Water-based composite ceramic coating and preparation method thereof

By adding raw materials such as kaolin and silicon nitride whiskers to the water-based composite ceramic coating and optimizing the formula, the problem of insufficient corrosion resistance and flexibility of the coating on the cookware substrate is solved, and better anti-corrosion and toughness effects are achieved.

CN118813136APending Publication Date: 2024-10-22JIANGMEN ANNUOTE COOKING UTENSILS MFG
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411041579.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

Existing water-based coatings have poor corrosion resistance and insufficient flexibility on cookware substrates, causing the sprayed iron layer to easily deform and crack the surface coating when stress is released.

Method used

By adding raw materials such as kaolin and silicon nitride whiskers to water-based composite ceramic coatings and optimizing the formula system, the permeability and flexibility of the coating are improved to form a coating with superior performance.

Benefits of technology

It significantly improves the corrosion resistance and flexibility of the coating, enhances the anti-corrosion effect on the cookware base material, and reduces the problem of coating cracking caused by deformation under heat.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004972520210000051
    Figure BDA0004972520210000051
  • Figure BDA0004972520210000052
    Figure BDA0004972520210000052
  • Figure BDA0004972520210000061
    Figure BDA0004972520210000061
Patent Text Reader

Abstract

The invention relates to a water-based composite ceramic coating and a preparation method thereof, and belongs to the technical field of ceramic coatings applied to cooking utensils, the ceramic coating comprises a component A, a component B, a component C and a component D, the component A comprises silica sol, alumina sol, fumed silica, titanium dioxide, kaolin, pigment, silicon nitride whisker, sericite, isopropanol, magnesium lithium silicate and deionized water; the component B comprises alkyl silane, propylene glycol monomethyl ether and an organic silicon flatting agent; the component C comprises formic acid and acetic acid; and the component D comprises silicon polymer resin, propylene glycol monomethyl ether and isopropanol. The soft kaolin, the silica sol and the aluminum sol are added in the preparation process, so that the anti-corrosion effect of the coating is improved; the beta-type silicon nitride whisker, the fumed silica micropowder and the sericite are added, so that the toughness of the composite ceramic coating is improved; in addition, the water-based polyester modified organic silicon resin is also added, so that the obtained water-based composite ceramic coating can improve the binding force of a coating on a cooker base material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of ceramic coatings applied to cookware, and in particular, relates to a water-based composite ceramic coating applied on a fusion-sprayed iron substrate and a preparation method thereof. Background Art

[0002] Aluminum cookware is a common base material for cookware. Among them, electromagnetic induction products often use hot-melt sprayed iron layers as magnetic and thermal conductive materials, and are mainly used in mid-to-high-end products. For the protective decoration of the hot-melt sprayed iron layer, environmentally friendly water-soluble or water-based coatings have been developed earlier. However, since the gaps in the hot-melt sprayed iron layer have reached 8-12%, water-based coatings with stronger permeability and better corrosion resistance are now needed. At the same time, due to the large difference in the thermal expansion coefficients of aluminum and iron, the hot-melt sprayed iron layer is easy to deform and crack its surface coating when stress is released. Therefore, it is now necessary to improve the flexibility of water-based coatings.

[0003] Based on the above problems, it is of great practical significance to provide a coating for a cookware substrate having excellent corrosion resistance and flexibility. Summary of the invention

[0004] The purpose of the present invention is to provide a water-based composite ceramic coating and a preparation method thereof, which can effectively solve the problems of poor corrosion resistance and insufficient flexibility of water-based coatings on cookware substrates in the prior art by adding appropriate proportions of kaolin and silicon nitride whiskers and optimizing the coating formula system.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] A water-based composite ceramic coating, comprising component A, component B, component C and component D;

[0007] The component A comprises the following raw materials: silica sol, aluminum sol, fumed silica, titanium dioxide, kaolin, pigment, silicon nitride whisker, sericite, isopropyl alcohol, lithium magnesium silicate and deionized water;

[0008] The B component includes the following raw materials: alkyl silane, propylene glycol methyl ether and silicone leveling agent;

[0009] The C component includes the following raw materials: formic acid and acetic acid;

[0010] The D component includes the following raw materials: silicone polymer resin, propylene glycol methyl ether and isopropyl alcohol.

[0011] As a preferred technical solution of the present invention, the mass ratio of component A, component B, component C and component D is 50-55:25-30:0.4-0.6:15-20.

[0012] As a preferred technical solution of the present invention, the silica sol in component A is 30-40 parts by weight, the aluminum sol is 20-30 parts by weight, the fumed silica is 3-6 parts by weight, the titanium dioxide is 10-15 parts by weight, the kaolin is 4-8 parts by weight, the pigment is 5-10 parts by weight, the silicon nitride whisker is 2-4 parts by weight, the sericite is 2-4 parts by weight, the isopropyl alcohol is 5-10 parts by weight, the lithium magnesium silicate is 0.2-0.5 parts by weight and the deionized water is 6-10 parts by weight.

[0013] Furthermore, the silica sol includes nano silica sol with a particle size of 10-30nm and nano silica sol with a particle size of 80-120nm; the fumed silica is micron-sized, i.e., fumed silica micropowder; the titanium dioxide is rutile titanium dioxide; the kaolin is 4000 mesh soft kaolin; the pigment is high-purity copper chromium black; and the silicon nitride whiskers are 50-150nm β-type silicon nitride whiskers.

[0014] Furthermore, the mass ratio of the 10-30 nm nano silica sol to the 80-120 nm nano silica sol is 1:1.

[0015] As a preferred technical solution of the present invention, the alkylsilane in component B includes at least one of n-propyltriethoxysilane and phenyltriethoxysilane.

[0016] Furthermore, the n-propyltriethoxysilane is 40-50 parts by weight, the phenyltriethoxysilane is 35-45 parts by weight, the propylene glycol methyl ether is 7-9 parts by weight, and the organosilicon leveling agent is 0.3 parts by weight.

[0017] Furthermore, the silicone leveling agent includes but is not limited to BYK-310 and BYK-381.

[0018] As a preferred technical solution of the present invention, the mass ratio of formic acid to acetic acid in component C is 1:1.

[0019] As a preferred technical solution of the present invention, the silicone polymer resin in component D is 70-80 parts by weight, propylene glycol methyl ether is 7-9 parts by weight, and isopropyl alcohol is 10-13 parts by weight.

[0020] Furthermore, the silicone polymer resin includes water-based polyester-modified silicone resin.

[0021] Furthermore, the water-based polyester-modified silicone resin includes any one of a polyacrylate-modified silicone resin and a polyurethane-modified silicone resin.

[0022] Furthermore, the molecular weight of the water-based polyester-modified silicone resin is 80,000-100,000.

[0023] A method for preparing a water-based composite ceramic coating, the preparation method specifically comprising the following steps:

[0024] S1. Preparation of component A: 10-30 nm nano silica sol, fumed silica, lithium magnesium silicate, titanium dioxide, kaolin, pigment, silicon nitride whisker, sericite, isopropyl alcohol and deionized water are stirred and mixed at a controlled speed, ground, and aluminum sol and 80-120 nm nano silica sol are added and mixed to obtain component A;

[0025] S2, preparation of component B: n-propyl triethoxysilane, phenyl triethoxysilane, propylene glycol methyl ether and an organosilicon leveling agent are mixed and stirred at a controlled speed to obtain component B;

[0026] S3, preparation of component C: mixing formic acid and acetic acid and stirring uniformly to obtain component C;

[0027] S4, preparation of component D: uniformly mixing silicone polymer resin, propylene glycol methyl ether and isopropyl alcohol and stirring at a controlled speed to obtain component D;

[0028] S5. Preparation of finished product: Mix component B and component C evenly to obtain mixture A, pre-stir component A at a controlled speed and add mixture A while stirring at the same speed, control the temperature and stir to obtain mixture B, add component D to mixture B and stir and mix evenly at a controlled speed to obtain a finished water-based composite ceramic coating.

[0029] Here, when mixture A is added to component A, the alkyl silane in component B contained in mixture A will be hydrolyzed into silanol in an acidic environment, and the silanol and silanol on the surface of the silica sol particles in component A are very active, and the interaction between the silica sol ions and the silanol produced by the hydrolysis of component B undergo self-condensation polymerization to form polysiloxanes with different alkyl groups; in addition, by adding component D to the above-mentioned mixture B and stirring evenly, a water-based composite ceramic coating with excellent performance can be obtained.

[0030] As a preferred technical solution of the present invention, the speed of the controlled stirring in step S1 is 1200-1300 rpm for 1-2 hours; the grinding is performed for 8-10 hours until the fineness is ≤3 μm.

[0031] As a preferred technical solution of the present invention, the speed of the controlled stirring in step S3 is 500-600 rpm, and the time is 0.5-1 h.

[0032] As a preferred technical solution of the present invention, the speed of the controlled stirring in step S4 is 1200-1300 rpm, and the time is 0.5-1 h.

[0033] As a preferred technical solution of the present invention, the speed of the speed-controlled pre-stirring of component A in step S5 is 400-600rpm; the temperature of the temperature-controlled stirring is 45-50°C, and the time is 4-5h; the speed of the speed-controlled stirring is 400-600rpm.

[0034] Beneficial effects of the present invention:

[0035] (1) The present invention adds soft kaolin, silica sol and aluminum sol to the water-based composite ceramic coating, thereby enhancing the permeability of the coating to the gaps of the cookware substrate and improving the anti-corrosion effect of the coating on the cookware substrate.

[0036] (2) The present invention adds β-silicon nitride whiskers, fumed silica powder and sericite to the water-based composite ceramic coating, thereby increasing the toughness of the composite ceramic coating and effectively reducing the cracking of the coating due to deformation of the cookware substrate in a hot state.

[0037] (3) The present invention adds water-based polyester modified silicone resin, and the obtained water-based composite ceramic coating can improve the bonding force of the coating on the cookware substrate. DETAILED DESCRIPTION

[0038] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0039] The water-based polyester modified silicone resin used in the embodiment of the present invention

[0040] Example 1

[0041] A water-based composite ceramic coating and a preparation method thereof, wherein the ceramic coating comprises component A, component B, component C and component D in a mass ratio of 53:270:0.5:18;

[0042] The A component includes the following raw materials by weight:

[0043]

[0044] The silica sol comprises a nano silica sol with a particle size of 30 nm and a nano silica sol with a particle size of 80 nm in a mass ratio of 1:1;

[0045] The B component includes the following raw materials by weight:

[0046]

[0047] The C component includes the following raw materials by weight:

[0048] 50 parts of formic acid;

[0049] 50 parts of acetic acid;

[0050] The D component includes the following raw materials by weight:

[0051] 75 parts of polyacrylate modified silicone resin;

[0052] Propylene glycol methyl ether 8 parts;

[0053] 13 parts of isopropyl alcohol;

[0054] The molecular weight of the polyacrylate-modified silicone resin is 90,000;

[0055] A method for preparing a water-based composite ceramic coating, the preparation method specifically comprising the following steps:

[0056] S1. Preparation of component A: 30 nm nano silica sol, fumed silica powder, lithium magnesium silicate, rutile titanium dioxide, 4000 mesh soft kaolin, copper chrome black, 50 nm β-silicon nitride whisker, sericite, isopropanol and deionized water were mixed at a controlled speed of 1300 rpm for 1 h, ground, and aluminum sol and 80 nm nano silica sol were added, mixed evenly to obtain component A;

[0057] S2. Preparation of component B: n-propyl triethoxysilane, phenyl triethoxysilane, propylene glycol methyl ether and BYK-310 were mixed and stirred at a controlled speed of 550 rpm for 0.5 h to obtain component B;

[0058] S3, preparation of component C: mixing formic acid and acetic acid and stirring uniformly to obtain component C;

[0059] S4, preparation of component D: polyacrylate modified silicone resin, propylene glycol methyl ether and isopropanol were mixed uniformly and stirred at a controlled speed of 1300 rpm for 1 hour to obtain component D;

[0060] S5. Preparation of finished product: Mix component B and component C evenly to obtain mixture A, pre-stir component A at a controlled speed of 400 rpm and add mixture A while stirring at this speed, control the temperature at 45°C and stir for 5 hours to obtain mixture B, add component D to mixture B and control the speed at 600 rpm to stir and mix evenly to obtain a finished water-based composite ceramic coating.

[0061] Example 2

[0062] A water-based composite ceramic coating and a preparation method thereof, wherein the ceramic coating comprises component A, component B, component C and component D in a mass ratio of 55:25:0.4:20;

[0063] The A component includes the following raw materials by weight:

[0064]

[0065]

[0066] The silica sol comprises a nano silica sol with a particle size of 20 nm and a nano silica sol with a particle size of 120 nm in a mass ratio of 1:1;

[0067] The B component includes the following raw materials by weight:

[0068]

[0069] The C component includes the following raw materials by weight:

[0070] 50 parts of formic acid;

[0071] 50 parts of acetic acid;

[0072] The D component includes the following raw materials by weight:

[0073] 70 parts of polyacrylate modified silicone resin;

[0074] Propylene glycol methyl ether 7 parts;

[0075] 10 parts of isopropyl alcohol;

[0076] The molecular weight of the polyacrylate-modified silicone resin is 100,000;

[0077] A method for preparing a water-based composite ceramic coating, the preparation method specifically comprising the following steps:

[0078] S1. Preparation of component A: 20 nm nano silica sol, fumed silica powder, lithium magnesium silicate, rutile titanium dioxide, 4000 mesh soft kaolin, copper chrome black, 100 nm β-type silicon nitride whisker, sericite, isopropanol and deionized water were mixed at a controlled speed of 1200 rpm for 1.5 h, ground, and aluminum sol and 120 nm nano silica sol were added, mixed evenly to obtain component A;

[0079] S2. Preparation of component B: n-propyl triethoxysilane, phenyl triethoxysilane, propylene glycol methyl ether and BYK-381 were mixed and stirred at a controlled speed of 500 rpm for 1 hour to obtain component B;

[0080] S3, preparation of component C: mixing formic acid and acetic acid and stirring uniformly to obtain component C;

[0081] S4, preparation of component D: polyacrylate modified silicone resin, propylene glycol methyl ether and isopropanol were mixed uniformly and stirred at a controlled speed of 1200 rpm for 1 hour to obtain component D;

[0082] S5. Preparation of finished product: Mix component B and component C evenly to obtain mixture A, pre-stir component A at a controlled speed of 600 rpm and add mixture A while stirring at this speed, control the temperature to 48°C and stir for 4 hours to obtain mixture B, add component D to mixture B and stir and mix evenly at a controlled speed of 400 rpm to obtain a finished water-based composite ceramic coating.

[0083] Example 3

[0084] A water-based composite ceramic coating and a preparation method thereof, wherein the ceramic coating comprises component A, component B, component C and component D in a mass ratio of 50:30:0.6:15;

[0085] The A component includes the following raw materials by weight:

[0086]

[0087] The silica sol comprises a nano silica sol with a particle size of 10 nm and a nano silica sol with a particle size of 100 nm in a mass ratio of 1:1;

[0088] The B component includes the following raw materials by weight:

[0089]

[0090] The C component includes the following raw materials by weight:

[0091] 50 parts of formic acid;

[0092] 50 parts of acetic acid;

[0093] The D component includes the following raw materials by weight:

[0094] 80 parts of polyurethane modified silicone resin;

[0095] Propylene glycol methyl ether 9 parts;

[0096] 11.5 parts of isopropyl alcohol;

[0097] The molecular weight of the polyurethane modified silicone resin is 80000;

[0098] A method for preparing a water-based composite ceramic coating, the preparation method specifically comprising the following steps:

[0099] S1. Preparation of component A: 10 nm nano silica sol, fumed silica powder, lithium magnesium silicate, rutile titanium dioxide, 4000 mesh soft kaolin, copper chrome black, 150 nm β-silicon nitride whisker, sericite, isopropanol and deionized water were stirred at 1250 rpm for 2 h, mixed evenly, ground, added aluminum sol and 100 nm nano silica sol, mixed evenly, and obtained component A;

[0100] S2. Preparation of component B: n-propyl triethoxysilane, phenyl triethoxysilane, propylene glycol methyl ether and BYK-310 were mixed and stirred at a controlled speed of 600 rpm for 1 hour to obtain component B;

[0101] S3, preparation of component C: mixing formic acid and acetic acid and stirring uniformly to obtain component C;

[0102] S4, preparation of component D: polyurethane modified silicone resin, propylene glycol methyl ether and isopropanol were uniformly mixed and stirred at a controlled speed of 1250 rpm for 0.5 h to obtain component D;

[0103] S5. Preparation of finished product: Mix component B and component C evenly to obtain mixture A, pre-stir component A at a controlled speed of 500 rpm and add mixture A while stirring at this speed, control the temperature to 50°C and stir for 4 hours to obtain mixture B, add component D to mixture B and stir and mix evenly at a controlled speed of 500 rpm to obtain a finished water-based composite ceramic coating.

[0104] Comparative Example 1

[0105] Compared with Example 1, the difference is that no 4000 mesh soft kaolin is added to component A of Comparative Example 1, and the silica sol is 38 parts by weight, the aluminum sol is 28 parts by weight, and the other parameters and operating steps remain unchanged.

[0106] Comparative Example 2

[0107] Compared with Example 1, the difference is that no silica sol is added to component A of Comparative Example 2, and the 4000 mesh soft kaolin is 23.5 parts by weight, the aluminum sol is 42.5 parts by weight, and the other parameters and operating steps remain unchanged.

[0108] Comparative Example 3

[0109] Compared with Example 1, the difference is that no aluminum sol is added to component A of Comparative Example 3, and the 4000 mesh soft kaolin is 18.5 parts by weight, the silica sol is 47.5 parts by weight, and the other parameters and operating steps remain unchanged.

[0110] Comparative Example 4

[0111] Compared with Example 1, the difference is that no 50 nm β-silicon nitride whisker is added to component A of Comparative Example 4, and the amount of fumed silica powder is 6 parts by weight, and the amount of sericite is 4.5 parts by weight, and the other parameters and operating steps remain unchanged.

[0112] Comparative Example 5

[0113] Compared with Example 1, the difference is that no fumed silica powder is added to component A of Comparative Example 5, and the 50 nm β-silicon nitride whisker is 5 parts by weight, and the sericite is 5.5 parts by weight, and the other parameters and operating steps remain unchanged.

[0114] Comparative Example 6

[0115] Compared with Example 1, the difference is that no sericite is added to component A of Comparative Example 6, and the 50 nm β-type silicon nitride whisker is 4.5 parts by weight, the fumed silica powder is 6 parts by weight, and the other parameters and operating steps remain unchanged.

[0116] Comparative Example 7

[0117] Compared with Example 1, the difference is that no polyacrylate-modified silicone resin is added to the D component of Comparative Example 7, and the other parameters and operation steps remain unchanged.

[0118] Test Case

[0119] The finished water-based composite ceramic coatings prepared in Examples 1-3 and Comparative Examples 1-7 were sprayed on iron cookware using the same compressed air spraying process, and the following performance tests were performed after leveling, drying, sintering and cooling, wherein the spraying thickness was 40 μm. The results are shown in Table 1.

[0120] Table 1

[0121]

[0122] Note: The performance test methods in Table 1 are as follows:

[0123] Salt spray corrosion test: 5wt% NaCl solution;

[0124] Acid resistance test: 5% sulfuric acid solution, soak for 7 days;

[0125] Alkali resistance test: 5% sodium hydroxide solution, soak for 7 days;

[0126] Flexibility (impact test) test: DuPont impact tester, 500g hammer cone, 50cm stroke;

[0127] Adhesion test: refer to standard ISO 12944.

[0128] It can be seen from the test data of salt spray corrosion resistance, acid resistance and alkali resistance in Table 1 above that the coating film of the finished water-based composite ceramic coating prepared by the present invention has better salt spray corrosion resistance and acid and alkali resistance, and can effectively enhance the permeability of the coating to the gaps of the cookware substrate, thereby improving the anti-corrosion effect of the coating on the cookware substrate.

[0129] It can be seen from the test data of flexibility in Table 1 that the coating film of the finished water-based composite ceramic coating prepared by the present invention has better toughness and can effectively reduce the cracking of the coating due to the deformation of the metal substrate in a hot state.

[0130] It can be seen from the test data of adhesion in Table 1 above that the finished water-based composite ceramic coating prepared by the present invention can effectively improve its bonding strength with the cookware substrate.

[0131] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0132] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. A water-based composite ceramic coating, characterized in that: The ceramic coating comprises component A, component B, component C and component D; The component A comprises the following raw materials: silica sol, aluminum sol, fumed silica, titanium dioxide, kaolin, pigment, silicon nitride whisker, sericite, isopropyl alcohol, lithium magnesium silicate and deionized water; The B component includes the following raw materials: alkyl silane, propylene glycol methyl ether and silicone leveling agent; The C component includes the following raw materials: formic acid and acetic acid; The D component includes the following raw materials: silicone polymer resin, propylene glycol methyl ether and isopropyl alcohol.

2. The water-based composite ceramic coating according to claim 1, characterized in that: The mass ratio of the component A, the component B, the component C and the component D is 50-55:25-30:0.4-0.6:15-20.

3. The water-based composite ceramic coating according to claim 1, characterized in that: The silica sol in component A is 30-40 parts by weight, the aluminum sol is 20-30 parts by weight, the fumed silica is 3-6 parts by weight, the titanium dioxide is 10-15 parts by weight, the kaolin is 4-8 parts by weight, the pigment is 5-10 parts by weight, the silicon nitride whisker is 2-4 parts by weight, the sericite is 2-4 parts by weight, the isopropyl alcohol is 5-10 parts by weight, the lithium magnesium silicate is 0.2-0.5 parts by weight and the deionized water is 6-10 parts by weight.

4. The water-based composite ceramic coating according to claim 1, characterized in that: The alkylsilane in the B component includes at least one of n-propyltriethoxysilane and phenyltriethoxysilane.

5. The water-based composite ceramic coating according to claim 4, characterized in that: The n-propyl triethoxysilane is 40-50 parts by weight, the phenyl triethoxysilane is 35-45 parts by weight, the propylene glycol methyl ether is 7-9 parts by weight, and the organosilicon leveling agent is 0.3 parts by weight.

6. The water-based composite ceramic coating according to claim 1, characterized in that: The mass ratio of formic acid to acetic acid in component C is 1:

1.

7. The water-based composite ceramic coating according to claim 1, characterized in that: In component D, the silicone polymer resin is 70-80 parts by weight, propylene glycol methyl ether is 7-9 parts by weight, and isopropyl alcohol is 10-13 parts by weight.

8. The water-based composite ceramic coating according to claim 7, characterized in that: The silicone polymer resin includes water-based polyester-modified silicone resin.

9. The water-based composite ceramic coating according to claim 8, characterized in that: The waterborne polyester-modified silicone resin includes any one of a polyacrylate-modified silicone resin and a polyurethane-modified silicone resin.

10. A method for preparing a water-based composite ceramic coating according to any one of claims 5 to 9, characterized in that: The preparation method specifically comprises the following steps: S1. Preparation of component A: 10-30 nm nano silica sol, fumed silica, lithium magnesium silicate, titanium dioxide, kaolin, pigment, silicon nitride whisker, sericite, isopropyl alcohol and deionized water are stirred and mixed at a controlled speed, ground, and aluminum sol and 80-120 nm nano silica sol are added and mixed to obtain component A; S2, preparation of component B: n-propyl triethoxysilane, phenyl triethoxysilane, propylene glycol methyl ether and an organosilicon leveling agent are mixed and stirred at a controlled speed to obtain component B; S3, preparation of component C: mixing formic acid and acetic acid and stirring uniformly to obtain component C; S4, preparation of component D: uniformly mixing silicone polymer resin, propylene glycol methyl ether and isopropyl alcohol and stirring at a controlled speed to obtain component D; S5. Preparation of finished product: Mix component B and component C evenly to obtain mixture A, pre-stir component A at a controlled speed and add mixture A while stirring at the same speed, control the temperature and stir to obtain mixture B, add component D to mixture B and stir and mix evenly at a controlled speed to obtain a finished water-based composite ceramic coating.

Citation Information

Patent Citations

  • Aqueous ceramic non-stick coating material for kitchenware surfaces and preparation method for aqueous ceramic non-stick coating material

    CN105778575A

  • Self-drying waterborne ceramic coating and preparation method thereof

    CN108329727A

  • Water-based ceramic coating and preparation method thereof

    CN111019517A

  • Water-based polysiloxane ceramic simulating coating

    CN111909616A