molded product will be shown. For example, in the step of preparing the preform, polyester, wax, and at least one selected from the group consisting of an inorganic layered double hydroxide and a zeolite are melt-kneaded to form the pellets. Forming into pellets makes the material composition uniform, which facilitates forming.

[0087] The wax may be a toner containing wax. More specifically, polyester, an electrophotographic toner containing wax, and at least one selected from the group consisting of an inorganic layered double hydroxide and a zeolite are melt-kneaded to form pellets.

[0088] It is also acceptable to: previously mix or melt-knead at least one selected from the group consisting of an inorganic layered double hydroxide and a zeolite with a polyester to obtain a modified polyester, and mix or melt-knead a toner containing a wax therewith.

[0089] In addition, for example, a toner bottle containing polyester to which an electrophotographic toner containing wax is attached may be used. That is, the step of preparing the preform preferably has a step of crushing a recovered toner bottle to which an electrophotographic toner is attached and obtaining a crushed product, a step of melt-kneading the crushed product and at least one selected from the group consisting of an inorganic layered double hydroxide and a zeolite and forming a pellet, and a step of forming a preform from the formed pellet. Then, preferably, the electrophotographic toner contains wax, and the toner bottle contains polyester.

[0090] The amount of the electrophotographic toner is preferably 0.100 to 1.000 mass %, more preferably 0.150 to 0.500 mass %, based on the total amount of the toner bottle and the electrophotographic toner attached to the toner bottle.

[0091] There is no particular restriction on the melt-kneading method, and a known method such as a twin-screw extruder can be used. The temperature of the melt-kneading can only allow the melt-kneading of the polyester and is not particularly limited. The temperature is, for example, 120 to 300° C., preferably 260 to 280° C. The conditions for the melt-kneading are also not particularly limited. After the melt-kneading, cooling is performed, and the melt-kneaded product can be formed into a pellet shape that can be injection molded using a known method such as a granulator.

[0092] After melt kneading and pellet formation, a step of crystallizing the pellets may be employed. Crystallization of the pellets improves processability for manufacturing a preform. Crystallization may be achieved by maintaining the pellets at preferably 100 to 180° C., more preferably 130 to 170° C., preferably for 1 to 12 hours, more preferably for about 3 to 7 hours. Incidentally, even when the pellets are crystallized, the pellets may be rendered amorphous by heating at the time of preform manufacturing.

[0093] Then, the obtained pellets are used as Figure 2 As shown, a preform 104 having a test tube shape is formed by injection molding. Specifically, a heating cylinder 105 heats the material loaded into the injection molding machine 101 and makes the material in a molten state. An extrusion screw 207 injects the molten material into preform molds 102 and 103. The material is cooled and then taken out of the mold to obtain a preform 104. In the step of preparing the preform, it is preferred to obtain the preform from the obtained pellets by injection molding. In addition, the preform preferably has a test tube shape.

[0094] Next, the forming step will be described. In the forming step, as Figure 3 As shown, biaxial stretch blow molding (biaxial stretch forming) of the preform 104 is performed. First, the preform 104 is placed in a heating furnace 107 and heated to a temperature that allows stretching. The heating time of this step is preferably within 3 minutes. By setting the heating time to within 3 minutes, the crystallization of the polyester in the preform during heating can be prevented. The heated preform 104 is taken out from the heating furnace 107 and arranged at the mouth of a blow mold 108, which includes a cavity formed inside by combining a left mold 108-1 and a right mold 108-2.

[0095] Incidentally, the preform 104 is preferably placed at the mouth of the blow mold in a short time (e.g., within 10 seconds) to prevent the temperature of the heated preform 104 from decreasing before the biaxial stretching step. As a result, the crystallization of the polyester in the preform due to the gradual cooling of the preform can be prevented from proceeding.

[0096] The heated preform 104 disposed in the blow mold 108 is stretched in the length direction using the stretch rod 109. This stretching is called primary stretching. For the primary stretching, it is preferred that the gas is flowed in such a way that the preform 104 does not contact the stretch rod 109. The pressure of the gas in this step is called the primary blow molding pressure.

[0097] After the primary stretching is performed, the gas 110 flows in from the preform mouth 106, and the preform 104 expands in the transverse direction (circumferential direction). This is called secondary stretching. In addition, the pressure of the gas in this step is called secondary blow molding pressure. Examples of the gas blown in may include air, nitrogen, carbon dioxide, and argon.

[0098] By performing the primary stretching and the secondary stretching, the preform 104 expands in the directions indicated by the arrows 301, comes into close contact with the inner wall of the blow mold 108, and is cooled and solidified in this state to obtain the blow molded product 112. The molding step preferably includes a step of stretching the preform 104 in the longitudinal direction of the preform 104 using a stretching rod and a step of flowing a gas into the preform 104 stretched in the longitudinal direction and stretching the preform 104 in the circumferential direction of the preform 104.

[0099] Then, the blow molded product 112 is taken out from the blow mold 108 by separating the left mold 108-1 and the right mold 108-2 of the blow mold 108. The blow molded product 112 is stretched in both the longitudinal and transverse directions, and thus becomes a molded product having high strength.

[0100] Therefore, in the stretching step of injection stretch blow molding, the preform is preferably amorphous (in an amorphous state). When the blow molding temperature is reached in the amorphous state, the resin is stretched and crystallized in the stretching direction by performing blow molding as it is, that is, biaxial stretch molding. This enables the formation of a bottle with high strength.

[0101] Injection stretch blow molding methods include a one-step method and a two-step method. The one-step method is a method of stretch blow molding using the residual heat of the preform immediately after being taken out of the mold as it is or under temperature adjustment. The two-step method is a method of stretch blow molding by temporarily cooling the preform to room temperature and then adjusting the temperature of the preform again.

[0102] In the case of a one-step method, Figure 4 As shown, after the preform 104 is injection molded from the injection molding machine 101, cooling is terminated in a short time of less than 10 seconds during injection molding to prevent the temperature of the preform 104 from becoming equal to or lower than the glass transition temperature of the resin. Then, it is immediately kept warm and heated to a blow molding temperature (for example, from 90° C. to 120° C.), and blow molding is performed to obtain a blow molded bottle 112. An apparatus including an integrated injection molding device and a blow molding device is used.

[0103] The two-step method is a method in which after injection molding a preform, the preform is cooled to below the glass transition temperature of the resin, taken out, and then heated to a blow molding temperature (e.g., from 90° C. to 120° C.) by another blow molding device for blow molding. An apparatus including a separate injection molding device and a blow molding device is used. For example, after molding the preform in the step of preparing the preform, the preform is cooled to below the glass transition temperature of the polyester. Then, the molding step is performed.

[0104] The one-step process is preferred because the preform is not cooled below the glass transition temperature and therefore requires less reheating energy than the two-step process.

[0105] Next, a description will be given of a method of confirming chemical attack on a toner bottle obtained by biaxial stretch blow molding.

[0106] The toner is contained in a toner bottle obtained by biaxial stretch blow molding. The toner bottle including the toner contained therein is placed in a use environment. In order to evaluate the chemical attack, the use environment is set to 50°C for 72 hours, and the toner bottle is placed in a constant temperature bath for testing. The toner bottle exposed to the use environment is taken out, and the toner adhered to the inner surface of the bottle among the toner contained in the toner bottle is taken out. When the toner containing port of the bottle is inverted to discharge the toner from the bottle and the toner adhered to the inner surface of the bottle is adhered by an adhesive tape or the like, the toner can be easily pulled out. The pulled out toner is observed with an electron microscope or the like to observe the deformation of the surface of the toner particles. As a result, for the toner particles subjected to the chemical attack, traces of deformation can be observed on the contact surface with the toner bottle.

[0107] Image forming equipment

[0108] Next, the image forming apparatus will be described below with reference to the drawings. Figure 1 1 is a schematic configuration explanatory diagram showing an electrophotographic four-color image forming apparatus, wherein reference numeral 80 denotes a main body of the image forming apparatus. The image forming apparatus 80 is configured as a so-called intermediate transfer tandem type image forming apparatus in which four-color image forming sections are arranged side by side on an intermediate transfer belt.

[0109] The image forming apparatus 80 performs image formation as follows. In the image forming apparatus 80, first, respective electrostatic latent images are formed on the photosensitive drums 17 (17y, 17m, 17c, 17bk) by the exposure devices 50 (50y, 50m, 50c, 50bk) based on the print data. In the image forming apparatus 80, the formed electrostatic latent images are developed by respective developing devices 21 (21y, 21m, 21c, 21bk) to form respective toner images.

[0110] In the image forming apparatus 80, the toner image is transferred to the intermediate transfer body 62 by the primary transfer device 60 (60y, 60m, 60c, 60bk), and the resulting toner image is transferred to the sheet S supplied from the paper supply device 63 in the secondary transfer section 64 (64a, 64b). In the image forming apparatus 80, the toner image transferred to the sheet S is fixed on the sheet S by the fixing device 68, and then discharged onto the paper discharge tray 70.

[0111] In the image forming apparatus 80, in which a toner image is formed by the developing apparatus 21, detachable toner bottles 3 (3Y, 3M, 3C, 3Bk) are used for the purpose of supplying respective toners to the developing apparatus 21. Therefore, the toner bottle according to at least one aspect of the present disclosure is used in the above manner.

[0112] The toner bottle contains polyester, wax, and at least one selected from the group consisting of an inorganic layered double hydroxide and zeolite.

[0113] Example

[0114] The present disclosure will be described in detail below by way of examples and comparative examples. However, the present disclosure is not limited to the examples. In the following examples and comparative examples, unless otherwise specified, "%" means "mass %".

[0115] Toner bottle manufacturing

[0116] Using a one-step blow molding device (ASB-70DPH, manufactured by NISSEI ASB MACHINE CO., LTD.), the Figure 6 The toner bottle 3 shown (total length 439.5 mm, diameter 101 mm) was blow-molded at a stretch ratio of "longitudinal ratio x transverse ratio = 6.7".

[0117] The "longitudinal ratio" of the blow molding stretch ratio is a value calculated by dividing the "total length after stretching" by the "total length (before stretching) of the portion (heating portion) of the preform reaching the stretching temperature".

[0118] The "transverse ratio" of the blow molding stretch ratio is a value calculated by dividing the "diameter of the middle portion after stretching" by the "diameter of the middle portion of the preform (before stretching)".

[0119] First, the materials described in the following Table 1 were melt-kneaded and then pelletized to prepare a masterbatch having a carbon black concentration of 5% by mass.

[0120] [Table 1]

[0121]

[0122] Then, the masterbatch having a carbon black concentration of 5% by mass prepared above and PET were mixed in the ratio shown in Table 2 below, and the resulting mixture was melt-kneaded and then granulated to obtain pellets of the resin mixture. The resulting pellets were dried at a temperature of 150° C. for 5 hours.

[0123] [Table 2]

[0124]

[0125] Blow molding conditions

[0126] The pellets of the resin mixture dried as described above were charged into an injection molding device of a one-step stretch blow molding machine (product name: ASB-70DPH; Nissei ASB Machine Co., Ltd.) and subjected to biaxial stretch blow molding to mold a toner bottle. The one-step stretch blow molding machine sequentially performs a step of obtaining a preform in a test tube shape by injection molding and a step of subjecting the preform to biaxial stretch blow molding to produce a bottle-shaped molded product (one-step method). The screw diameter of the injection molding machine in the molding machine is 54 mm.

[0127] As a preform molding die, a die capable of molding a preform having an outer diameter of 30 mm, a wall thickness of 3.7 mm, and a length of 220 mm was first prepared, and the preform was molded under the following molding conditions.

[0128] -Screw diameter: 54mm

[0129] - Screw position before filling the cavity with resin mixture: 95mm

[0130] -Injection speed

[0131] Until the screw advances 5 mm: 50% of the maximum speed

[0132] Until the screw advances 20 mm further: 30% of maximum speed

[0133] Until the screw advances 35 mm further: 25% of maximum speed

[0134] PV switch position: 35mm

[0135] -Injection pressure

[0136] -Until PV switching: 12.0MPa

[0137] -After PV switching: 4.5MPa (maintaining pressure)

[0138] -Pressure holding time after PV switching

[0139] -4.57 seconds

[0140] -Heating tube temperature: 280℃

[0141] -Cooling time: 8.0 seconds

[0142] -Mold temperature: 18℃

[0143] Once the cooling time of 8.0 seconds had elapsed, the preform was then demoulded and transported to the biaxial stretch blow molding station of a one-step stretch blow molding machine. The temperature of the preform during transport was controlled as follows.

[0144] -Preform heating temperature

[0145] Position of 10% of the total length of the preform from the top of the preform: 180°

[0146] Position of 25% of the total length of the preform from the top of the preform: 200°

[0147] Position of 50% of the total length of the preform from the top of the preform: 200°C

[0148] Position of 75% of the total length of the preform from the top of the preform: 180°

[0149] The preform adjusted to the above temperature was set in a cylindrical mold having a size corresponding to that of a toner bottle and having a temperature adjusted to 18° C., and subjected to biaxial stretch blow molding to produce a blow molded bottle. The preform being conveyed was heated so that the surface temperature of the central portion of the preform was 100° C. immediately before entering the cylindrical mold.

[0150] First, the stretch rod is inserted into the preform through the opening of the preform from the retracted position, and is driven forward until it contacts the top of the preform. The air pressure driving the stretch rod is set to 1.2 MPa, so that the stretch rod is further driven forward. Then, 0.5 seconds after the further advancement of the stretch rod begins, primary air is introduced into the preform through the opening of the preform. The pressure of the primary air is set to 1.0 MPa. Subsequently, secondary air is introduced 0.15 seconds after the introduction of the primary air. The pressure of the secondary air is set to 2.9 MPa. From the beginning of the introduction of the primary air, air is introduced into the preform after 7.0 seconds. Then, the pressure in the preform is restored to normal pressure after 2.5 seconds. Thus, a toner bottle produced by blow molding is obtained. The bottle is a toner bottle of virgin PET that has not been recycled.

[0151] According to the above method, 200 toner bottles using virgin PET were prepared.

[0152] Example 1-1

[0153] Production of recycled pellets

[0154] Two hundred unused toner cartridges filled with black toner (trade name: Toner NPG-67; manufactured by CANON INC.) were prepared. The black toner included wax. The entire amount of black toner in each toner cartridge was transferred to 200 toner bottles prepared as described above. Thereafter, the opening of the toner bottle was made vertically downward to discharge the black toner inside thereof. After this operation, a small amount of black toner still adhered to the inner wall of each toner bottle.

[0155] In this step, the amount of black toner remaining in the toner bottle was 0.321% by mass based on the mass of the toner bottle body on an average value of 200 toner bottles. Incidentally, here, the mass of the toner bottle body is the mass of the toner bottle and the toner remaining only inside it after all supply components etc. installed in the toner bottle are removed.

[0156] Then, each toner bottle was pulverized into a size of about 5 to 10 mm square using a pulverizer to obtain a pulverized product (hereinafter also referred to as a "flake product"). For the obtained flake product, the wax content was measured using GPC and FT-IR, and it was found that the wax content was 0.022 parts by mass per 100 parts by mass of the flake product.

[0157] To 99.5% by mass of the flake product, a hydrotalcite compound (trade name: DHT-4C, manufactured by Kyowa Chemical Industry Co., Ltd.) as an inorganic layered double hydroxide was added in an amount of 0.5% by mass, and the resulting mixture was melt-kneaded using a twin-screw extruder (PC-46, manufactured by IKEGAI Co., Ltd.) at a temperature of 260° C., a screw speed of 200 rpm, and a discharge rate of 50 kg / h, and then granulated. The inorganic layered double hydroxide used here is in a filler shape and has a number average particle diameter of 0.38 μm.

[0158] The pellets obtained by melt-kneading with an extruder were kept at a temperature of 150° C. for 5 hours, thereby crystallizing the pellets for molding (this recycled material is referred to as MR-PET (1-1)).

[0159] Blow molded bottle manufacturing

[0160] MR-PET (1-1) was loaded into a one-step stretch blow molding machine, and biaxial stretch blow molding was performed in the same manner as the blow molding conditions (the obtained toner bottle is referred to as toner bottle (1-1)). The toner was contained in the toner bottle (1-1), and a confirmation test of chemical attack was performed under an environment of 50° C. for 72 hours. As a result, even when the toner attached to the inner surface of the toner bottle was observed, no deformation of the surface of the toner particles was confirmed.

[0161] Toner bottles (1-2) and (1-3) and a comparative toner bottle (1-4) were obtained by blow molding in the same manner as in Example 1-1, except that the mixing ratio of the flake product and the inorganic layered double hydroxide (hydrotalcite-based compound) was changed as shown in Table 3. All the toner bottles could be blow molded without any problem.

[0162] For each of the obtained toner bottles, deformation of the toner particle surface was observed in the same manner as in Example 1-1.

[0163] [Table 3]

[0164]

[0165] Toner Bottle(1-2)

[0166] In the case where the addition amount of the inorganic layered double hydroxide was 1.0 mass %, the preform was subjected to biaxial stretching blow molding. As a result, the blow molding could be performed without any problem. The evaluation of chemical attack was performed using the toner bottle (1-2). As a result, even when the toner attached to the inner surface of the toner bottle was observed, no deformation of the toner particle surface was confirmed.

[0167] Toner Bottles (1-3)

[0168] In the case where the addition amount of the inorganic layered double hydroxide was 0.1 mass %, biaxial stretch blow molding of the preform was performed. As a result, blow molding could be performed without problems. Evaluation of chemical attack was performed using the toner bottle (1-3). As a result, even when the toner attached to the inner surface of the toner bottle was observed, no deformation of the toner particle surface was confirmed.

[0169] Compare Toner Bottles (1-4)

[0170] When the addition amount of the inorganic layered double hydroxide was 0.0 mass %, the preform was subjected to biaxial stretch blow molding. As a result, the blow molding could be carried out without any problem. The evaluation of chemical attack was carried out using comparative toner bottles (1-4). As a result, deformation of the surface of the toner particles attached to the inner surface of the toner bottle was confirmed, and chemical attack occurred. The reason is considered to be as follows. When the inorganic layered double hydroxide is not added, the wax causing the chemical attack is not adsorbed by the inorganic layered double hydroxide, and thus the wax migrates to the inner surface of the toner bottle. As a result, chemical attack occurred.

[0171] Production of recycled pellets

[0172] Example 2-1

[0173] Zeolite (trade name: SILTON MT-8000; manufactured by Mizusawa Industrial Chemicals, Ltd.) was added in an amount of 0.5% by mass to 99.5% by mass of the flake product prepared in the same manner as in Example 1-1, and the resulting mixture was melt-kneaded using a twin-screw extruder (PC-46, manufactured by IKEGAI Co., Ltd.) at a temperature of 260° C., a screw speed of 200 rpm, and a discharge rate of 50 kg / h, and then pelletized. The zeolite used here was in the form of a filler. The pellets obtained by melt-kneading with the aid of an extruder were kept at a temperature of 150° C. for 5 hours to crystallize the pellets for molding (this recycled material is referred to as MR-PET (2-1)).

[0174] Blow molded bottle manufacturing

[0175] MR-PET (2-1) was loaded into a one-step stretch blow molding machine, and biaxial stretch blow molding was performed in the same manner as the blow molding conditions (the obtained toner bottle is referred to as toner bottle (2-1)). The toner was contained in the toner bottle (2-1), and a confirmation test of chemical attack was performed under an environment of 50° C. for 72 hours. As a result, even when the toner attached to the inner surface of the toner bottle was observed, no deformation of the toner particle surface was confirmed.

[0176] Toner bottles (2-2) and (2-3) and a comparative toner bottle (2-4) were obtained by blow molding in the same manner as in Example 2-1, except that the mixing ratio of the flake product and zeolite was changed as shown in Table 4. All the toner bottles could be blow molded without any problem.

[0177] For each of the obtained toner bottles, deformation of the toner particle surface was observed in the same manner as in Example 2-1.

[0178] [Table 4]

[0179]

[0180] Toner Bottle(2-2)

[0181] When the addition amount of zeolite was 1.0 mass %, the preform was subjected to biaxial stretch blow molding. As a result, the blow molding could be performed without any problem. The evaluation of chemical attack was performed using the toner bottle (2-2). As a result, even when the toner attached to the inner surface of the toner bottle was observed, no deformation of the toner particle surface was confirmed.

[0182] Toner Bottles (2-3)

[0183] In the case where the addition amount of zeolite was 0.1 mass %, biaxial stretch blow molding of the preform was performed. As a result, blow molding could be performed without problems. Evaluation of chemical attack was performed using the toner bottle (2-3). As a result, even when the toner attached to the inner surface of the toner bottle was observed, no deformation of the toner particle surface was confirmed.

[0184] Compare Toner Bottles (2-4)

[0185] When the addition amount of zeolite was 0.0 mass %, biaxial stretch blow molding of the preform was performed. As a result, blow molding could be performed without problems. Evaluation of chemical attack was performed using comparative toner bottles (2-4). As a result, deformation on the surface of the toner particles attached to the inner surface of the toner bottle was confirmed, and chemical attack occurred. The reason is considered to be as follows. When zeolite is not added, the wax that causes the chemical attack is not adsorbed by the zeolite. Therefore, the wax migrates to the inner surface of the toner bottle, and chemical attack occurs.

[0186] While the present invention has been described with reference to exemplary embodiments, it is to be understood that the invention is not limited to the disclosed exemplary embodiments. The scope of the following claims is to be accorded the broadest interpretation so as to encompass all such modifications and equivalent structures and functions.

Claims

1. A stretch blow molded product comprising: Polyester; wax; and At least one selected from the group consisting of inorganic layered double hydroxides and zeolites.

2. The stretch blow molded product according to claim 1, wherein The total content of the inorganic layered double hydroxide and the zeolite is 0.09 to 1.2% by mass based on the mass of the stretch blow molded article.

3. The stretch blow molded product according to claim 1 or 2, wherein The inorganic layered double hydroxide comprises a hydrotalcite compound.

4. The stretch blow molded product according to claim 1 or 2, wherein The polyester is recycled polyester.

5. The stretch blow molded product according to claim 1 or 2, wherein The polyester includes at least one selected from the group consisting of polyethylene terephthalate and polyethylene naphthalate.

6. The stretch blow molded product according to claim 1 or 2, wherein The stretch blow molded product is a toner bottle.

7. A toner bottle, comprising: Polyester; wax; and At least one selected from the group consisting of inorganic layered double hydroxides and zeolites.

8. The method for producing a stretch blow molded product according to any one of claims 1 to 6, wherein the method include: a step of preparing a preform comprising the polyester, the wax, and at least one selected from the group consisting of the inorganic layered double hydroxide and the zeolite; and A step of stretch blow molding the preform to obtain the stretch blow molded product.

9. The method for producing a stretch blow molded product according to claim 8, wherein The steps of preparing the preform include: a step of crushing a recovered toner bottle to which electrophotographic toner is attached and obtaining a crushed product; The step of melt-kneading the pulverized product and at least one selected from the group consisting of the inorganic layered double hydroxide and the zeolite to form pellets; and The step of forming the preform from the formed granules, wherein The electrophotographic toner comprises the wax, and The toner bottle includes the polyester.

10. A molded article comprising: Polyester; wax; and At least one selected from the group consisting of inorganic layered double hydroxides and zeolites.

11. A pellet comprising: Polyester; wax; and At least one selected from the group consisting of inorganic layered double hydroxides and zeolites.