Process method for improving surface contact of silicon carbide diode

By using a combination of polysilicon mask layer and silicon carbide epitaxial layer in silicon carbide diodes to control the ion implantation window and oxide layer thickness, the surface damage and leakage problems caused by high-temperature ion implantation are solved, the production yield and performance are improved, and the production rate is reduced. manufacturing costs.

CN118824847APending Publication Date: 2024-10-22TIANJIN HUANXIN TECH DEV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411095261.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

The existing silicon carbide diode surface contact process causes increased surface damage due to high-temperature ion implantation when forming the p-type region, which increases leakage and manufacturing costs. Moreover, the contact metals and doping methods in different areas are complex, which affects the production yield.

Method used

In the preparation process of silicon carbide diodes, a polysilicon mask layer is used with a silicon carbide epitaxial layer to form a trench structure through photolithography and oxidation, control the ion implantation window, perform two ion implantations and oxidation, optimize the doping effect, and reduce the The trench structure width avoids damaging the Schottky contact surface and improves ohmic contact performance without adding photolithography steps.

Benefits of technology

It effectively reduces surface damage of silicon carbide diodes, improves production yield and front surge current capability, reduces manufacturing costs, and improves the performance of silicon carbide diodes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118824847A_ABST
    Figure CN118824847A_ABST
Patent Text Reader

Abstract

The invention provides a process method for improving surface contact of a silicon carbide diode, which comprises the following steps of: preparing a mask layer on an epitaxial layer of a substrate; performing ion implantation for the first time to form a first ion implantation region; oxidizing the substrate after the first ion implantation to form an oxide layer; performing second ion implantation to form a second ion implantation region; and removing the mask layer and the oxide layer. The method has the beneficial effects that the mask layer and the epitaxial layer which is not covered by the mask layer are oxidized at the same time to form the oxide layer, and the width of the ion implantation window is reduced during the second ion implantation, so that the second doped region is located in the first doped region and does not appear in a boundary region, adjacent to the epitaxial layer, of the first doped region; and the surface state of the Schottky contact surface is not damaged while the ohmic contact surface is obtained, so that the production yield of the silicon carbide diode is ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of semiconductor chips, and in particular relates to a process method for improving the surface contact of a silicon carbide diode. Background Art

[0002] Silicon carbide material is a compound semiconductor material with unique physical and chemical properties. It has very high hardness, chemical stability and high thermal conductivity. Compared with silicon, it exhibits wide bandgap, high critical electric field strength and high saturation mobility. These characteristics make silicon carbide outstanding among semiconductor materials and can be used to manufacture high-power electronic components. At present, commercial production of silicon carbide diodes and MOSFETs has been achieved. The currently more mature silicon carbide diode structure adopts the JBS or MPS structure, that is, a structure in which the P region and the n region are alternately formed in the active area. By designing different size combinations, it is possible to achieve a compatible forward low voltage drop of the Schottky diode and a reverse low leakage current of the PN diode. Therefore, it is required that the front metal is a Schottky contact in the n-type region and an ohmic contact in the p-type region.

[0003] At present, silicon carbide power chips all use n-type epitaxial layers. Since the coefficient of ion diffusion in silicon carbide materials is very small, the p-type region is obtained by high-temperature ion implantation. In terms of the process of Schottky contact in the front n-type region and ohmic contact in the p-type region, there are two mainstream methods: using a single metal Ti to form a Schottky contact in the n-type region, and the ohmic contact in the p-type region is obtained by heavy doping to obtain a nearly ideal ohmic contact with the metal (heavily doped pn junctions can generate significant tunnel currents. When metals and semiconductors are in contact, if the semiconductor doping concentration is very high, the barrier region becomes very thin, and electrons also need to pass through the barrier through the tunnel effect to generate a considerable tunnel current, which may even exceed the thermal electron emission current and become the main component of the current. When the tunnel current dominates, its contact resistance can be very small and can be used as an ohmic contact. Therefore, when the semiconductor is heavily doped, its contact with the metal can form a nearly ideal ohmic contact.) The disadvantage of this method is that large doses of ion implantation will increase the damage to the silicon carbide surface, especially at the junction of the n-region and the p-region. Since the n-region requires Schottky contact, large surface damage will increase the Schottky contact defects of the silicon carbide, increase leakage in the junction area, and cause yield loss. Different metals are used for ohmic contact and Schottky contact to meet the different contact requirements of silicon carbide in n-type and p-type regions. The ohmic contact is not obtained by heavy doping. It is necessary to formulate a special contact metal in the p-type region and then make the metal for Schottky contact. The disadvantage of this method is that it adds one more photolithography and metal deposition, which increases the manufacturing cost. Summary of the invention

[0004] In view of the above problems, the present invention provides a process method for improving the surface contact of a silicon carbide diode to solve the above or other former problems existing in the prior art.

[0005] In order to solve the above technical problems, the technical solution adopted by the present invention is: a process method for improving the surface contact of a silicon carbide diode, comprising the following steps: preparing a mask layer on the epitaxial layer of the substrate; Performing a first ion implantation to form a first ion implantation region; Oxidizing the substrate after the first ion implantation to form an oxide layer; Performing a second ion implantation to form a second ion implantation region; The mask layer and the oxide layer are removed.

[0006] Furthermore, the mask layer is prepared by deposition, and the material of the mask layer is different from that of the epitaxial layer.

[0007] Furthermore, the material of the mask layer is silicon.

[0008] Furthermore, the thickness of the mask layer is 1-2 μm.

[0009] Furthermore, before the first ion implantation, the mask layer is subjected to photolithography, etching and de-resistance to form an ion implantation window.

[0010] Furthermore, the mask layer is oxidized to form a first oxide layer, and the epitaxial layer not covered by the mask layer is oxidized to form a second oxide layer, and the thickness of the first oxide layer is greater than the thickness of the second oxide layer.

[0011] Further, oxidation is performed by dry oxidation or wet oxidation, and the oxidation temperature is 1000-1200°C.

[0012] Furthermore, the width of the first ion implantation region is greater than the width of the second ion implantation region.

[0013] Furthermore, the ion implantation dose during the first ion implantation is smaller than the ion implantation dose during the second ion implantation, and the ion implantation energy during the first ion implantation is larger than the ion implantation energy during the second ion implantation.

[0014] Furthermore, the ion implantation dose during the first ion implantation is less than 1×10 14 atom / cm -2 The ion implantation dose during the second ion implantation is greater than 1x10 14 atom / cm -2 .

[0015] Due to the adoption of the above technical solution, during the preparation process of the silicon carbide diode, a mask layer is prepared on the epitaxial layer, the material of the mask layer is different from the material of the epitaxial layer, the material of the epitaxial layer is silicon carbide, and the material of the mask layer is polycrystalline silicon; a groove structure is prepared on the mask layer by photolithography and etching to form an ion implantation window, and after the first ion implantation, the substrate provided with the mask layer and the epitaxial layer is oxidized so that the mask layer and the epitaxial layer not covered by the mask layer are oxidized at the same time, the mask layer is oxidized to form a first oxide layer, and the silicon carbide is oxidized to form a second oxide layer, so that the width of the groove structure is reduced, and therefore, during the second ion implantation, the width of the ion implantation window is reduced, so that the second doping area is located at the first The first doping region will not appear in the boundary region adjacent to the first doping region and the epitaxial layer, and the surface state of the Schottky contact surface will not be damaged while obtaining the ohmic contact surface, thereby ensuring the production yield of the silicon carbide diode; since the mask layer and the epitaxial layer are made of different materials, the thickness of the oxide layer formed after oxidation is different, and the thickness of the first oxide layer formed after the mask layer is oxidized is greater than the thickness of the second oxide layer formed after the epitaxial layer is oxidized, during the second ion injection, a part of the energy is blocked, so that the injected peak concentration moves to the surface, thereby optimizing the doping effect; in the preparation process of the silicon carbide diode, the performance of the silicon carbide diode is improved without adding a photolithography step, and the cost is not increased. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 is a schematic structural diagram of a first ion implantation region formed by a first implantation according to an embodiment of the present invention; Figure 2 is a schematic diagram of a structure of an oxide layer formed after oxidation according to an embodiment of the present invention (the oxide layer includes a first oxide layer and a second oxide layer); Figure 3 is a schematic structural diagram of a second ion implantation region formed by a second implantation according to an embodiment of the present invention; Figure 4 Schematic diagram of the structure of a silicon carbide diode according to an embodiment of the present invention.

[0017] In the figure: 1. Substrate; 2. Epitaxial layer; 3. Mask layer; 4. First implanted ions; 5. First doped region; 6. Oxide layer; 60. First oxide layer; 61. Second oxide layer; 7. Second doped region; 8. Second implanted ions; 9. Front metal; 10. Back metal; 11. Schottky contact; 12. Ohmic contact. DETAILED DESCRIPTION

[0018] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments.

[0019] Figure 1A structural schematic diagram of an embodiment of the present invention is shown. This embodiment relates to a process method for improving the surface contact of a silicon carbide diode. The mask layer and the epitaxial layer not covered by the mask layer are oxidized during the two doping processes, thereby reducing the width of the ion implantation window during the second doping process, without affecting the Schottky surface contact state, without increasing the number of photolithography times, and reducing cost investment.

[0020] A process for improving the surface contact of a silicon carbide diode, such as Figure 1-Figure 4 As shown, the following steps are included: A substrate 1 is prepared, and an epitaxial layer 2 is formed on one side of the substrate 1. In this step, the substrate 1 is a silicon carbide substrate 1, and the epitaxial layer 2 is a silicon carbide epitaxial layer 2. The epitaxial layer 2 can be a silicon carbide n-type epitaxial layer 2 or a silicon carbide p-type epitaxial layer 2. The type of the epitaxial layer 2 is selected according to actual needs.

[0021] After the epitaxial layer 2 is prepared, a mask layer 3 is prepared on the epitaxial layer 2 of the substrate 1, and the mask layer 3 is patterned to form an ion implantation window for subsequent ion implantation steps. When preparing the mask layer 3, a deposition method is adopted to form a mask layer 3 with a thin film structure on the epitaxial layer 2. The deposition method is preferably an LPCVD method.

[0022] The mask layer 3 is a single-layer thin film structure, and the material forming the mask layer 3 is silicon, which can be polycrystalline silicon.

[0023] The thickness of the mask layer 3 is 1-2 μm. The thickness of the mask layer 3 is selected according to actual needs and no specific requirements are given here.

[0024] The above-mentioned patterning process of the mask layer 3 includes sequentially performing photolithography, etching and stripping on the mask layer 3, wherein in the photolithography process, a layer of photoresist is coated on the mask layer 3, and exposure and development are performed according to actual graphic design requirements to form an area to be etched, that is, to form an ion implantation window area; In the etching process, the mask layer 3 in the area to be etched is removed to expose the epitaxial layer 2. Here, the area on the surface of the epitaxial layer 2 not covered by the mask layer 3 forms an ion implantation window for ion implantation and doping. In some feasible embodiments, the etching method is preferably dry etching; In the stripping process, the photoresist on the mask layer 3 is removed, so that the mask layer 3 is exposed, so as to facilitate the subsequent oxidation process.

[0025] After removing the photoresist, the mask layer 3 is completely exposed. The pattern on the photoresist is transferred to the mask layer 3 through photolithography and etching to form a mask layer 3 with a groove structure. The groove structure is the ion implantation window. The bottom of the groove structure is the epitaxial layer 2, and the sidewall of the groove structure is the mask layer 3.

[0026] Then the first ion implantation is performed, such as Figure 1 As shown, a first ion implantation region is formed in the epitaxial layer 2 for first doping. During the first ion implantation, first implantation ions 4 are implanted. The first implantation ions 4 of the first ion implantation are ion implantations of a relatively low dose, forming a first doped region 5 .

[0027] The first implanted ions may be p-type ions, such as aluminum ions, or n-type ions, such as phosphorus ions or nitrogen ions. The type of the first implanted ions is selected according to the conductivity type of the epitaxial layer 2, and no specific requirements are made here.

[0028] After the first ion implantation, the substrate 1 after the first ion implantation is oxidized to form an oxide layer 6, such as Figure 2 As shown, in this step, the substrate 1 after the first ion implantation is placed in an oxidation furnace, and the substrate 1 is oxidized by dry oxidation or wet oxidation. During the oxidation process, the mask layer 3 and the epitaxial layer 2 not covered by the mask layer 3 are oxidized at the same time. After the mask layer 3 is oxidized, a first oxide layer 60 is formed, and after the epitaxial layer 2 not covered by the mask layer 3 is oxidized, a second oxide layer 61 is formed. That is, the mask layer 3 on the side wall of the trench structure, the epitaxial layer 2 at the bottom of the trench structure, and the mask layer 3 on the top of the trench structure are oxidized at the same time, so that the width of the trench structure is reduced, that is, the width of the ion implantation window is reduced, and the width of the first ion implantation area is greater than the width of the second ion implantation area. Since the epitaxial layer 2 is silicon carbide and the mask layer 3 is polycrystalline silicon, the material of the epitaxial layer 2 is different from the material of the mask layer 3. Therefore, under the same oxidation conditions, the thickness of the second oxide layer 61 formed after the oxidation of the epitaxial layer 2 is different from the thickness of the first oxide layer 60 formed after the oxidation of the mask layer 3. The thickness of the first oxide layer 60 formed after the oxidation of the mask layer 3 is greater than the thickness of the second oxide layer 61 formed after the oxidation of the epitaxial layer 2, that is, the thickness of the first oxide layer 60 on the two side walls of the trench structure is greater than the thickness of the second oxide layer 61 at the bottom of the trench structure.

[0029] In the above-mentioned oxidation process, the oxidation temperature is 1000-1200°C. In some feasible embodiments, the oxidation temperature can be 1000°C, 1100°C, 1200°C or any temperature value between 1000-1200°C. The oxidation temperature is selected according to actual needs and no specific requirements are made here.

[0030] In the above oxidation process, the oxidation time is 10-60 minutes, and can be 20 minutes, 30 minutes, 40 minutes or 50 minutes. The oxidation time is selected according to actual needs and no specific requirements are made here.

[0031] After the oxidation is completed, a second ion implantation is performed, such as Figure 3 As shown, a second ion implantation area is formed and a second doping is performed. During the second ion implantation, the second implantation ions 8 are implanted in the same ion implantation window. Since both side walls of the trench structure are oxidized to form a first oxide layer 60, the width of the trench structure is reduced, that is, the width of the ion implantation window is reduced, so that the area for doping by the second ion implantation is limited to the area for doping by the first ion implantation, that is, the second doping area 7 formed by the second ion implantation is located in the first doping area 5, and will not appear in the boundary area adjacent to the epitaxial layer and the first doping area 5. While obtaining the ohmic contact surface 12, the surface state of the Schottky contact surface 11 will not be destroyed, thereby ensuring the yield of the product; at the same time, the silicon carbide at the bottom of the trench structure is also oxidized to form a second oxide layer 61, which can block part of the energy during the second ion implantation, so that the peak concentration of the implantation moves to the surface, thereby optimizing the doping effect.

[0032] The second ion implantation is a higher dose ion implantation for heavy doping. The second implanted ions 8 can be p-type ions, such as aluminum ions. The second implanted ions 8 can also be n-type ions. The type of the second implanted ions 8 is selected according to the conductivity type of the epitaxial layer 2, and no specific requirements are made here.

[0033] The ion implantation dose during the first ion implantation is less than the ion implantation dose during the second ion implantation, so that a heavily doped region is formed during the second ion implantation. The ion implantation dose during the first ion implantation is less than 1x10 14 atom / cm 2 The ion implantation dose during the second ion implantation is greater than 1x10 14 atom / cm 2 The ion implantation dose during the first ion implantation and the ion implantation dose during the second ion implantation are selected according to actual needs, and no specific requirements are made here.

[0034] During the first ion injection and the second ion injection, the first ion injection temperature and the second ion injection temperature are both 400-600°C, which can be 400°C, 500°C, 600°C or any temperature value between 400-600°C. It is selected and set according to actual needs, and no specific requirements are made here.

[0035] During the first ion injection and the second ion injection, the ion injection energy of the first ion injection is greater than the ion injection energy of the second ion injection, the first ion injection energy is greater than 50Kev, and the second ion injection energy is less than 50Kev. The first ion injection energy and the second ion injection energy are selected according to actual needs, and no specific requirements are made here.

[0036] After the second ion implantation is completed, the mask layer 3 and the oxide layer 6 are removed. Figure 4 As shown, the mask layer 3 and the oxide layer 6 are removed by wet etching. For example, the mask layer 3 and the oxide layer 6 can be etched by chemicals containing hydrofluoric acid and nitric acid. The chemicals can be polysilicon etching solution or BOE, both of which are commercially available products and can be selected according to actual needs.

[0037] After the mask layer 3 and the oxide layer 6 are removed, the processes of photolithography, etching, annealing, and preparing the front metal 9 and the back metal 10 are sequentially performed to form a silicon carbide diode. Here, the processes of photolithography, etching, annealing, and preparing the front metal 9 and the back metal 10 are all conventional processes and will not be described in detail here.

[0038] The silicon carbide diode prepared by the above process method has improved performance, increased front surge current capability, and improved product yield.

[0039] Due to the adoption of the above technical solution, during the preparation process of the silicon carbide diode, a mask layer is prepared on the epitaxial layer, the material of the mask layer is different from the material of the epitaxial layer, the material of the epitaxial layer is silicon carbide, and the material of the mask layer is polycrystalline silicon; a groove structure is prepared on the mask layer by photolithography and etching to form an ion implantation window, and after the first ion implantation, the substrate provided with the mask layer and the epitaxial layer is oxidized so that the mask layer and the epitaxial layer not covered by the mask layer are oxidized at the same time, the mask layer is oxidized to form a first oxide layer, and the silicon carbide is oxidized to form a second oxide layer, so that the width of the groove structure is reduced, and therefore, during the second ion implantation, the width of the ion implantation window is reduced, so that the second doping area is located at the first The first doping region will not appear in the boundary region adjacent to the first doping region and the epitaxial layer, and the surface state of the Schottky contact surface will not be damaged while obtaining the ohmic contact surface, thereby ensuring the production yield of the silicon carbide diode; since the mask layer and the epitaxial layer are made of different materials, the thickness of the oxide layer formed after oxidation is different, and the thickness of the first oxide layer formed after the mask layer is oxidized is greater than the thickness of the second oxide layer formed after the epitaxial layer is oxidized, during the second ion injection, a part of the energy is blocked, so that the injected peak concentration moves to the surface, thereby optimizing the doping effect; in the preparation process of the silicon carbide diode, the performance of the silicon carbide diode is improved without adding a photolithography step, and the cost is not increased.

[0040] The embodiments of the present invention are described in detail above, but the contents described are only preferred embodiments of the present invention and cannot be considered to limit the scope of implementation of the present invention. All equivalent changes and improvements made within the scope of the present invention should still fall within the scope of the patent coverage of the present invention.

Claims

1. A process for improving the surface contact of silicon carbide diodes, Features: The following steps are included: preparing a mask layer on the epitaxial layer of the substrate; Performing a first ion implantation to form a first ion implantation region; Oxidizing the substrate after the first ion implantation to form an oxide layer; Performing a second ion implantation to form a second ion implantation region; The mask layer and the oxide layer are removed.

2. The process for improving the surface contact of a silicon carbide diode according to claim 1, Features: The mask layer is prepared by deposition, and the material of the mask layer is different from the material of the epitaxial layer.

3. The process for improving the surface contact of a silicon carbide diode according to claim 2, Features: The mask layer is made of silicon.

4. The process for improving the surface contact of a silicon carbide diode according to claim 3, Features: The thickness of the mask layer is 1-2 μm.

5. The process for improving the surface contact of a silicon carbide diode according to any one of claims 1 to 4, Features: Before the first ion implantation, the mask layer is subjected to photolithography, etching and de-bonding to form an ion implantation window.

6. The process for improving the surface contact of a silicon carbide diode according to claim 5, Features: The mask layer is oxidized to form a first oxide layer, and the epitaxial layer not covered by the mask layer is oxidized to form a second oxide layer. The thickness of the first oxide layer is greater than that of the second oxide layer.

7. The process for improving the surface contact of a silicon carbide diode according to claim 6, Features: The oxidation is carried out by dry oxidation or wet oxidation, and the oxidation temperature is 1000-1200°C.

8. The process for improving the surface contact of a silicon carbide diode according to any one of claims 1 to 4 and 6 to 7, Features: The width of the first ion implantation region is greater than the width of the second ion implantation region.

9. The process for improving the surface contact of a silicon carbide diode according to claim 8, Features: The ion implantation dose during the first ion implantation is smaller than the ion implantation dose during the second ion implantation, and the ion implantation energy during the first ion implantation is larger than the ion implantation energy during the second ion implantation.

10. The process for improving the surface contact of a silicon carbide diode according to claim 9, Features: The ion implantation dose during the first ion implantation is less than 1×10 14 atom / cm -2 The ion implantation dose during the second ion implantation is greater than 1x10 14 atom / cm -2 .