Solid rocket nozzle composite expansion section and forming method thereof

By using a multi-ring structure combination of polyacrylonitrile carbon fiber/boron phenolic resin ablation layer and high silicone cloth tape/boron phenolic resin insulation layer in the expansion section of the solid rocket nozzle, combined with molding and winding processes, the existing problem is solved The technology overcomes the problems of high ablation layer resistance, high cost, and poor interface consistency, and achieves efficient ablation resistance and heat insulation performance and low-cost solid rocket nozzle expansion section.

CN118815618AActive Publication Date: 2024-10-22SHAANXI PULIMEI MATERIAL TECH CO LTD

Patent Information

Application Number
CN202411300137.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-18
Publication Date
2024-10-22
Estimated Expiration
2044-09-18

AI Technical Summary

Technical Problem

The existing fiber-reinforced resin-based expansion section has insufficient performance and cost under high temperature, high pressure and ablation conditions. The ablation layer has general resistance and high cost. The winding process is complex and the interface consistency is poor.

Method used

Polyacrylonitrile carbon fiber/boron phenolic resin material is used as the ablation layer, and high silicone cloth tape/boron phenolic resin material is used as the heat insulation layer. A multi-ring structure is formed through molding and winding processes, combined with hot pressing and curing to improve the ablation layer. The strength and stability of the connection to the insulation layer.

Benefits of technology

It achieves the dual functions of anti-ablation and heat insulation, with low ablation rate, low cost, high interface bonding strength, stable product size, good consistency, ablation layer line ablation rate reduced by 20%, and composite interface bonding strength. Less than 10MPa, the cost is 50% lower than the traditional cloth tape composite winding structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118815618A_ABST
    Figure CN118815618A_ABST
Patent Text Reader

Abstract

The invention discloses a solid rocket nozzle composite expansion section and a forming method thereof, and belongs to the technical field of composite expansion section forming, the solid rocket nozzle composite expansion section comprises an ablative layer, the ablative layer comprises a polyacrylonitrile carbon fiber / boron phenolic resin material layer, and the ablative layer is formed through acrylonitrile carbon fiber and boron phenolic resin premix and compression molding; the heat insulation layer comprises a high silica cloth tape / boron phenolic resin material layer; the thermal insulation layer is wound on the outer side of the ablative layer, and a multi-ring structure is formed on a connecting interface of the ablative layer and the thermal insulation layer. The anti-ablation heat-insulation structure has dual effects of anti-ablation and heat insulation, and is low in ablation rate, safe and reliable in structural connection, stable in product interface size and good in consistency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to a composite expansion section of a solid rocket nozzle and a molding method thereof, belonging to the technical field of composite expansion section molding. Background Art

[0002] The expansion section is a key component in the nozzle of a solid rocket engine to improve the energy conversion efficiency. It has to withstand high temperature, high pressure and high gas flow erosion and ablation during the operation of the engine. The fiber-reinforced resin-based expansion section has the advantages of high reliability, short production cycle and low cost, and is widely used in high-performance solid rocket engines at home and abroad. At present, the preparation methods of fiber-reinforced resin-based expansion sections at home and abroad mainly include overlapping tape winding, oblique tape winding, petal laying and molding. Among them, the expansion section with short working time and not serious ablation generally adopts high-silica fiber reinforced resin or carbon fiber reinforced resin material through compression molding; for the expansion section with severe ablation conditions and harsh working conditions, a carbon fiber phenolic / high-silica fiber phenolic composite structure is generally used. Carbon fiber phenolic is used as the ablation layer material, and high-silica phenolic is used as the thermal insulation layer material. This structure has the dual functions of anti-ablation and thermal insulation. Its molding process includes short fiber composite molding (QJ2727A-2014 "Carbon Fiber / Phenolic-High Silica Fiber / Phenolic Composite Molded Products Specification") and cloth tape winding (GJB3402-98 Carbon Cloth / Phenolic-High Silica Cloth / Phenolic Composite Winding Products Specification).

[0003] For QJ2727A-2014, the cost is low, and the process is more complicated. It needs to go through at least two or three moldings to form. Although the viscose carbon fiber used has good processability, its ablation resistance is average. In practical use, the thickness needs to be increased to improve its reliability, which increases the negative mass of the engine; for GJB3402-98, the cost is high, and the product has good mechanical properties, but the winding process requires stricter program design for tape winding, and the control pressure of the curing process is smaller than that of molding. The density of the carbon layer is generally low, and the barium phenolic resin used for the tape has a low carbon residue rate. There are wrinkles on the interface of the two materials, and the consistency is poor. At the end of work, the tape layers fall off.

[0004] In response to this phenomenon, this case designed a carbon fiber / phenolic-high silica cloth tape / phenolic composite structure as a solid rocket engine nozzle expansion section to realize its application in the solid rocket engine nozzle. Summary of the invention

[0005] According to one aspect of the present application, a composite expansion section for a solid rocket nozzle is provided. The expansion section has the dual functions of anti-ablation and heat insulation, a low ablation rate, a safe and reliable structural connection, and a stable product interface size and good consistency.

[0006] A composite expansion section for a solid rocket nozzle, characterized by comprising: an ablation layer, the ablation layer comprising a polyacrylonitrile carbon fiber / boron phenolic resin material layer, and formed by premixing the acrylonitrile carbon fiber and the boron phenolic resin and molding; A heat-insulating layer, the heat-insulating layer comprising a high-silica cloth tape / boron phenolic resin material layer; The heat insulation layer is wound around the outside of the ablation layer, and a connection interface between the ablation layer and the heat insulation layer forms a multi-ring structure.

[0007] Furthermore, the multi-ring structure includes a plurality of grooves and bosses alternately and continuously arranged at the connection interface between the ablation layer and the heat insulation layer; The interval between adjacent multi-ring structures is 1 to 3 times the width of the heat insulation layer, the height of the multi-ring structure is 1.5 mm to 3 mm, and the width of the multi-ring structure is 1 / 8 to 1 / 10 of the height of the expansion section.

[0008] Furthermore, the thickness of the ablation layer and the thermal insulation layer is confirmed according to the actual working condition of the expansion section, and according to the heat transfer path, the thickness of the ablation layer at the outlet part of the solid rocket nozzle is set to be gradually larger than the thickness of the ablation layer at the inlet part of the solid rocket nozzle.

[0009] Furthermore, the thickness of the ablation layer at the outlet portion of the solid rocket nozzle is greater than the thickness of the ablation layer at the inlet portion of the solid rocket nozzle.

[0010] According to another aspect of the present application, the present application also provides a method for forming a composite expansion section of a solid rocket nozzle, characterized in that it includes: S1: Preparation of the ablation layer, weighing a certain amount of polyacrylonitrile carbon fiber and boron phenolic resin for pretreatment to obtain a polyacrylonitrile carbon fiber / boron phenolic resin premix, and then molding it using a compression molding mold and performing heat preservation treatment; S2: After the heat preservation is completed, the product is naturally cooled to room temperature and demolded to obtain a polyacrylonitrile carbon fiber / boron phenolic resin blank. The demolded polyacrylonitrile carbon fiber / boron phenolic resin blank is cleaned and excess flash is removed. After the appearance is checked to be intact, the blank is loaded into a winding core mold; S3: Preparation of thermal insulation layer, obtaining high silica tape / boron phenolic resin material layer; S4: According to the set procedure, a high silica tape / boron phenolic resin material layer is wound around the outside of the polyacrylonitrile carbon fiber / boron phenolic resin blank; S5: After the winding is completed, a polyacrylonitrile carbon fiber / boron phenolic resin blank coated with the high-silica cloth tape / boron phenolic resin material layer is obtained, and then cured and formed in an autoclave, wherein the autoclave molding pressure is greater than or equal to 3.0 MPa; S6: After curing is completed, perform demoulding inspection and keep records.

[0011] Furthermore, the preparation of the polyacrylonitrile carbon fiber / boron phenolic resin premix comprises the following steps: Step 1: drying the polyacrylonitrile carbon fiber in an oven at a drying temperature of 90° C. to 100° C. for a drying time greater than or equal to 2 hours; Step 2: dissolving the boron phenolic resin and standing it for more than 24 hours after dissolution; Step 3: Mix the polyacrylonitrile carbon fiber and the dissolved boron phenolic resin according to the proportion, seal and let stand for more than 24 hours; Step 4: Tear the premixed material loose, and then let it air-dry for more than 24 hours at a temperature of 15℃ to 25℃ and a humidity of less than or equal to 45%; Step 5: The dried premix is ​​dried in an oven at a temperature of 80°C to 85°C for 5 hours or more and is set aside for later use.

[0012] Furthermore, in terms of mass ratio, the ratio of the polyacrylonitrile carbon fiber to the boron phenolic resin is 57:43.

[0013] Furthermore, the ablation layer also includes filler; In terms of mass ratio, the ratio of the polyacrylonitrile carbon fiber, the boron phenolic resin and the filler is 55:42:3.

[0014] Furthermore, before the compression molding using the compression molding die, the method further comprises: preheating the compression molding die at a temperature of 100° C.±5° C. for a preheating time of 1 h to 3 h; Among them, the pressure during compression molding is greater than or equal to 500kg / cm 2 , the insulation temperature is 100℃±5℃, the insulation time is 1h~3h, and the pressurization time is 25min~30min after mold closing.

[0015] The beneficial effects of this application include: The present application provides a composite expansion section for a solid rocket nozzle and a molding method thereof, wherein the expansion section has the dual functions of anti-ablation and heat insulation, and the linear ablation rate of the ablation layer reaches 0.02 mm / s, which is at least 20% lower than the linear ablation rate of the composite molding or cloth tape composite winding structure; at the same time, the composite interface bonding strength is not less than 10 MPa, the cost is at least 50% lower than the cloth tape composite winding structure, and the product interface size is stable and the consistency is good. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 This is a schematic diagram of the structure of the nozzle expansion section of a solid rocket engine in one embodiment of the present application; Figure 2 This is a structural diagram of the ablative layer forming tooling for the nozzle expansion section of a solid rocket engine in one embodiment of the present application; Figure 3 This is a schematic diagram of the structure of the nozzle expansion section of the solid rocket engine in Example 1 of the present application; Figure 4 This is a schematic diagram of the structure of the nozzle expansion section of the solid rocket engine in Example 2 of the present application; List of parts and reference numerals: 1 - ablation layer; 2 - thermal insulation layer; 3 - groove; 4 - boss; 5 - male mold; 6 - female mold; 7 - top plate. DETAILED DESCRIPTION

[0017] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.

[0018] See also Figure 1 , a composite expansion section of a solid rocket nozzle, characterized in that it comprises: The ablation layer 1 comprises a polyacrylonitrile carbon fiber / boron phenolic resin material layer, and is formed by premixing the acrylonitrile carbon fiber and the boron phenolic resin and molding; A heat-insulating layer 2, wherein the heat-insulating layer 2 comprises a high-silica cloth tape / boron phenolic resin material layer; The heat insulation layer 2 is wound around the outside of the ablation layer 1 , and the connection interface between the ablation layer 1 and the heat insulation layer 2 forms a multi-ring structure.

[0019] Specifically, during the operation of the solid rocket engine, the ablative layer 1 plays a role in resisting ablation and resisting the scouring of high temperature and high-speed airflow, thereby ensuring the integrity and stability of the nozzle structure. The ablative layer 1 is made of a mixture of polyacrylonitrile carbon fiber and boron phenolic resin, and is prepared by compression molding. This material combination has good ablative and mechanical properties. The main function of the thermal insulation layer 2 is to reduce the transfer of heat to the inside of the nozzle and protect the internal structure and components from high temperatures. The thermal insulation layer 2 uses a combination of high-silica cloth tape and boron phenolic resin, and is wrapped around the outside of the ablative layer 1 to form a multi-ring structure connection interface, which helps to improve the thermal protection effect of the nozzle while ensuring the stability and reliability of the structure; Among them, polyacrylonitrile carbon fiber has extremely high tensile strength and modulus, can withstand large external forces, and at the same time, the thermal decomposition temperature of the fiber is high, and it has excellent high-temperature performance; boron phenolic resin has higher heat resistance, instantaneous high-temperature resistance, thermal oxidation resistance, and neutron radiation resistance than ordinary phenolic resin. Since the BO bond energy is higher than the CC bond energy, the heat resistance and ablation resistance of boron phenolic resin are much higher than ordinary phenolic resin, and the BO bond has good flexibility. Therefore, the brittleness of boron phenolic resin is reduced and the mechanical properties are improved. The ablation layer 1 is made of a mixture of polyacrylonitrile carbon fiber and boron phenolic resin, and is prepared by compression molding. This material combination has good ablation performance and mechanical properties.

[0020] The multi-ring structure includes a plurality of alternately and continuously arranged grooves 3 and bosses 4 at the connection interface between the ablation layer 1 and the thermal insulation layer 2, which helps to enhance the connection strength and stability between the ablation layer 1 and the thermal insulation layer 2. At the same time, the structure helps to optimize the heat transfer path and improve the overall thermal insulation performance; The interval between adjacent multi-ring structures is 1 to 3 times the width of the heat insulation layer 2 , the height of the multi-ring structure is 1.5 mm to 3 mm, and the width of the multi-ring structure is 1 / 8 to 1 / 10 of the height of the expansion section.

[0021] Wherein, the height of the expansion section refers to Figure 1 The length of the expansion section in the oblique direction shown is specifically the usable length of the expansion section when the expansion section is set on the solid rocket nozzle.

[0022] The thickness of the ablation layer 1 and the thermal insulation layer 2 is confirmed according to the actual working condition of the expansion section, and according to the heat transfer path, the thickness of the ablation layer at the outlet of the solid rocket nozzle is set to be gradually larger than the thickness of the ablation layer at the inlet of the solid rocket nozzle.

[0023] The thickness of the ablation layer at the outlet portion of the solid rocket nozzle is greater than the thickness of the ablation layer at the inlet portion of the solid rocket nozzle.

[0024] Specifically, the ablative layer 1 has a greater thickness at the outlet portion of the solid rocket nozzle. This is to cope with the more intense high-temperature, high-speed airflow scouring at the nozzle outlet. A thicker ablative layer 1 can provide better anti-ablation performance and a longer service life. In contrast, the ablative layer 1 has a smaller thickness at the inlet portion of the solid rocket nozzle. This is because the airflow velocity at the nozzle inlet is relatively low and the temperature is relatively low, so an overly thick ablative layer 1 is not required to provide protection.

[0025] The present application designs a high-performance solid rocket engine nozzle expansion section, which has the dual functions of anti-ablation and heat insulation. The linear ablation rate of the ablation layer 1 reaches 0.02mm / s, which is at least 20% lower than the linear ablation rate of the composite molding or cloth-tape composite winding structure. The composite interface bonding strength is not less than 10MPa, and the cost is at least 50% lower than the cloth-tape composite winding structure. The product interface size is stable and consistent, the peak height of the composite interface wrinkles does not exceed 2mm, and the structural connection is safe and reliable. It has been tested on the ground and the effect is intact.

[0026] The composite interface wrinkle peak height refers to the maximum deviation of the wave crest from the average plane in the interface wrinkle phenomenon caused by material heating, stress concentration or other factors in the expansion section of the solid rocket engine nozzle. This parameter can reflect the stability and performance of the nozzle expansion section interface.

[0027] The physical properties of the material, such as the elastic modulus and Poisson's ratio, will affect its response to stress and temperature changes. The structural design of the nozzle, the connection method, and the temperature and pressure control during the manufacturing process will all affect the peak height of the interface wrinkles.

[0028] A method for forming a composite expansion section of a solid rocket nozzle, characterized by comprising: S1: Preparation of the ablation layer, weighing a certain amount of polyacrylonitrile carbon fiber and boron phenolic resin for pretreatment to obtain a polyacrylonitrile carbon fiber / boron phenolic resin premix, and then molding it using a compression molding mold and performing heat preservation treatment; Wherein, the pressing mold structure is as follows Figure 2 As shown, the compression molding die includes a male die 5, a female die 6 and a top plate 7 which are assembled with each other. The female die 6 is a die having a cavity, and the shape of the cavity is the same as the shape of the final product, i.e., the expansion section. During the molding process, the material to be processed will be placed in the cavity of the female die 6. The male die 5 is a solid die, and its shape is opposite to the cavity of the female die 6, i.e., it corresponds to the shape of the final product. During the molding process, the male die 5 will press into the material in the female die 6, and deform the material by applying force, so as to obtain the desired product shape. The top plate 7 is an important component in the compression molding die, and is located at the top of the die. It is used to provide support and positioning during the pressing process, and to help push out the finished product during demolding.

[0029] S2: After the heat preservation is completed, the product is naturally cooled to room temperature and demolded to obtain a polyacrylonitrile carbon fiber / boron phenolic resin blank. The demolded polyacrylonitrile carbon fiber / boron phenolic resin blank is cleaned and excess flash is removed. After the appearance is checked to be intact, the blank is loaded into a winding core mold; S3: Preparation of thermal insulation layer, obtaining high silica tape / boron phenolic resin material layer; S4: According to the set procedure, a high silica tape / boron phenolic resin material layer is wound around the outside of the polyacrylonitrile carbon fiber / boron phenolic resin blank; S5: After the winding is completed, a polyacrylonitrile carbon fiber / boron phenolic resin blank coated with the high-silica cloth tape / boron phenolic resin material layer is obtained, and then cured and formed in an autoclave, wherein the autoclave molding pressure is greater than or equal to 3.0 MPa; S6: After curing is completed, perform demoulding inspection and keep records.

[0030] The preparation of the polyacrylonitrile carbon fiber / boron phenolic resin premix comprises the following steps: Step 1: drying the polyacrylonitrile carbon fiber in an oven at a drying temperature of 90° C. to 100° C. for a drying time greater than or equal to 2 hours; Step 2: dissolving the boron phenolic resin and standing it for more than 24 hours after dissolution; Step 3: Mix the polyacrylonitrile carbon fiber and the dissolved boron phenolic resin according to the proportion, seal and let stand for more than 24 hours; Step 4: Tear the premixed material loose, and then let it air-dry for more than 24 hours at a temperature of 15℃ to 25℃ and a humidity of less than or equal to 45%; Step 5: The dried premix is ​​dried in an oven at a temperature of 80°C to 85°C for a time greater than or equal to 5 hours and is set aside after drying.

[0031] In terms of mass ratio, the ratio of the polyacrylonitrile carbon fiber to the boron phenolic resin is 57:43.

[0032] The ablative layer 1 further comprises a filler; In terms of mass ratio, the ratio of the polyacrylonitrile carbon fiber, the boron phenolic resin and the filler is 55:42:3.

[0033] The filler may be an inorganic filler such as silicon micropowder or alumina, or a nanofiller such as nanosilicon dioxide or nanocarbon tubes, to further enhance or adjust the performance of the composite material.

[0034] Before the compression molding is performed using the compression molding die, the method further includes: preheating the compression molding die at a temperature of 100° C.±5° C. for a preheating time of 1 hour to 3 hours; Among them, the pressure during compression molding is greater than or equal to 500kg / cm 2 , the insulation temperature is 100℃±5℃, the insulation time is 1h~3h, and the pressurization time is 25min~30min after mold closing.

[0035] Example 1: It is required that the peak height of the interface wrinkles of the solid rocket engine nozzle expansion section does not exceed 2mm, the ablation rate of the ablation layer line does not exceed 0.05mm / s (oxyacetylene test), and the composite interface bonding strength is not less than 10MPa; the normal working time of the engine is 26s. The specific steps are: 1) Expansion section structure design: like Figure 3 As shown, this type of expansion section consists of an ablation layer 1 and a heat insulation layer 2, wherein the interface is connected by a multi-ring structure, the multi-ring structure interval is generally twice the width of the heat insulation layer 2, the ring height is 1.5 mm, the ring width is 1 / 10 of the expansion section height, and the number of rings is 3. The ablation layer 1 is made of polyacrylonitrile carbon fiber / boron phenolic resin premix material, and the heat insulation layer 2 is made of high silica cloth tape / boron phenolic resin material.

[0036] Specifically, the groove width of the multi-ring structure is 40 mm, and the boss width of the multi-ring structure is 20 mm. The groove and boss widths refer to the widths of the groove and boss. Figure 3 The projection distance in the horizontal direction.

[0037] 2) Preparation of polyacrylonitrile carbon fiber / boron phenolic resin premix: a) Prepare polyacrylonitrile carbon fiber with a length of 50 mm, and dry it in an oven at a temperature of 90°C to 100°C for 2 hours; b) dissolving the boron phenolic resin with a solvent and leaving it to stand for 24 hours; c) Mix the polyacrylonitrile carbon fiber: boron phenolic resin: filler in a ratio of 55:42:3, seal and let stand for 24 hours; d) Tear the premixed material loose manually or by equipment, and then leave it at room temperature for 24 hours, with the temperature not lower than 15°C and the humidity not exceeding 45%; e) The dried premix is ​​dried in an oven at a temperature of 80°C to 85°C for 5 hours; after drying, it is packed in clean premix bags or barrels.

[0038] 3) Forming of expansion section: a) Calculate the loading amount according to the product design density, weigh 450g of polyacrylonitrile carbon fiber / boron phenolic resin premix, and then pretreat it in an oven for 35min at a temperature of 90℃; b) Clean the pressing mold and preheat it at 100℃±5℃ for 2h; c) evenly loading the pretreated polyacrylonitrile carbon fiber / boron phenolic resin premix into the preheated mold in multiple times; d) Pressurize the mold on a four-column hydraulic press with a pressure of no less than 500kg / cm 2, insulation temperature 100℃±5℃, time 1h, pressurization time is 25min~30min after mold closing; e) After the insulation is completed, the product is cooled naturally to room temperature and demoulded; f) Clean the demoulded polyacrylonitrile carbon fiber / boron phenolic resin blank, remove excess flash, check the appearance and install it into the winding core mold; g) According to the set procedure, the high silica cloth / boron phenolic resin is wound on the polyacrylonitrile carbon fiber / boron phenolic resin blank; h) After winding, the blank is coated and then cured in an autoclave, and the autoclave molding pressure is 3.0MPa; i) After curing, the demoulding inspection was completed. The appearance was intact, without cracks or missing materials. After inspection, the internal structure of the product was intact, without cracks or bubbles, and the maximum peak wave height of the interface wrinkles was 0.7mm.

[0039] Example 2: It is required that the peak height of the interface wrinkles of the solid rocket engine nozzle expansion section does not exceed 2mm, the ablation rate of the ablation layer line does not exceed 0.05mm / s (oxyacetylene test), and the composite interface bonding strength is not less than 10MPa; the normal working time of the engine is 38s. The specific steps are: 1) Expansion section structure design: like Figure 4 As shown, this type of expansion section consists of an ablation layer 1 and a heat insulation layer 2, wherein the interface is connected by a multi-ring structure, the interval is generally twice the width of the cloth tape, the ring height is 2 mm, the ring width is 1 / 8 of the expansion section height, and the number of rings is 5. The ablation layer 1 is made of polyacrylonitrile carbon fiber / boron phenolic resin premix material, and the heat insulation layer 2 is made of high silica cloth tape / boron phenolic resin material.

[0040] Specifically, the groove width of the multi-ring structure is 40 mm, and the boss width of the multi-ring structure is 50 mm. The groove and boss widths refer to the widths of the groove and boss. Figure 4 The projection distance in the horizontal direction.

[0041] 2) Preparation of polyacrylonitrile carbon fiber / boron phenolic resin premix: a) Prepare polyacrylonitrile carbon fiber with a length of 55 mm, and dry it in an oven at a temperature of 90°C to 100°C for 3 hours; b) dissolving the boron phenolic resin with a solvent and leaving it to stand for 30 hours; c) Mix the polyacrylonitrile carbon fiber: boron phenolic resin: filler in a ratio of 55:42:3, seal and let stand for 32 hours; d) Tear the premixed material loose manually or by equipment, and then leave it to air at room temperature for 30 hours, with the temperature not lower than 15°C and the humidity not exceeding 45%; e) The dried premix is ​​dried in an oven at a temperature of 80°C to 85°C for 6 hours; after drying, it is packed in clean premix bags or barrels.

[0042] 3) Forming of the expansion section: a) Calculate the charge amount according to the product design density, weigh 1500g of polyacrylonitrile carbon fiber / boron phenolic resin premix, and then pretreat it in an oven for 40min at a temperature of 100°C; b) Clean the pressing mold and preheat it at 100℃±5℃ for 3h; c) evenly loading the pretreated polyacrylonitrile carbon fiber / boron phenolic resin premix into the preheated mold in multiple times; d) Pressurize the mold on a four-column hydraulic press with a pressure of no less than 500kg / cm 2 , insulation temperature 100℃±5℃, time 1h, pressurization time is 25min~30min after mold closing; e) After the insulation is completed, the product is cooled naturally to room temperature and demoulded; f) Clean the demoulded polyacrylonitrile carbon fiber / boron phenolic resin blank, remove excess flash, check the appearance and install it into the winding core mold; g) According to the set procedure, the high silica cloth / boron phenolic resin is wound on the polyacrylonitrile carbon fiber / boron phenolic resin blank; h) After winding, the blank is coated and then cured in an autoclave with a molding pressure of 3.5 MPa; i) After curing, the product was demoulded and inspected. The appearance was intact, without cracks or missing materials. After inspection, the internal structure of the product was intact, without cracks or bubbles, and the maximum peak height of the interface wrinkles was 1.2mm.

[0043] The above are only a few embodiments of the present application and do not constitute any form of limitation to the present application. Although the present application is disclosed as above with preferred embodiments, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical solution.

Claims

1. A composite expansion section for a solid rocket nozzle, characterized in that: include: an ablation layer, the ablation layer comprising a polyacrylonitrile carbon fiber / boron phenolic resin material layer, and formed by premixing the acrylonitrile carbon fiber and the boron phenolic resin and molding; A heat-insulating layer, the heat-insulating layer comprising a high-silica cloth tape / boron phenolic resin material layer; The heat insulation layer is wound around the outside of the ablation layer, and a connection interface between the ablation layer and the heat insulation layer forms a multi-ring structure.

2. A solid rocket nozzle composite expansion section according to claim 1, characterized in that: The multi-ring structure comprises a plurality of grooves and bosses alternately and continuously arranged at the connection interface between the ablation layer and the heat insulation layer; The interval between adjacent multi-ring structures is 1 to 3 times the width of the heat insulation layer, the height of the multi-ring structure is 1.5 mm to 3 mm, and the width of the multi-ring structure is 1 / 8 to 1 / 10 of the height of the expansion section.

3. The solid rocket nozzle composite expansion section according to claim 1, characterized in that: The thickness of the ablation layer and the thermal insulation layer are confirmed according to the actual working conditions of the expansion section, and according to the heat transfer path, the thickness of the ablation layer at the outlet of the solid rocket nozzle is set to be gradually larger than the thickness of the ablation layer at the inlet of the solid rocket nozzle.

4. A solid rocket nozzle composite expansion section according to claim 3, characterized in that: The thickness of the ablation layer at the outlet portion of the solid rocket nozzle is greater than the thickness of the ablation layer at the inlet portion of the solid rocket nozzle.

5. A method for forming a composite expansion section of a solid rocket nozzle, characterized in that: include: S1: Preparation of the ablation layer, weighing a certain amount of polyacrylonitrile carbon fiber and boron phenolic resin for pretreatment to obtain a polyacrylonitrile carbon fiber / boron phenolic resin premix, and then molding it using a compression molding mold and performing heat preservation treatment; S2: After the heat preservation is completed, the product is naturally cooled to room temperature and demolded to obtain a polyacrylonitrile carbon fiber / boron phenolic resin blank. The demolded polyacrylonitrile carbon fiber / boron phenolic resin blank is cleaned and excess flash is removed. After the appearance is checked to be intact, the blank is loaded into a winding core mold; S3: Preparation of thermal insulation layer, obtaining high silica tape / boron phenolic resin material layer; S4: According to the set procedure, a high silica tape / boron phenolic resin material layer is wound around the outside of the polyacrylonitrile carbon fiber / boron phenolic resin blank; S5: After the winding is completed, a polyacrylonitrile carbon fiber / boron phenolic resin blank coated with the high-silica cloth tape / boron phenolic resin material layer is obtained, and then cured and formed in an autoclave, wherein the autoclave molding pressure is greater than or equal to 3.0 MPa; S6: After curing is completed, perform demoulding inspection and keep records.

6. The method for forming a composite expansion section of a solid rocket nozzle according to claim 5, characterized in that: The preparation of the polyacrylonitrile carbon fiber / boron phenolic resin premix comprises the following steps: Step 1: drying the polyacrylonitrile carbon fiber in an oven at a drying temperature of 90° C. to 100° C. for a drying time greater than or equal to 2 hours, wherein the length of the polyacrylonitrile carbon fiber is 35 mm to 60 mm; Step 2: dissolving the boron phenolic resin and standing it for more than 24 hours after dissolution; Step 3: Mix the polyacrylonitrile carbon fiber and the dissolved boron phenolic resin according to the proportion, seal and let stand for more than 24 hours; Step 4: Tear the premixed material loose, and then let it air-dry for more than 24 hours at a temperature of 15℃ to 25℃ and a humidity of less than or equal to 45%; Step 5: The dried premix is ​​dried in an oven at a temperature of 80°C to 85°C for a time greater than or equal to 5 hours and is set aside after drying.

7. The method for forming a composite expansion section of a solid rocket nozzle according to claim 6, characterized in that: In terms of mass ratio, the ratio of the polyacrylonitrile carbon fiber to the boron phenolic resin is 57:

43.

8. The method for forming a composite expansion section of a solid rocket nozzle according to claim 6, characterized in that: The ablative layer further comprises a filler; In terms of mass ratio, the ratio of the polyacrylonitrile carbon fiber, the boron phenolic resin and the filler is 55:42:

3.

9. The method for forming a composite expansion section of a solid rocket nozzle according to claim 5, characterized in that: Before the compression molding is performed using the compression molding die, the method further includes: preheating the compression molding die at a temperature of 100° C.±5° C. for a preheating time of 1 hour to 3 hours; Among them, the pressure during compression molding is greater than or equal to 500kg / cm 2 , the insulation temperature is 100℃±5℃, the insulation time is 1h~3h, and the pressurization time is 25min~30min after mold closing.

Citation Information

Patent Citations

  • Semi-curing molding method for double-layer glass-fiber-reinforced thermosetting molded part

    CN108145996A

  • Thermal-insulating anti-scouring heat shielding layer and preparation method thereof

    CN109367151A

  • High-strength ceramizable resin composite material and preparation method thereof

    CN110216930A

  • Heat insulation layer structure of solid rocket engine long-tail nozzle, and preparation method thereof

    CN112223856A

  • Spaceflight ablation heat-proof chopped fiber / phenolic aldehyde high-density premix, manual premixing preparation method and composite material thereof

    CN113637287A

Cited By

  • Solid rocket engine expansion section and forming method thereof

    CN119844244A

  • Solid rocket engine divergent section and method of forming

    CN119844244B