Coated steel wire, manufacturing method thereof and cord thread

By using CuXZn or CuZn/CuXZn coating on steel wire products and adding samarium, lanthanum, cerium or magnesium elements, the problem of corrosion of steel wire products in humid and hot environments in the existing technology is solved, and higher corrosion resistance and adhesion are achieved. Attached retention rate.

CN118814232APending Publication Date: 2024-10-22JIANGSU XINGDA STEEL TYPE CORD

Patent Information

Application Number
CN202411004080.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

Existing steel wire products are prone to corrosion in humid and hot environments, leading to coating peeling and bonding failure, and lack high corrosion resistance.

Method used

Using CuXZn coating or CuZn/CuXZn coating, by adding samarium, lanthanum, cerium or magnesium elements to the coating, a single or double layer coating is formed to improve the salt resistance, heat corrosion resistance and moisture corrosion resistance of the coating, and improve the aging Maintain stronger adhesion and adhesion retention during the process.

Benefits of technology

The corrosion resistance of steel wire products is significantly improved and the service life is extended. Especially under salt aging conditions, the corrosion resistance and adhesion retention rate of CuLaZn coating are superior to traditional CuZn coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118814232A_ABST
    Figure CN118814232A_ABST
Patent Text Reader

Abstract

The invention discloses a plated steel wire, a manufacturing method thereof and a cord in the technical field of steel wire product production and manufacturing, the plated layer of the plated steel wire is a single-layer plated layer or a double-layer plated layer, the single-layer plated layer is a CuXZn plated layer, the double-layer plated layer is a CuZn layer and a CuXZn layer in sequence from inside to outside and is represented as a CuZn / CuXZn plated layer, or the double-layer plated layer is a CuXZn layer and a CuZn layer in sequence from inside to outside and is represented as a CuXZn / CuZn plated layer, and the double-layer plated layer is represented as a CuXZn / CuZn plated layer. X is selected from one of samarium, lanthanum, cerium and magnesium. Compared with a traditional CuZn coating, the coated steel wire provided by the invention has more excellent salt resistance, thermal erosion resistance and wet erosion resistance, has equivalent positive vulcanization adhesive force, but has stronger adhesive force and higher adhesion retention rate in the subsequent aging process, especially salt aging.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of steel wire product production and manufacturing, and in particular to a coated steel wire and a production method thereof and a cord. Background Art

[0002] Steel wire products are used as skeleton materials through the vulcanization reaction between rubber and steel wire surface coating. In the prior art, the steel wire coating is mainly brass coating. In actual use, if the steel wire products are in a humid and hot air environment, the brass coating will react electrochemically with the steel wire under humid saline and alkali conditions, resulting in corrosion and shedding of the steel wire or coating. The periodic reciprocating force of the steel wire products or contact with other corrosive media will also accelerate the failure of the bonding between the steel wire products and rubber. Therefore, how to improve the corrosion resistance of steel wire products is the key to ensuring the service life and safety of the products. Summary of the invention

[0003] The object of the present invention is to overcome the deficiencies in the prior art and to provide a coated steel wire and a method for manufacturing the same, as well as a cord. The high corrosion-resistant coating has better salt resistance, heat erosion resistance and moisture erosion resistance than the traditional CuZn coating, and has comparable adhesion during positive vulcanization, but has stronger adhesion and higher adhesion retention during the subsequent aging process, especially salt aging.

[0004] To achieve the above object, the present invention is implemented by adopting the following technical solutions:

[0005] On the one hand, the present invention provides a coated steel wire, comprising a steel wire substrate and a coating, wherein the coating is a single-layer coating or a double-layer coating, wherein the single-layer coating is a CuXZn coating, the steel wire coated with the CuXZn coating is a CuXZn coated steel wire, the double-layer coating is a CuZn layer and a CuXZn layer from the inside to the outside, expressed as a CuZn / CuXZn coating, or is a CuXZn layer and a CuZn layer from the inside to the outside, expressed as a CuXZn / CuZn coating, the steel wire coated with the CuZn / CuXZn coating is a CuZn / CuXZn coated steel wire, the steel wire coated with the CuXZn / CuZn coating is a CuXZn / CuZn coated steel wire, and X is selected from one of samarium, lanthanum, cerium and magnesium;

[0006] Furthermore, the content of X in the CuXZn coating is 0.1-1%wt of the total coating; and the mass ratio of copper to zinc is 1.5-2.4.

[0007] Furthermore, the X content in the CuXZn coating is 0.2-0.6%wt of the total coating amount, and the mass ratio of copper to zinc is 1.75-2.0.

[0008] Furthermore, the mass ratio of copper to zinc in the CuZn / CuXZn coating and the CuXZn / CuZn coating is 1.56-2.03.

[0009] Furthermore, the mass ratio of copper to zinc in the CuZn / CuXZn coating and the CuXZn / CuZn coating is 1.63-1.94.

[0010] Furthermore, in the CuZn / CuXZn coating and the CuXZn / CuZn coating, the thickness of the CuXZn layer is greater than 1 / 3 of the thickness of the entire coating.

[0011] In a second aspect, the present invention provides a method for manufacturing the coated steel wire.

[0012] The manufacturing method of the CuXZn coated steel wire comprises the following steps:

[0013] Obtain the steel wire to be plated;

[0014] The steel wire is plated with a single metal layer, which is in the order of Cu layer, X layer and Zn layer from the inside to the outside;

[0015] The steel wire coated with a single metal layer is heated to fuse the three-phase interfaces to form a CuXZn coating to obtain a coated steel wire;

[0016] The manufacturing method of the CuZn / CuXZn coated steel wire comprises the following steps:

[0017] Obtain the steel wire to be plated;

[0018] The steel wire is plated with a single metal layer, which is a Cu layer and a Zn layer from the inside to the outside;

[0019] The steel wire coated with a single metal layer is heated to fuse the three-phase interfaces to form a CuZn coating, thereby obtaining a coated steel wire matrix;

[0020] The coated steel wire substrate is coated with a single metal layer, which is a Cu layer, an X layer and a Zn layer in order from the inside to the outside;

[0021] Heating the coated steel wire substrate coated with a single metal layer to fuse the three-phase interfaces to form a CuZn / CuXZn coating to obtain a coated steel wire;

[0022] The manufacturing method of the CuXZn / CuZn coated steel wire comprises the following steps:

[0023] Obtain the steel wire to be plated;

[0024] The steel wire is plated with a single metal layer, which is in the order of Cu layer, X layer and Zn layer from the inside to the outside;

[0025] The steel wire coated with a single metal layer is heated to fuse the three-phase interfaces to form a CuXZn coating, thereby obtaining a coated steel wire matrix;

[0026] The coated steel wire substrate is coated with a single metal layer, which is a Cu layer and a Zn layer in order from the inside to the outside;

[0027] The coated steel wire substrate coated with a single metal layer is heated to fuse the three-phase interfaces to form a CuXZn / CuZn coating to obtain the coated steel wire.

[0028] Furthermore, the heating is performed by an electric heating process;

[0029] Wherein, the electric heating power of the heating steel wire coated with a single metal layer is 3.5~4.2kw;

[0030] The electric heating power of the heated single metal layer coated steel wire substrate is 3.2-3.6 kw.

[0031] Furthermore, in the process of sequentially coating the steel wire with a single metal layer, the residence time between the coated X layer and the coated Zn layer is ≤12s; and the residence time of the X layer exposed to the air is ≤8s.

[0032] In a third aspect, the present invention provides a cord, the manufacturing material of which includes the above-mentioned coated steel wire.

[0033] Furthermore, the coated steel wires are compressed into filament units, and one or more filament units are twisted together in a certain direction to form a cord.

[0034] Compared with the prior art, the present invention has the following beneficial effects:

[0035] The present invention provides a coated steel wire, a manufacturing method thereof and a cord, wherein the coating of the coated steel wire is a single-layer coating or a double-layer coating, wherein the single-layer coating is a CuXZn coating, and the double-layer coating is a CuZn layer and a CuXZn layer from the inside to the outside, expressed as a CuZn / CuXZn coating, or a CuXZn layer and a CuZn layer from the inside to the outside, expressed as a CuXZn / CuZn coating, X is selected from one of samarium, lanthanum, cerium and magnesium, and by adding samarium, lanthanum, cerium or magnesium elements to the coating, the coating has better salt resistance, heat corrosion resistance and moisture corrosion resistance than the traditional CuZn coating, and the positive vulcanization adhesion is equivalent, but it has stronger adhesion and higher adhesion retention rate in the subsequent aging process, especially salt aging. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 is a schematic structural diagram of a coated steel wire coated with a CuXZn coating provided by an embodiment of the present invention;

[0037] Figure 2is a schematic structural diagram of a coated steel wire coated with a CuZn / CuXZn coating provided by an embodiment of the present invention;

[0038] Figure 3 is a schematic structural diagram of a coated steel wire coated with a CuXZn / CuZn coating provided by an embodiment of the present invention;

[0039] Figure 4 is a coating morphology diagram of a CuLaZn coated steel wire provided in an embodiment of the present invention;

[0040] Figure 5 is a coating morphology diagram of a CuZn coated steel wire provided in a comparative example of the present invention;

[0041] Figure 6 This is a corrosion morphology diagram of a CuLaZn coated steel wire in a 10% saline solution provided by an embodiment of the present invention;

[0042] Figure 7 This is a corrosion morphology diagram of a CuZn-coated steel wire in a 10% saline solution provided in a comparative example of the present invention;

[0043] Figure 8 This is a corrosion morphology diagram of a CuLaZn coated steel wire provided by an embodiment of the present invention eroded in hot air at 100°C;

[0044] Fig. 9 This is a corrosion morphology diagram of a CuZn-coated steel wire provided in a comparative example of the present invention when it is corroded in hot air at 100°C;

[0045] Fig.10 is a corrosion morphology diagram of a CuLaZn coated steel wire provided by an embodiment of the present invention corroded at 50°C / 80%RH;

[0046] Fig.11 This is a corrosion morphology diagram of the CuZn-coated steel wire provided in the comparative example of the present invention when corroded at 50°C / 80%RH.

[0047] In the figure: 1. Steel wire matrix; 2. CuZn layer; 3. CuXZn layer. DETAILED DESCRIPTION

[0048] The present invention will be further described below in conjunction with the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present invention, and cannot be used to limit the protection scope of the present invention.

[0049] Example 1

[0050] This embodiment provides a coated steel wire and a manufacturing method thereof. Taking the CuLaZn coated steel wire as an example, its structure is as follows: Figure 1 As shown, the method includes:

[0051] Obtain 2.05 mm heat-treated wire;

[0052] The heat-treated wire is coated with a Cu layer, a La layer and a Zn layer in sequence, wherein the La-containing plating solution raw materials include lanthanum chloride heptahydrate and boric acid, and the interfaces among the Cu layer, the La layer and the Zn layer are fused by electrothermal treatment at a power of 3.8 kW to obtain a CuLaZn coated steel wire.

[0053] The total residence time of the La layer from lanthanum plating to zinc plating is 8s, and the residence time exposed to air is 5s. The coating weight of the prepared CuLaZn coated steel wire is 3.78g / kg, the Cu content is 64.22%wt, the La content is 0.42%wt, the balance is zinc, and the mass ratio of Cu / Zn is 1.82.

[0054] Example 2

[0055] This embodiment provides a cord, specifically a CuLaZn coated steel cord, the manufacturing material includes the CuLaZn coated steel wire as described in Embodiment 1,

[0056] The 2.05 mm CuLaZn coated steel wire was drawn under liquid lubrication to obtain 0.35 mm filament units, and then two groups of filament units were twisted to obtain a 2+2 structured CuLaZn coated steel cord.

[0057] Comparative Example 1

[0058] This comparative example 1 provides a CuZn coated steel wire and a method for manufacturing the same, the method comprising:

[0059] Obtain 2.05 mm heat-treated wire;

[0060] The heat-treated wire was plated with a Cu layer and a Zn layer in sequence, and the interface between the Cu layer and the Zn layer was fused by 3.6 kW electric heating to obtain a CuZn-coated steel wire.

[0061] The coating weight of the prepared CuZn coated steel wire is 3.84 g / kg, the Cu content is 64.54%wt, and the balance is zinc.

[0062] Comparative Example 2

[0063] This comparative example provides a cord, specifically a CuZn-coated steel cord, the manufacturing material of which includes the CuZn-coated steel wire as described in comparative example 1,

[0064] The 2.05 mm CuZn-coated steel wire was drawn under liquid lubrication to obtain 0.35 mm filament units, and then two groups of filament units were twisted to obtain a 2+2 structured CuZn-coated steel cord.

[0065] The coating structure and microscopic morphology of the CuLaZn coated steel wire provided in Example 1 and the CuZn coated steel wire provided in Comparative Example 1 are shown in FIG. Figure 4 and Figure 5 ,like Figure 4 and Figure 5 As shown in the figure, after the rare earth lanthanum is introduced into the coating, the morphology of the coating is obviously different from that of CuZn, the grains of the coating are refined, and the whole morphology is branch-like.

[0066] The CuLaZn-coated steel wire and CuZn-coated steel wire of the same length were cut respectively, and placed in 10% salt water to test the difference in corrosion resistance between the two.

[0067] Figure 7 This is the corrosion morphology of CuZn coated steel wire immersed in 10% saline solution for 6 hours, as shown in Figure 7 As shown in Figure 2, multiple corrosion sites have appeared on the surface of the CuZn-coated steel wire. Figure 6 This is the corrosion morphology of CuLaZn coated steel wire immersed in 10% saline solution for 16 hours, as shown in Figure 8 As shown, at this time, the surface of the CuLaZn coated steel wire is only slightly dark, but no corrosion spots are observed on the entire CuLaZn coating surface.

[0068] The CuLaZn-coated steel wire and CuZn-coated steel wire of the same length were cut respectively, and the two were placed in 100°C hot air respectively to test the difference in corrosion resistance between the two.

[0069] Fig. 9 This is the corrosion morphology of CuZn coated steel wire corroded in 100℃ hot air for 7 days, such as Fig. 9 As shown, at this time, the surface of the CuZn-coated steel wire is obviously dark, and black rust spots are formed on the surface of the CuZn coating; Figure 8 This is the corrosion morphology of the CuLaZn coated steel wire corroded in 100℃ hot air for 7 days. As shown in the figure, at this time, the surface color of the CuLaZn coated steel wire is only slightly darker, and no obvious black rust spots are formed.

[0070] The CuLaZn-coated steel wire and CuZn-coated steel wire of the same length were cut respectively, and the two were placed in a box at 50℃ / 80% relative humidity to test the difference in corrosion resistance between the two.

[0071] Fig.11 This is the corrosion morphology of CuZn coated steel wire after corrosion for 3 days at 50℃ / 80%RH, as shown in Fig.11 As shown, the surface of the CuZn-coated steel wire is obviously darker, and red rust appears on the surface of the steel wire; Fig.10 This is the corrosion morphology of CuLaZn coated steel wire after 3 days of corrosion at 50℃ / 80%RH, as shown in Fig.10As shown, the surface of the CuLaZn coated steel wire is also dark, but no rust spots are observed on the surface of the steel wire.

[0072] From the above corrosion resistance test results, it can be seen that the salt resistance of the CuLaZn coated steel wire provided in Example 1 of the present invention is significantly better than that of the CuZn coated steel wire provided in Comparative Example 1. After rust spots appear on the CuZn coated steel wire, the etching time of the CuLaZn coated steel wire is extended by more than 3 times, but no surface rust is observed. The heat erosion resistance and moisture erosion resistance of the CuLaZn coated steel wire are also better than those of the CuZn coated steel wire.

[0073] The CuLaZn coated steel cord provided in Example 2 and the CuZn coated steel cord provided in Comparative Example 2 were vulcanized and cured with different semi-steel cord rubbers of W, Y, and Z, respectively. After curing, they were aged for 7 days under 10% salt water conditions, 14 days under 100°C hot air conditions, and 14 days under 93°C / 95%RH wet heat conditions, and the adhesion of the two coatings was tested respectively. The results are shown in Tables 1 to 3.

[0074] Table 1 Adhesion of CuLaZn coated cord and CuZn coated cord to W compound after curing

[0075]

[0076] Table 2 Adhesion of CuLaZn coated cord and CuZ coated cord to Y rubber after curing

[0077]

[0078] Table 3 Adhesion of CuLaZn coated cord and CuZn coated cord to Z rubber after curing

[0079]

[0080] It can be clearly understood from Tables 1 to 3 that, in the face of different rubber systems, the positive vulcanization adhesion of the CuLaZn coating and the CuZn coating is basically equivalent, but in the subsequent aging process, the adhesion and adhesion retention rate of the CuLaZn coating are better than those of the CuZn coating, especially in the experiment of aging for 7 days under 10% salt water conditions, the adhesion retention rate of the CuLaZn coating is generally better than that of the CuZn coating by about 8%, while in the experiments of aging for 14 days under 100°C hot air conditions and aging for 14 days under 93°C / 95%RH wet heat conditions, the adhesion retention rate of the CuLaZn coating is generally better than that of the CuZn coating by about 3%.

[0081] Example 3

[0082] This embodiment provides a CuZn / CuLaZn coated steel wire and a manufacturing method thereof, wherein the structure is as follows: Figure 2As shown, the method includes:

[0083] Obtain 2.05 mm heat-treated wire;

[0084] The heat-treated wire is plated with Cu and Zn in sequence, and the two are alloyed with an electrothermal power of 3.9kw. On the basis of the CuZn coating, a Cu layer, a La layer and a Zn layer are plated in sequence, wherein the La-containing plating solution raw materials include lanthanum chloride heptahydrate and boric acid. The interfaces among the Cu layer, the La layer and the Zn layer are fused by electrothermal power of 3.5kw to obtain CuZn / CuLaZn coated steel wire.

[0085] The total residence time of the La layer from lanthanum plating to zinc plating is 8s, and the residence time exposed to air is 5s. The coating weight of the prepared CuZn / CuLaZn coated steel wire is 3.69g / kg, the Cu content is 65.20%wt, the La content is 0.31%wt, the balance is zinc, and the mass ratio of Cu / Zn is 1.78.

[0086] Example 4

[0087] This embodiment provides a cord, specifically a layered coated steel cord, the manufacturing material includes the CuZn / CuLaZn coated steel wire as described in Embodiment 3,

[0088] The 2.05 mm CuZn / CuLaZn coated steel wire was drawn under liquid lubrication to obtain 0.35 mm filament units, and then two groups of filament units were twisted to obtain a 2+2 structured layered coated steel cord.

[0089] Example 5

[0090] This embodiment provides a CuLaZn / CuZn coated steel wire and a manufacturing method thereof, wherein the structure is as follows: Figure 3 As shown, the method includes:

[0091] Obtain 2.05 mm heat-treated wire;

[0092] The heat-treated wire is plated with Cu layer, La layer and Zn layer in sequence, and the three layers are alloyed with an electrothermal power of 4.1kw. The La-containing plating solution raw materials include lanthanum chloride heptahydrate and boric acid. On the basis of the CuLaZn coating, the Cu layer and the Zn layer are plated in sequence. The interface between the Cu layer and the Zn layer is fused by electrothermal power of 3.4kw to obtain CuLaZn / CuZn coated steel wire.

[0093] The total residence time of the La layer from lanthanum plating to zinc plating is 8s, and the residence time exposed to air is 5s. The coating weight of the prepared CuLaZn / CuZn coated steel wire is 3.71g / kg, the Cu content is 63.80%wt, the La content is 0.28%wt, the balance is zinc, and the mass ratio of Cu / Zn is 1.84.

[0094] Example 6

[0095] This embodiment provides a cord, specifically a layered coated steel cord, the manufacturing material of which includes the CuLaZn / CuZn coated steel wire as described in Embodiment 5,

[0096] The 2.05 mm CuLaZn / CuZn coated steel wire was drawn under liquid lubrication to obtain 0.35 mm filament units, and then two groups of filament units were twisted to obtain a 2+2 structured layered coated steel cord.

[0097] The cords of Examples 4 and 6 and the cords of Comparative Example 2 were corroded in 10% salt water, 100°C hot air, and 50°C / 80%RH environments, respectively. The corrosion resistance comparison results are shown in Table 4 below. The adhesion of the coating was cured by positive vulcanization in the W semi-steel cord rubber compound, and aged for 7 days under 10% salt water conditions, 14 days under 100°C hot air conditions, and 14 days under 93°C / 95%RH wet heat conditions. The results are shown in Table 5. The salt resistance, moisture resistance, and heat corrosion resistance of the layered coated cord in Table 4 are better than those of the CuZn cord, which also shows that the La-containing cord has a significantly better corrosion resistance than CuZn. The adhesion performance of the layered coated cord and the CuZn cord in the semi-steel W rubber compound in Table 5 is better than that of the CuZn cord, especially in salt aging resistance. After aging for 7 days in 10% salt water, the adhesion retention rate is still between 81 and 87%. The addition of La significantly slows down the attenuation of adhesion after salt water erosion.

[0098] Table 4 Comparison of corrosion resistance of layered coated cord and CuZn coated cord

[0099]

[0100] Table 5 Comparison of the bonding between layered coated cord and CuZn cord W

[0101]

[0102] The embodiments of the present invention are described above in conjunction with the accompanying drawings, but the present invention is not limited to the above-mentioned specific implementation methods. The above-mentioned specific implementation methods are merely illustrative and not restrictive. Under the enlightenment of the present invention, ordinary technicians in this field can also make many forms without departing from the scope of protection of the purpose of the present invention and the claims, which all fall within the protection of the present invention.

Claims

1. A coated steel wire, characterized in that: The invention comprises a steel wire substrate and a coating, wherein the coating is a single-layer coating or a double-layer coating, wherein the single-layer coating is a CuXZn coating, and the steel wire coated with the CuXZn coating is a CuXZn coated steel wire, the double-layer coating is a CuZn layer and a CuXZn layer from the inside to the outside, which is expressed as a CuZn / CuXZn coating, or is a CuXZn layer and a CuZn layer from the inside to the outside, which is expressed as a CuXZn / CuZn coating, the steel wire coated with the CuZn / CuXZn coating is a CuZn / CuXZn coated steel wire, and the steel wire coated with the CuXZn / CuZn coating is a CuXZn / CuZn coated steel wire, and X is selected from one of samarium, lanthanum, cerium and magnesium.

2. The coated steel wire according to claim 1, characterized in that: The content of X in the CuXZn coating is 0.1-1%wt of the total coating amount; the mass ratio of copper to zinc is 1.5-2.

4.

3. The coated steel wire according to claim 2, characterized in that: The X content in the CuXZn coating is 0.2-0.6%wt of the total coating amount, and the mass ratio of copper to zinc is 1.75-2.

0.

4. The coated steel wire according to claim 1, characterized in that: The mass ratio of copper to zinc in the CuZn / CuXZn coating and the CuXZn / CuZn coating is 1.56-2.

03.

5. The coated steel wire according to claim 4, characterized in that: The mass ratio of copper to zinc in the CuZn / CuXZn coating and the CuXZn / CuZn coating is 1.63-1.

94.

6. The coated steel wire according to claim 1, characterized in that: In the CuZn / CuXZn coating and the CuXZn / CuZn coating, the thickness of the CuXZn layer is greater than 1 / 3 of the thickness of the entire coating.

7. A method for manufacturing a coated steel wire according to any one of claims 1 to 6, characterized in that: The manufacturing method of the CuXZn coated steel wire comprises the following steps: Obtain the steel wire to be plated; The steel wire is plated with a single metal layer, which is in the order of Cu layer, X layer and Zn layer from the inside to the outside; The steel wire coated with a single metal layer is heated to fuse the three-phase interfaces to form a CuXZn coating to obtain a coated steel wire; The manufacturing method of the CuZn / CuXZn coated steel wire comprises the following steps: Obtain the steel wire to be plated; The steel wire is plated with a single metal layer, which is a Cu layer and a Zn layer from the inside to the outside; The steel wire coated with a single metal layer is heated to fuse the three-phase interfaces to form a CuZn coating, thereby obtaining a coated steel wire matrix; The coated steel wire substrate is coated with a single metal layer, which is a Cu layer, an X layer and a Zn layer in order from the inside to the outside; Heating the coated steel wire substrate coated with a single metal layer to fuse the three-phase interfaces to form a CuZn / CuXZn coating to obtain a coated steel wire; The manufacturing method of the CuXZn / CuZn coated steel wire comprises the following steps: Obtain the steel wire to be plated; The steel wire is plated with a single metal layer, which is in the order of Cu layer, X layer and Zn layer from the inside to the outside; The steel wire coated with a single metal layer is heated to fuse the three-phase interfaces to form a CuXZn coating, thereby obtaining a coated steel wire matrix; The coated steel wire substrate is coated with a single metal layer, which is a Cu layer and a Zn layer in order from the inside to the outside; The coated steel wire substrate coated with a single metal layer is heated to fuse the three-phase interfaces to form a CuXZn / CuZn coating to obtain the coated steel wire.

8. The method for manufacturing a coated steel wire according to claim 7, characterized in that: The heating is performed by an electric heating process; Wherein, the electric heating power of the heating steel wire coated with a single metal layer is 3.5~4.2kw; The electric heating power of the heated single metal layer coated steel wire substrate is 3.2-3.6 kw.

9. The method for manufacturing a coated steel wire according to claim 7, characterized in that: In the process of sequentially plating the single metal layers on the steel wire, the residence time between the plated X layer and the plated Zn layer is ≤12s; and the residence time of the X layer exposed to the air is ≤8s.

10. A cord, characterized in that: The manufacturing material thereof comprises the coated steel wire as claimed in any one of claims 1 to 6; the coated steel wire is compressed into filament units, and one or more filament units are twisted together in a certain direction to form a cord.

Citation Information

Patent Citations

  • Brass-based composite coating and preparing method

    CN110079699A

  • Tire rubber reinforcing steel cord and tire

    JP1997109609A

  • Coated wire material excellent in wire drawability and corrosion resistance, wire body for reinforcing rubber excellent in corrosion resistance obtained by drawing the same, and composite material comprising the wire body for reinforcing rubber and rubber

    JP2007100119A

  • Plated steel wire, steel cord and rubber-steel cord complex

    JP2018119190A

  • A steel cord for tire

    KR1020020078168A

Cited By

  • Coated steel wire and manufacturing method therefor, and cord thread

    WO2026020721A1