Semiconductor structure and forming method thereof

By using protective layers and deoxidation treatment technology in semiconductor structures, the problem of difficulty in improving the quality of source-drain interconnection layers in semiconductor devices is solved, and the performance and stability of the semiconductor structure are improved.

CN118824971APending Publication Date: 2024-10-22SEMICON MFG INT (SHANGHAI) CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310437822.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-21
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

As semiconductor device dimensions shrink, it becomes more difficult to form high-quality source-drain interconnect layers, affecting the performance of the semiconductor structure.

Method used

A semiconductor structure is adopted, which includes a substrate, a gate structure, a source-drain doped layer, a source-drain interconnection layer, a source-drain cap layer and a protective layer, by forming a protective layer on top of the source-drain interconnection layer and on its surface Perform deoxidation treatment to make the material of the source-drain interconnection layer the same as the internal material, improving its quality and preventing re-oxidation.

Benefits of technology

Through deoxidation treatment and the use of protective layers, the quality and performance of the source-drain interconnection layer are improved, thereby improving the overall performance of the semiconductor structure and reducing the resistance and contact resistance of the interconnection layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118824971A_ABST
    Figure CN118824971A_ABST
Patent Text Reader

Abstract

The invention discloses a semiconductor structure and a forming method thereof. A gate structure on the substrate; the source-drain doping layer is positioned in the substrate on two sides of the gate structure; the source-drain interconnection layer is located on the two sides of the gate structure and covers the source-drain doping layer, the source-drain interconnection layer is electrically connected with the source-drain doping layer, and the material of the top surface of the source-drain interconnection layer is the same as that of the interior of the source-drain interconnection layer; the source-drain cap layer is located at the top of the source-drain interconnection layer; and the protection layer is located between the source-drain interconnection layer and the source-drain cap layer, and the protection layer is in contact with the top surface of the source-drain interconnection layer. The material of the top surface of the source-drain interconnection layer is the same as the material inside the source-drain interconnection layer, the quality of the source-drain interconnection layer is improved, the top of the source-drain interconnection layer is covered with the protection layer in contact with the top surface of the source-drain interconnection layer, and the protection layer can protect the source-drain interconnection layer, so that the source-drain interconnection layer is not easy to oxidize again, and the reliability of the source-drain interconnection layer is improved. Therefore, the performance of the source-drain interconnection layer is improved, and the performance of the semiconductor structure is further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The embodiments of the present invention relate to the field of semiconductor manufacturing, and in particular to a semiconductor structure and a method for forming the same. Background Art

[0002] With the rapid development of the semiconductor integrated circuit (IC) industry, semiconductor technology continues to move towards smaller process nodes driven by Moore's Law, making integrated circuits develop in the direction of smaller size, higher circuit precision and higher circuit complexity.

[0003] In order to meet the interconnection requirements after the critical dimensions are reduced, the interconnection between devices or between metal lines of different layers is realized through the interconnection structure. Therefore, before the back-end interconnection process, the local interconnection structure of the device is usually formed first, for example, the source-drain interconnection layer electrically connected to the source-drain doping layer, that is, the zeroth metal layer (M0).

[0004] However, in the development of integrated circuits, the functional density (i.e., the number of internal connection structures of each chip) is gradually increasing, while the geometric size (i.e., the minimum component size that can be produced using process steps) is gradually decreasing, which correspondingly increases the difficulty of forming the source-drain interconnection layer. Summary of the invention

[0005] The problem solved by the embodiments of the present invention is to provide a semiconductor structure and a method for forming the same, so as to improve the performance of the semiconductor structure.

[0006] To solve the above problems, the present invention provides a semiconductor structure, comprising: a substrate; a gate structure located on the substrate; a source-drain doped layer located in the substrate on both sides of the gate structure; a source-drain interconnection layer located on both sides of the gate structure and covering the source-drain doped layer, the source-drain interconnection layer being electrically connected to the source-drain doped layer, the material on the top surface of the source-drain interconnection layer being the same as the material inside the layer; a source-drain capping layer located on top of the source-drain interconnection layer; and a protective layer located between the source-drain interconnection layer and the source-drain capping layer, the protective layer being in contact with the top surface of the source-drain interconnection layer.

[0007] Optionally, the protection layer further extends to cover the sidewalls of the source / drain capping layer, and the protection layer covering the sidewalls of the source / drain capping layer serves as a self-aligned spacer layer.

[0008] Optionally, the semiconductor structure also includes: one or both of a source-drain contact hole plug and a gate source-drain contact hole plug; wherein the source-drain contact hole plug is located on the top of the source-drain interconnection layer, and the source-drain contact hole plug passes through the source-drain cap layer between the self-aligned sidewalls, and is electrically connected to the source-drain interconnection layer; the gate source-drain contact hole plug is located on the top of the adjacent gate structure and source-drain interconnection layer, and the gate source-drain contact hole plug passes through the source-drain cap layer between the self-aligned sidewall layers, and is electrically connected to the gate structure and the source-drain interconnection layer.

[0009] Optionally, the material of the protective layer includes one or more of metal, non-oxide metal compound and metal oxide.

[0010] Optionally, the protective layer includes a first sub-protective layer located on the surface of the source-drain interconnection layer, and a second sub-protective layer covering the first sub-protective layer, the material of the first sub-protective layer includes metal oxide, and the material of the second sub-protective layer includes metal or non-oxide metal compound.

[0011] Optionally, the material of the first sub-protection layer includes titanium oxide, and the material of the second sub-protection layer includes titanium carbide.

[0012] Optionally, along the normal direction of the top surface of the substrate, the thickness of the protection layer located on the top of the source-drain interconnection layer ranges from 10 angstroms to 100 angstroms.

[0013] Correspondingly, an embodiment of the present invention also provides a method for forming a semiconductor structure, comprising: providing a substrate, a gate structure being formed on the substrate, source-drain doped layers being formed in the substrate on both sides of the gate structure, a source-drain interconnection layer covering the source-drain doped layers being formed on the substrate on the side of the gate structure, and the source-drain interconnection layer being electrically connected to the source-drain doped layers; removing a portion of the thickness of the source-drain interconnection layer along the normal direction of the top surface of the substrate to form a groove located between adjacent gate structures; forming a protective layer covering the source-drain interconnection layer at the bottom of the groove; after forming the protective layer, performing a reduction treatment on the surface of the source-drain interconnection layer to achieve deoxidation; after the reduction treatment, filling the groove with a source-drain capping layer.

[0014] Optionally, in the step of forming the protective layer, the material of the protective layer includes a metal or a non-oxide metal compound; in the process of reducing the surface of the source-drain interconnection layer, the protective layer with a partial thickness on the surface of the source-drain interconnection layer is also oxidized to convert the material of the partial thickness of the protective layer into a metal oxide.

[0015] Optionally, in the step of forming the protective layer, the material of the protective layer includes titanium carbide; and in the step of oxidizing a portion of the thickness of the protective layer, the material of the metal oxide includes titanium oxide.

[0016] Optionally, in the step of forming the protection layer, the protection layer also covers the sidewalls of the groove, and the protection layer located on the sidewalls of the groove is used as a self-aligned spacer layer.

[0017] Optionally, after the source-drain capping layer is filled in the groove, the formation method further includes: forming one or both of a source-drain contact hole plug and a gate source-drain contact hole plug; wherein, the step of forming the source-drain contact hole plug includes: forming a source-drain contact hole plug on the top of the source-drain interconnection layer, the source-drain contact hole plug passes through the source-drain capping layer between the self-aligned sidewall layers, and is electrically connected to the source-drain interconnection layer; the step of forming the gate source-drain contact hole plug includes: forming a gate source-drain contact hole plug on the top of the adjacent gate structure and source-drain interconnection layer, the gate source-drain contact hole plug passes through the source-drain capping layer between the self-aligned sidewall layers, and is electrically connected to the gate structure and the source-drain interconnection layer.

[0018] Optionally, in the step of forming the protective layer, the protective layer also covers the side walls of the groove and the top of the gate structure outside the groove; the step of filling the source and drain capping layer in the groove includes: filling the capping material layer in the groove; performing a planarization process to remove the protective layer and the capping material layer outside the groove, and the remaining capping material layer serves as the source and drain capping layer.

[0019] Optionally, after forming the groove and before forming the protective layer, the formation method further includes: oxidizing the source-drain interconnection layer at the bottom of the groove so that the top surface of the source-drain interconnection layer is oxidized into an oxide layer; in the step of forming the protective layer, the protective layer covers the oxide layer; in the process of reducing the surface of the source-drain interconnection layer, the oxide layer is also reduced so that the oxide layer is reduced to the source-drain interconnection layer.

[0020] Optionally, in the step of oxidizing the source-drain interconnection layer at the bottom of the groove, the thickness of the oxide layer is in a range of 10 angstroms to 50 angstroms along a normal direction of the top surface of the substrate.

[0021] Optionally, in the step of performing reduction treatment on the surface of the source-drain interconnection layer, the reaction gas includes hydrogen, and the gas flow rate of the hydrogen is 10 standard ml / min to 100 standard ml / min.

[0022] Optionally, in the step of forming the protection layer, along the normal direction of the top surface of the substrate, the thickness of the protection layer located on the top of the source-drain interconnection layer ranges from 10 angstroms to 100 angstroms.

[0023] Optionally, the process of removing a portion of the thickness of the source-drain interconnection layer includes an atomic layer etching process.

[0024] Optionally, the process parameters of the atomic layer etching process include: the etching gas includes chlorine gas and hexafluoroacetylacetone gas, or the etching gas includes oxygen and hexafluoroacetylacetone gas, the pressure of the etching chamber is 10 mTorr to 500 mTorr, the gas flow rate of hexafluoroacetylacetone gas is 10 standard ml / min to 500 standard ml / min, the gas flow rate of chlorine gas is 10 standard ml / min to 500 standard ml / min, the gas flow rate of oxygen is 10 standard ml / min to 500 standard ml / min, and the etching time is 5 seconds to 50 seconds.

[0025] Compared with the prior art, the technical solution of the embodiment of the present invention has the following advantages:

[0026] The semiconductor structure provided by the embodiment of the present invention includes a protective layer located between the source-drain interconnection layer and the source-drain cap layer and in contact with the top surface of the source-drain doping layer. The material of the top surface of the source-drain interconnection layer is the same as the material inside it, that is, the top surface of the source-drain interconnection layer has been deoxidized, thereby improving the quality of the source-drain interconnection layer. Moreover, since the top of the source-drain interconnection layer is covered with the protective layer in contact with the top surface, the protective layer can protect the source-drain interconnection layer, making the source-drain interconnection layer less likely to be oxidized, thereby improving the performance of the source-drain interconnection layer, and further improving the performance of the semiconductor structure.

[0027] In the method for forming a semiconductor structure provided by an embodiment of the present invention, a protective layer covering the source-drain interconnection layer is formed at the bottom of the groove, and after the protective layer is formed, the surface of the source-drain interconnection layer is subjected to a reduction treatment to achieve deoxidation; deoxidation is achieved by performing a reduction treatment, so that the material on the top surface of the source-drain interconnection layer is the same as the material inside the layer, so as to improve the quality of the source-drain interconnection layer, and because the top of the source-drain interconnection layer is covered with the protective layer, the protective layer can protect the source-drain interconnection layer, so that the source-drain interconnection layer after the surface of the source-drain interconnection layer is subjected to a reduction treatment is not easily oxidized again, thereby improving the performance of the source-drain interconnection layer, and further improving the performance of the semiconductor structure. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is a structural schematic diagram of a semiconductor structure of the present invention;

[0029] Figures 2 to 7It is a schematic structural diagram corresponding to each step in an embodiment of a method for forming a semiconductor structure of the present invention. DETAILED DESCRIPTION

[0030] As can be seen from the background technology, as the size of semiconductor devices is gradually reduced, the difficulty of forming source-drain interconnection layers increases accordingly. How to improve the formation quality of source-drain interconnection layers to improve the performance of semiconductor structures has become an urgent problem to be solved.

[0031] In order to solve the above technical problems, an embodiment of the present invention provides a semiconductor structure, including: a substrate; a gate structure located on the substrate; a source-drain doped layer located in the substrate on both sides of the gate structure; a source-drain interconnection layer located on both sides of the gate structure and covering the source-drain doped layer, the source-drain interconnection layer is electrically connected to the source-drain doped layer, and the material of the top surface of the source-drain interconnection layer is the same as the material inside the source-drain interconnection layer; a source-drain cap layer located on the top of the source-drain interconnection layer; and a protective layer located between the source-drain interconnection layer and the source-drain cap layer, and the protective layer is in contact with the top surface of the source-drain interconnection layer. The semiconductor structure provided by the embodiment of the present invention includes a protective layer located between the source-drain interconnection layer and the source-drain cap layer and in contact with the top surface of the source-drain doping layer. The material of the top surface of the source-drain interconnection layer is the same as the material inside it, that is, the top surface of the source-drain interconnection layer has been deoxidized, thereby improving the quality of the source-drain interconnection layer. Moreover, since the top of the source-drain interconnection layer is covered with the protective layer in contact with the top surface, the protective layer can protect the source-drain interconnection layer, making the source-drain interconnection layer less likely to be oxidized, thereby improving the performance of the source-drain interconnection layer, and further improving the performance of the semiconductor structure.

[0032] In order to make the above-mentioned purposes, features and advantages of the embodiments of the present invention more obvious and understandable, specific embodiments of the present invention are described in detail below with reference to the accompanying drawings.

[0033] Figure 1 It is a schematic structural diagram of an embodiment of a semiconductor structure of the present invention.

[0034] refer to Figure 1 In this embodiment, the semiconductor structure includes: a substrate 100; a gate structure 110, located on the substrate 100; a source-drain doped layer 120, located in the substrate 100 on both sides of the gate structure 110; a source-drain interconnection layer 130, located on both sides of the gate structure 110 and covering the source-drain doped layer 120, the source-drain interconnection layer 130 is electrically connected to the source-drain doped layer 120, and the material of the top surface of the source-drain interconnection layer 130 is the same as the material inside the source-drain interconnection layer 130; a source-drain capping layer 150, located on the top of the source-drain interconnection layer 130; a protective layer 140, located between the source-drain interconnection layer 130 and the source-drain capping layer 150, and the protective layer 140 is in contact with the top surface of the source-drain interconnection layer 130.

[0035] The substrate 100 is used to provide a process platform for the process of the semiconductor structure. In the present embodiment, the substrate 100 is used to form a field effect transistor. As an example, the substrate 100 is used to form a fin field effect transistor (FinFET). In the present embodiment, the substrate 100 includes a substrate (not shown), and the substrate is a silicon substrate. In other embodiments, the material of the substrate can also be other materials such as germanium, silicon germanium, silicon carbide, gallium arsenide or indium gallium, and the substrate can also be other types of substrates such as a silicon substrate on an insulator or a germanium substrate on an insulator. It should be noted that the substrate can be a planar substrate or a substrate with a channel protrusion structure.

[0036] The gate structure 110 is used to form a field effect transistor with the conductive channel and the source-drain doped layer 120 .

[0037] In this embodiment, the gate structure 110 is a device gate structure. When the device is working, the device gate structure is used to control the opening and closing of the conductive channel. Specifically, the gate structure 110 includes a gate dielectric layer (not shown) and a gate electrode layer (not shown) covering the gate dielectric layer.

[0038] The gate dielectric layer is used to isolate the gate electrode layer from the substrate 100 .

[0039] In this embodiment, the gate structure 110 is a metal gate structure, and therefore, the material of the gate electrode layer includes one or more of TiN, TaN, Ta, Ti, TiAl, W, Al, TiSiN and TiAlC. The gate electrode layer includes a work function layer and an electrode layer covering the work function layer, or may include only the work function layer.

[0040] Correspondingly, the gate dielectric layer includes a high-k gate dielectric layer. The material of the high-k gate dielectric layer is a high-k dielectric material, and the high-k dielectric material refers to a dielectric material having a relative dielectric constant greater than the relative dielectric constant of silicon oxide. Specifically, the material of the high-k gate dielectric layer can be selected from HfO2, ZrO2, HfSiO, HfSiON, HfTaO, HfTiO, HfZrO or Al2O3, etc.

[0041] In other embodiments, the gate structure may also be a polysilicon gate structure.

[0042] In this embodiment, the semiconductor structure further includes: a gate sidewall 111, which is located on the sidewall of the gate structure 110. The gate sidewall 111 is used to protect the sidewall of the device gate structure. The gate sidewall 111 can be a single-layer structure or a stacked structure, and the material of the gate sidewall 111 includes one or more of silicon oxide, silicon nitride, silicon carbide, silicon carbonitride, silicon carbonitride, silicon oxynitride, boron nitride and boron carbonitride.

[0043] In this embodiment, the semiconductor structure further includes: a gate cap layer 112, which is located on the top of the gate structure 110. The gate cap layer 112 can be used to protect the top of the gate structure 110 during the process of forming the source-drain contact hole plug, thereby reducing the probability of damage to the gate structure 110, and short circuit problems between the gate structure 110 and the source-drain interconnection layer 130, or between the gate structure 110 and the source-drain contact hole plug.

[0044] A source-drain cap layer 150 is also formed on the top of the source-drain interconnect layer 130 to protect the top of the source-drain interconnect layer 130. Therefore, the gate cap layer 112 is made of a material having etching selectivity with the source-drain cap layer 150, thereby ensuring that the gate cap layer 112 can protect the gate structure 110. Therefore, in this embodiment, the material of the gate cap layer 112 includes one or more of silicon nitride, silicon carbide, silicon carbonitride, silicon carbonitride oxide, silicon nitride oxide, boron nitride and boron carbonitride. As an example, the material of the gate cap layer 112 is silicon nitride.

[0045] The source-drain doped layer 120 is used as the source region and the drain region of the transistor. When the device is working, the source-drain doped layer 120 is used to provide a carrier source.

[0046] The source-drain interconnection layer 130 is electrically connected to the source-drain doped layer 120 , and is used to realize electrical connection between the source-drain doped layer 120 and an external circuit.

[0047] The material of the top surface of the source-drain interconnection layer 130 is the same as the material inside thereof, that is, the top surface of the source-drain interconnection layer 130 has been deoxidized, thereby improving the quality of the source-drain interconnection layer 130 .

[0048] In this embodiment, the material of the source-drain interconnection layer 130 is cobalt, which has a low resistance, thereby reducing the resistance and contact resistance of the source-drain interconnection layer 130 itself and improving electrical performance. In other embodiments, the material of the source-drain interconnection layer 130 can also be other metal materials with low resistance.

[0049] In this embodiment, the semiconductor structure further includes: an etch stop layer 121, which is located between the source-drain interconnection layer 130 and the gate sidewall 111. The etch stop layer 121 is used to isolate the adjacent source-drain interconnection layer 130 and the gate structure 110, which is beneficial to reduce the electrical coupling effect between the adjacent source-drain interconnection layer 130 and the gate structure 110, thereby reducing the parasitic capacitance and improving the performance of the semiconductor structure. In addition, before forming the source-drain interconnection layer 130, the etch stop layer 121 covers the top of the source-drain doped layer 120, and in the process of forming the source-drain interconnection layer 130, it is often necessary to etch the dielectric layer to form an opening. The etch stop layer 121 located on the top of the source-drain doped layer 120 is also used to define the position of the etching stop in the step of etching the dielectric layer, thereby ensuring that the opening can expose the source-drain doped layer 120 while reducing the probability of damage to the source-drain doped layer 120.

[0050] It should be noted that the material of the etch stop layer 121 is one or more of silicon oxide, silicon nitride, silicon oxynitride, silicon oxycarbide, silicon carbon nitride, silicon carbon oxynitride, low-k dielectric material and ultra-low-k dielectric material. Among them, the low-k dielectric material refers to a dielectric material with a relative dielectric constant greater than or equal to 2.6 and less than or equal to 3.9, and the ultra-low-k dielectric material refers to a dielectric material with a relative dielectric constant less than 2.6.

[0051] The source-drain capping layer 150 can be used to protect the top of the source-drain interconnection layer 130 during the formation of the gate contact hole plug, thereby reducing the probability of damage to the source-drain interconnection layer 130 and short circuit problems between the source-drain interconnection layer 130 and the gate structure 110.

[0052] In this embodiment, the material of the source-drain capping layer 150 includes one or more of silicon nitride, silicon carbide, silicon carbonitride, silicon carbonitride oxide, silicon nitride oxide, boron nitride and boron carbonitride. As an example, the material of the gate capping layer 112 is silicon nitride. Accordingly, the material of the source-drain capping layer 150 is silicon carbide.

[0053] The protective layer 140 is located between the source-drain interconnection layer 130 and the source-drain capping layer 150, and is in contact with the top surface of the source-drain doped layer 120. The material of the top surface of the source-drain interconnection layer 130 is the same as the material inside it, that is, the top surface of the source-drain interconnection layer 130 has been deoxidized, which improves the quality of the source-drain interconnection layer 130. Moreover, since the top of the source-drain interconnection layer 130 is covered with the protective layer 140 in contact with the top surface thereof, the protective layer 140 can protect the source-drain interconnection layer 130 during the deoxidation process, so that the source-drain interconnection layer 130 is not easily oxidized again, thereby improving the performance of the source-drain interconnection layer 130, and further improving the performance of the semiconductor structure.

[0054] In a specific embodiment, the source-drain interconnection layer 130 has been subjected to a reduction treatment, and the protection layer 140 is used to protect the top surface of the source-drain interconnection layer 130 during the reduction treatment, so that the source-drain interconnection layer 130 is not easily oxidized again.

[0055] In this embodiment, the protection layer 140 further extends to cover the sidewalls of the source / drain capping layer 150 , and the protection layer 140 covering the sidewalls of the source / drain capping layer 150 serves as a self-aligned spacer. The protective layer 140 covering the side wall of the source-drain capping layer 150 serves as a self-aligned gate contact (SAGC). The self-aligned gate contact can serve as an etching stop layer along the extension direction perpendicular to the gate structure 110 when forming a source-drain contact plug, a gate source-drain contact plug or a gate contact plug, thereby achieving self-alignment of the source-drain contact plug, the gate source-drain contact plug or the gate contact plug, reducing the process difficulty of forming the source-drain contact plug, the gate source-drain contact plug or the gate contact plug, and correspondingly improving the position accuracy, size accuracy and morphology accuracy of the source-drain contact plug, the gate source-drain contact plug or the gate contact plug, thereby improving the quality of the source-drain contact plug, the gate source-drain contact plug or the gate contact plug, and further improving the performance of the semiconductor structure.

[0056] It should be noted that since the protective layer 140 covering the side walls of the source and drain capping layer 150 serves as a self-aligned sidewall layer, the hardness of the self-aligned sidewall layer is generally higher; if the protective layer also serves as a source and drain capping layer, when forming a source and drain contact hole plug or a gate source and drain contact hole plug, it is necessary to remove part of the thickness of the protective layer, which easily increases the process difficulty of forming the source and drain contact hole plug or the gate source and drain contact hole plug. Therefore, the protective layer is not suitable as a source and drain capping layer.

[0057] It should also be noted that after the protective layer is formed, the surface of the source-drain interconnection layer needs to be reduced to achieve deoxidation; if the source-drain cap layer is used as a protective layer and directly covers the top of the source-drain interconnection layer, the thickness of the protective layer is likely to be large, thereby increasing the difficulty of reducing the surface of the source-drain interconnection layer. Moreover, if the source-drain cap layer is used as a protective layer, the source-drain cap layer also serves as a self-aligned sidewall layer, which tends to reduce the range of material selection for the source-drain cap layer, thereby increasing the difficulty of forming the source-drain cap layer.

[0058] It should be noted that the thickness of the protective layer 140 located at the top of the source-drain interconnection layer 130 along the normal direction of the top surface of the substrate 100 should not be too large or too small. If the thickness of the protective layer 140 located at the top of the source-drain interconnection layer 130 is too large, it is easy to cause the remaining space reserved for the source-drain cap layer 150 to be too small, which is easy to increase the process difficulty of forming the source-drain cap layer 150; if the thickness of the protective layer 140 located at the top of the source-drain interconnection layer 130 is too small, it is easy for the protective layer 140 covering the top of the source-drain interconnection layer 130 to have a poor protection effect on the top surface of the source-drain interconnection layer 130, thereby increasing the probability of the source-drain interconnection layer 130 being oxidized again. Therefore, in this embodiment, along the normal direction of the top surface of the substrate 100, the thickness of the protective layer 140 located at the top of the source-drain interconnection layer 130 ranges from 10 angstroms to 100 angstroms.

[0059] In this embodiment, the material of the protective layer 140 includes one or more of metal, non-oxide metal compound and metal oxide. Generally, metal, non-oxide metal compound and metal oxide have high hardness, which can reduce the probability of damage to the source-drain interconnection layer 130 during the process of forming the source-drain contact hole plug.

[0060] In this embodiment, the protective layer 140 includes a first sub-protective layer 141 located on the surface of the source-drain interconnection layer 130, and a second sub-protective layer 142 covering the first sub-protective layer. The material of the first sub-protective layer 141 includes metal oxide, and the material of the second sub-protective layer 142 includes metal or non-oxide metal compound.

[0061] It should be noted that, in the case of forming a material layer of a metal or non-oxide metal compound, the surface of the source-drain interconnection layer 130 is subjected to a reduction treatment. In the process of achieving deoxidation, a partial thickness of the material layer of the metal or non-oxide metal compound is subjected to an oxidation treatment to convert the metal or non-oxide metal compound into a metal oxide. This makes it easy for the surface of the source-drain interconnection layer 130 to be fully reduced, which is beneficial to improving the quality of the source-drain interconnection layer 130 and thus facilitating electron transmission.

[0062] As an example, the material of the first sub-protective layer 141 includes titanium oxide, and the material of the second sub-protective layer 142 includes titanium carbide. Titanium carbide is a conductive material with a high melting point and good wear resistance, and in the process of deoxidizing the top surface of the source-drain interconnection layer 130, a partial thickness of the titanium carbide layer can also be oxidized to convert a partial thickness of the titanium carbide layer into titanium oxide, which has good electron transmission properties, so that the heterostructure composed of the source-drain interconnection layer 130, the first sub-protective layer 141, and the second sub-protective layer 142 has good electron transmission properties.

[0063] In this embodiment, the semiconductor structure also includes: one or both of: a source-drain contact hole plug (V0 Gate, V0G) 161 and a gate source-drain contact hole plug (V0 Drain Rectangle, V0DR) 162; wherein, the source-drain contact hole plug 161 is located on the top of the source-drain interconnection layer 130, and the source-drain contact hole plug 161 penetrates the source-drain cap layer 150 between the self-aligned sidewalls, and is electrically connected to the source-drain interconnection layer 130; the gate source-drain contact hole plug 162 is located on the top of the adjacent gate structure 110 and the source-drain interconnection layer 130, and the gate source-drain contact hole plug 162 penetrates the source-drain cap layer 150 between the self-aligned sidewall layers, and is electrically connected to the gate structure 110 and the source-drain interconnection layer 130.

[0064] The source-drain contact plugs 161 are used to realize electrical connection between the source-drain doped layer 120 and an external circuit.

[0065] The gate source-drain contact plugs 162 are used to realize electrical connection between the adjacent source-drain doped layers 120 and the gate structure 110 , and electrical connection between the adjacent source-drain doped layers 120 and the gate structure 110 and an external circuit.

[0066] It should be noted that, in the present embodiment, a protective layer 140 is provided between the source-drain contact plug 161 and the source-drain interconnection layer 130, and between the gate source-drain contact plug 162 and the source-drain interconnection layer 130; the protective layer 140 is located between the source-drain contact plug 161 and the source-drain interconnection layer 130, and between the gate source-drain contact plug 162 and the source-drain interconnection layer 130, which is beneficial to reduce the probability of the source-drain interconnection layer 130 being damaged during the formation of the source-drain contact plug 161 and the gate source-drain contact plug 162. In other embodiments, the protective layer may also be penetrated as required, so that the drain contact plug and the gate source-drain contact plug may be in direct contact with the source-drain interconnection layer. Specifically, the materials of the source-drain contact plug 161 and the gate source-drain contact plug 162 are both conductive materials, for example, the conductive materials include metal materials such as tungsten, cobalt, and ruthenium.

[0067] In this embodiment, the semiconductor structure further includes: a gate contact hole plug (V0 Gate, V0G) 163, which is located on the top of the gate structure 110, and the gate contact hole plug 163 passes through the gate cap layer 112 between the self-aligned spacer layers and is electrically connected to the gate structure 110. The gate contact hole plug 163 is used to realize the electrical connection between the gate structure 110 and the external circuit.

[0068] In this embodiment, the gate contact hole plug 163 is an active gate contact hole plug (Contact Over ActiveGate, COAG). Compared with the solution in which the gate contact hole plug contacts the gate structure located in the isolation area, the use of COAG is beneficial to saving chip area and further reducing the chip size.

[0069] Specifically, the gate contact plug 163 is made of a conductive material, such as metal materials such as tungsten, cobalt, and ruthenium.

[0070] Correspondingly, the present invention also provides a method for forming a semiconductor structure. Figures 2 to 7 It is a schematic structural diagram corresponding to each step in an embodiment of a method for forming a semiconductor structure of the present invention.

[0071] refer to Figure 2 A substrate 500 is provided, a gate structure 510 is formed on the substrate 500, source-drain doped layers 520 are formed in the substrate 500 on both sides of the gate structure 510, a source-drain interconnection layer 530 covering the source-drain doped layer 520 is formed on the substrate 500 on the side of the gate structure 510, and the source-drain interconnection layer 530 is electrically connected to the source-drain doped layer 520.

[0072] The substrate 500 is used to provide a process platform for subsequent process steps. In the present embodiment, the substrate 500 is used to form a field effect transistor. As an example, the substrate 500 is used to form a fin field effect transistor (FinFET). In the present embodiment, the substrate 500 includes a substrate (not shown), which is a silicon substrate. In other embodiments, the material of the substrate may also be other materials such as germanium, silicon germanium, silicon carbide, gallium arsenide or indium gallium, and the substrate may also be other types of substrates such as a silicon substrate on an insulator or a germanium substrate on an insulator. It should be noted that the substrate may be a planar substrate or a substrate having a channel protrusion structure.

[0073] The gate structure 510 is used to form a field effect transistor with the conductive channel and the source-drain doped layer 520. In this embodiment, the gate structure 510 is a device gate structure. When the device is working, the device gate structure 510 is used to control the opening and closing of the conductive channel. Specifically, the gate structure 510 includes a gate dielectric layer (not shown) and a gate electrode layer (not shown) covering the gate dielectric layer.

[0074] The gate dielectric layer is used to isolate the gate electrode layer from the substrate 500 .

[0075] In this embodiment, the gate structure 510 is a metal gate structure, and therefore, the material of the gate electrode layer includes one or more of TiN, TaN, Ta, Ti, TiAl, W, Al, TiSiN and TiAlC. The gate electrode layer includes a work function layer and an electrode layer covering the work function layer, or may include only the work function layer.

[0076] Correspondingly, the gate dielectric layer includes a high-k gate dielectric layer. The material of the high-k gate dielectric layer is a high-k dielectric material, and the high-k dielectric material refers to a dielectric material having a relative dielectric constant greater than the relative dielectric constant of silicon oxide. Specifically, the material of the high-k gate dielectric layer can be selected from HfO2, ZrO2, HfSiO, HfSiON, HfTaO, HfTiO, HfZrO or Al2O3, etc.

[0077] In other embodiments, the gate structure may also be a polysilicon gate structure.

[0078] In this embodiment, in the step of providing the substrate 500, a gate sidewall 511 is formed on the sidewall of the gate structure 510. The gate sidewall 511 is used to protect the sidewall of the device gate structure. The gate sidewall 511 can be a single-layer structure or a stacked structure, and the material of the gate sidewall 511 includes one or more of silicon oxide, silicon nitride, silicon carbide, silicon carbonitride, silicon carbonitride, silicon oxynitride, boron nitride and boron carbonitride.

[0079] In this embodiment, in the step of providing the substrate 500 , a gate cap layer 512 is formed on the top of the gate structure 510 .

[0080] The gate cap layer 512 is used to protect the top of the gate structure 510 during the subsequent process of forming the source-drain contact hole plugs, thereby reducing the probability of damage to the gate structure 510 and short circuit problems between the gate structure 510 and the source-drain interconnection layer 530, or between the gate structure 510 and the source-drain contact hole plugs.

[0081] Subsequently, a source-drain cap layer is formed on the top of the source-drain interconnection layer 530 to protect the top of the source-drain interconnection layer 530. Therefore, the gate cap layer 512 is made of a material having etching selectivity with the source-drain cap layer, thereby ensuring that the gate cap layer 512 can protect the gate structure 510. Therefore, in this embodiment, the material of the gate cap layer 512 includes one or more of silicon nitride, silicon carbide, silicon carbonitride, silicon carbonitride oxide, silicon nitride oxide, boron nitride and boron carbonitride. As an example, the material of the gate cap layer 512 is silicon nitride.

[0082] As an example, the gate cap layer 512 is flush with the top of the source-drain interconnection layer 530 .

[0083] The source-drain doped layer 520 is used as the source region and the drain region of the transistor. When the device is working, the source-drain doped layer 520 is used to provide a carrier source.

[0084] The source-drain interconnection layer 530 is electrically connected to the source-drain doped layer 520 to achieve electrical connection between the source-drain doped layer 520 and an external circuit.

[0085] In this embodiment, the material of the source-drain interconnection layer 530 is cobalt, which has a low resistance, thereby reducing the resistance and contact resistance of the source-drain interconnection layer 530 itself and improving electrical performance. In other embodiments, the material of the source-drain interconnection layer 530 may also be other metal materials with low resistance.

[0086] In this embodiment, in the step of providing the substrate 500 , an etching stop layer 521 is formed between the source-drain interconnection layer 530 and the gate spacer 511 .

[0087] The etch stop layer 521 is used to isolate adjacent source-drain interconnection layers 530 and gate structures 510 , which is beneficial to reduce the electrical coupling effect between adjacent source-drain interconnection layers 530 and gate structures 510 , thereby reducing parasitic capacitance and improving the performance of the semiconductor structure.

[0088] In addition, before forming the source-drain interconnection layer 530, the etch stop layer 521 covers the top of the source-drain doped layer 520, and in the process of forming the source-drain interconnection layer 530, it is often necessary to etch the dielectric layer to form an opening. The etch stop layer 521 located on the top of the source-drain doped layer 520 is also used to define the etching stop position in the step of etching the dielectric layer, thereby ensuring that the opening can expose the source-drain doped layer 520 while reducing the probability of damage to the source-drain doped layer 520.

[0089] It should be noted that the material of the etch stop layer 521 is one or more of silicon oxide, silicon nitride, silicon oxynitride, silicon oxycarbide, silicon carbon nitride, silicon carbon oxynitride, low-k dielectric material and ultra-low-k dielectric material. Among them, the low-k dielectric material refers to a dielectric material with a relative dielectric constant greater than or equal to 2.6 and less than or equal to 3.9, and the ultra-low-k dielectric material refers to a dielectric material with a relative dielectric constant less than 2.6.

[0090] refer to Figure 3 , along the normal direction of the top surface of the substrate 500 , a portion of the source-drain interconnection layer 530 is removed to form a groove 531 located between adjacent gate structures 510 .

[0091] The groove 531 provides a space for the subsequent formation of a source / drain capping layer.

[0092] In this embodiment, the process of removing a portion of the thickness of the source-drain interconnection layer 530 includes an atomic layer etching process.

[0093] When the atomic layer etching process etches the source-drain interconnection layer 530, the material is removed layer by layer at the atomic scale in an orderly manner, that is, equal etching can be achieved, which is beneficial to reduce the influence of the load effect of the pattern on the uniformity of the etching rate, thereby achieving precise control; and when the atomic layer etching process etches the source-drain interconnection layer 530, it has a higher etching selectivity ratio, thereby ensuring that while removing a portion of the thickness of the source-drain interconnection layer 530, the etching damage to other film layers (for example, the gate cap layer 512, the gate side wall 511, etc.) is small, which is beneficial to the stability of the pattern transfer.

[0094] It should be noted that the atomic layer etching process includes multiple atomic layer etching cycles. Only one atomic layer etching cycle is described below.

[0095] When etching the source-drain interconnection layer 530, the atomic layer etching cycle includes: oxidizing or chlorinating the material of the source-drain interconnection layer 530 to form an oxide layer or a chloride layer; reacting the oxide layer or the chloride layer with hexafluoroacetylacetone gas to generate volatile hexafluoroacetylacetonate or acetylacetone compound.

[0096] As an example, the material of the source-drain interconnection layer 530 is cobalt. Therefore, the reaction equation is as follows:

[0097] 2Co+xO2—>2CoOx

[0098] CoO x +2xhfacH—>Co(hfac) 2x ↑+xH2O↑

[0099] or,

[0100] Co+Cl2—>CoCl2

[0101] CoCl2+hfacH—>Co(hfac)Cl↑+HCl↑

[0102] CoCl2+(2-x)hfacH—>Co(hfac) (2-x) Cl x +(2-x)HCl↑

[0103] Specifically, the process parameters of the atomic layer etching process include: the etching gas includes chlorine gas and hexafluoroacetylacetone gas, or the etching gas includes oxygen and hexafluoroacetylacetone gas, the pressure of the etching chamber is 10 mTorr to 500 mTorr, the gas flow rate of hexafluoroacetylacetone gas is 10 standard ml / min to 500 standard ml / min, the gas flow rate of chlorine gas is 10 standard ml / min to 500 standard ml / min, the gas flow rate of oxygen is 10 standard ml / min to 500 standard ml / min, and the etching time is 5 seconds to 50 seconds.

[0104] First, the material of the source-drain interconnection layer 530 is oxidized or chlorinated to form an oxide layer or a chloride layer; then, the oxide layer or the chloride layer is reacted with hexafluoroacetylacetone gas to generate volatile hexafluoroacetylacetonate or acetylacetone compound, thereby easily reducing the difficulty of the atomic layer etching process to remove a portion of the thickness of the source-drain interconnection layer 530. Therefore, in this embodiment, the etching gas of the atomic layer etching process includes chlorine gas and hexafluoroacetylacetone gas, or the etching gas includes oxygen and hexafluoroacetylacetone gas.

[0105] The pressure of the etching chamber should not be too small or too large. If the pressure of the etching chamber is too small, the rate of removing the source-drain interconnect layer of a certain thickness is likely to be too slow, affecting the process efficiency and increasing the process cost; if the pressure of the etching chamber is too large, the rate of removing the source-drain interconnect layer of a certain thickness is likely to be too fast, so that the thickness of the remaining source-drain interconnect layer is difficult to meet the process requirements, thereby affecting the performance of the semiconductor structure. Therefore, in this embodiment, the pressure of the etching chamber is 10 mTorr to 500 mTorr.

[0106] The gas flow rate should not be too small or too low. If the gas flow rate of oxygen or chlorine is too small, the effect of oxidizing or chlorinating the material of the source-drain interconnection layer 530 is not obvious, resulting in poor effect of removing a portion of the thickness of the source-drain interconnection layer 530; if the gas flow rate of oxygen or chlorine is too large, it is easy to increase the probability of other film layers (for example, the etching stop layer 521) being oxidized or chlorinated, that is, the probability of other film layers being damaged is increased; if the gas flow rate of hexafluoroacetylacetone gas is too small, it is easy to remove a portion of the thickness of the source-drain interconnection layer 530. The dimensional accuracy and morphological accuracy of the grooves located between adjacent gate structures are also poor; if the gas flow rate of hexafluoroacetylacetone gas is too large, it is easy to increase the probability of other film layers (for example, the etching stop layer 521) reacting with the hexafluoroacetylacetone gas, that is, the probability of other film layers being damaged is increased. Therefore, in this embodiment, the gas flow rate of hexafluoroacetylacetone gas is 10 standard ml / min to 500 standard ml / min, the gas flow rate of chlorine gas is 10 standard ml / min to 500 standard ml / min, and the gas flow rate of oxygen is 10 standard ml / min to 500 standard ml / min.

[0107] The etching time should not be too short or too long. If the etching time is too short, the effect of removing part of the source-drain interconnection layer is not good, and the dimensional accuracy and morphological accuracy of the grooves between adjacent gate structures are not good; if the etching time is too long, the thickness of the remaining source-drain interconnection layer is difficult to meet the process requirements, thereby affecting the performance of the semiconductor structure. Therefore, in this embodiment, the etching time is 5 seconds to 50 seconds.

[0108] refer to Figure 4In this embodiment, after forming the groove 531 and before forming the protective layer, the forming method further includes: oxidizing the source-drain interconnection layer 530 at the bottom of the groove 531 so that the top surface of the source-drain interconnection layer 530 is oxidized into an oxide layer 532 .

[0109] In the process of removing a portion of the thickness of the source-drain interconnection layer 530 to form the groove 531 between the adjacent gate structures 510, the top surface of the source-drain interconnection layer 530 is easily oxidized, but the oxidation degree of the surface of the source-drain interconnection layer 530 located in different regions is different and difficult to control, thereby increasing the difficulty of the subsequent reduction treatment of the surface of the source-drain interconnection layer 530 to achieve the deoxidation of the surface of the source-drain interconnection layer 530. However, the source-drain interconnection layer 530 at the bottom of the groove 531 is oxidized so that the top surface of the source-drain interconnection layer 530 is oxidized into an oxide layer 532, which makes it easy to make the thickness of the oxide layer 532 on the top surface of the source-drain interconnection layer 530 more uniform, thereby reducing the difficulty of the subsequent reduction treatment of the surface of the source-drain interconnection layer 530 to achieve the deoxidation of the surface of the source-drain interconnection layer 530.

[0110] The thickness of the oxide layer 532 should not be too large or too small. If the thickness of the oxide layer 532 is too large, it is easy for a portion of the thickness of the oxide layer 532 to remain after the subsequent reduction treatment of the surface of the source-drain interconnection layer 530, thereby increasing the self-resistance and contact resistance of the source-drain interconnection layer 530, or it is necessary to increase the time of the subsequent reduction treatment, thereby increasing unnecessary process time; if the thickness of the oxide layer 532 is too small, it is easy for the thickness of the oxide layer 532 on the top surface of the source-drain interconnection layer 530 to be poorly uniform, thereby reducing the process difficulty of the reduction treatment on the surface of the source-drain interconnection layer 530. Therefore, in the present embodiment, in the step of oxidizing the source-drain interconnection layer 530 at the bottom of the groove 531, the thickness of the oxide layer 532 along the normal direction of the top surface of the substrate 500 ranges from 10 angstroms to 50 angstroms.

[0111] Continue to refer Figure 4 , a protection layer 540 covering the source-drain interconnection layer 530 is formed at the bottom of the groove 531 .

[0112] The surface of the source-drain interconnection layer 530 will be subsequently reduced. Before the reduction, the protective layer 540 has covered the source-drain interconnection layer 530, which can protect the source-drain interconnection layer 530, so that the source-drain interconnection layer 530 is not easily oxidized after the subsequent reduction treatment, thereby improving the performance of the source-drain interconnection layer 530 and further improving the performance of the semiconductor structure.

[0113] In this embodiment, in the step of forming the protection layer 540 , the protection layer 540 also covers the sidewalls of the groove 531 , and the protection layer 540 located on the sidewalls of the groove 531 is used as a self-aligned spacer layer.

[0114] When subsequently forming source-drain contact hole plugs, gate source-drain contact hole plugs or gate contact hole plugs, the self-aligned sidewalls can serve as an etching stop layer along the extension direction perpendicular to the gate structure 510, thereby achieving self-alignment in forming source-drain contact hole plugs, gate source-drain contact hole plugs or gate contact hole plugs, reducing the process difficulty of forming source-drain contact hole plugs, gate source-drain contact hole plugs or gate contact hole plugs, and correspondingly improving the position accuracy, size accuracy and morphology accuracy of the source-drain contact hole plugs, gate source-drain contact hole plugs or gate contact hole plugs, thereby improving the quality of the source-drain contact hole plugs, gate source-drain contact hole plugs or gate contact hole plugs, and further improving the performance of the semiconductor structure.

[0115] It should be noted that since the protective layer 140 covering the side wall of the groove 531 serves as a self-aligned sidewall layer, the hardness of the self-aligned sidewall layer is generally higher; if the protective layer also serves as a source and drain capping layer, when the source and drain contact hole plugs or the gate source and drain contact hole plugs are subsequently formed, it is necessary to remove part of the thickness of the protective layer, which will easily increase the process difficulty of forming the source and drain contact hole plugs or the gate source and drain contact hole plugs. Therefore, the protective layer is not suitable as a source and drain capping layer.

[0116] It should also be noted that after the protective layer is formed, the surface of the source-drain interconnection layer needs to be reduced to achieve deoxidation; if the source-drain cap layer is used as a protective layer and directly covers the top of the source-drain interconnection layer, the thickness of the protective layer is likely to be large, thereby increasing the difficulty of the subsequent reduction treatment of the surface of the source-drain interconnection layer 530. Moreover, if the source-drain cap layer is used as a protective layer, the source-drain cap layer also serves as a self-aligned sidewall layer, which tends to reduce the range of material selection for the source-drain cap layer, thereby increasing the difficulty of forming the source-drain cap layer.

[0117] In this embodiment, in the step of forming the protection layer 540 , the protection layer 540 also covers the sidewalls of the groove 531 and the top of the gate structure 510 outside the groove 531 .

[0118] In the step of forming the protective layer 540, the protective layer 540 also covers the side walls of the groove 531 and the top of the gate structure 510 outside the groove 531, which can easily reduce the process difficulty of forming the protective layer 540 and improve the formation quality of the protective layer 540, thereby improving the performance of the semiconductor structure.

[0119] In this embodiment, after forming the groove 531 and before forming the protective layer, the forming method further includes: performing oxidation treatment on the source-drain interconnection layer 530 at the bottom of the groove 531, so that the top surface of the source-drain interconnection layer 530 is oxidized into an oxide layer 532. Accordingly, in the step of forming the protective layer 540, the protective layer 540 covers the oxide layer 532.

[0120] It should be noted that the thickness of the protective layer 540 located at the top of the source-drain interconnection layer 530 along the normal direction of the top surface of the substrate 500 should not be too large or too small. If the thickness of the protective layer 540 located at the top of the source-drain interconnection layer 530 is too large, it is easy to cause the remaining space reserved for the source-drain cap layer to be too small, which makes it difficult to fill the source-drain cap layer in the groove 531 later; if the thickness of the protective layer 540 located at the top of the source-drain interconnection layer 530 is too small, it is easy for the protective layer 540 covering the top of the source-drain interconnection layer 530 to have a poor protection effect on the top surface of the source-drain interconnection layer 530, thereby increasing the probability that the source-drain interconnection layer 530 is oxidized again after the surface of the source-drain interconnection layer 530 is reduced. Therefore, in the present embodiment, in the step of forming the protective layer 540, the thickness of the protective layer 540 located at the top of the source-drain interconnection layer 530 along the normal direction of the top surface of the substrate 500 ranges from 10 angstroms to 100 angstroms.

[0121] In this embodiment, in the step of forming the protection layer 540 , the material of the protection layer 540 includes metal or non-oxide metal compound.

[0122] It should be noted that metals and non-oxide metal compounds generally have a higher hardness, which can reduce the probability of damage to the source-drain interconnection layer 530 during the subsequent process of forming source-drain contact hole plugs.

[0123] It should also be noted that the metal or non-oxide metal compound is a conductive material. In the subsequent reduction treatment of the surface of the source-drain interconnection layer 530 to achieve deoxidation, an oxidation treatment is also performed on a partial thickness of the protective layer 540 to convert a partial thickness of the protective layer 540 into a metal oxide. This makes it easy for the surface of the source-drain interconnection layer 530 to be fully reduced, which is beneficial to improving the quality of the source-drain interconnection layer 530 and thus facilitating electron transmission.

[0124] As an example, in the step of forming the protection layer 540 , the material of the protection layer 540 includes titanium carbide.

[0125] Titanium carbide is a conductive material with a high melting point and good wear resistance. The surface of the source-drain interconnection layer 530 can be subsequently reduced. In the process of deoxidation, a partial thickness of the titanium carbide layer is also oxidized to convert a partial thickness of the titanium carbide layer into titanium oxide. Titanium oxide has good electron transmission properties, so that the heterostructure formed by the source-drain interconnection layer 530 and the protective layer 540 has good electron transmission properties.

[0126] refer to Figure 5 After forming the protection layer 540, the surface of the source-drain interconnection layer 530 is subjected to reduction treatment to achieve deoxidation.

[0127] After forming the protection layer 540, the surface of the source-drain interconnection layer 530 is subjected to reduction treatment to achieve deoxidation; deoxidation is achieved by performing reduction treatment, so that the material on the top surface of the source-drain interconnection layer 530 is the same as the material inside it, so as to improve the quality of the source-drain interconnection layer 530, and because the top of the source-drain interconnection layer 530 is covered with the protection layer 540, the protection layer 540 can protect the source-drain interconnection layer 530, so that the source-drain interconnection layer 530 after the surface of the source-drain interconnection layer 530 is not easily oxidized again, thereby improving the performance of the source-drain interconnection layer 530, and further improving the performance of the semiconductor structure.

[0128] Specifically, in the step of performing reduction treatment on the surface of the source-drain interconnection layer 530 , the reaction gas includes hydrogen gas, and the gas flow rate of the hydrogen gas is 10 standard ml / min to 100 standard ml / min.

[0129] Hydrogen is a highly reducing gas, and its process is highly mature, easy to obtain, and convenient for reduction treatment.

[0130] The gas flow rate of hydrogen should not be too small or too large. If the gas flow rate of hydrogen is too small, it is easy to reduce the efficiency of the reduction process, and it is also easy to cause the surface of the source-drain interconnection layer 530 to not be completely deoxidized, thereby increasing the self-resistance and contact resistance of the source-drain interconnection layer 530, thereby affecting the performance of the semiconductor structure; if the gas flow rate of hydrogen is too large, it is easy to reduce the stability and uniformity of the reduction process, and it may also affect other film layers. Therefore, in this embodiment, the gas flow rate of hydrogen is 10 standard milliliters / minute to 100 standard milliliters / minute.

[0131] In this embodiment, in the step of forming the protection layer 540 , the protection layer 540 covers the oxide layer 532 . Accordingly, in the process of reducing the surface of the source-drain interconnection layer 530 , the oxide layer 532 is also reduced to be reduced to the source-drain interconnection layer 530 .

[0132] In this embodiment, in the step of forming the protective layer 540, the material of the protective layer 540 includes a metal or a non-oxide metal compound. Accordingly, in the process of reducing the surface of the source-drain interconnection layer 530, the protective layer 540 of a portion of the thickness of the surface of the source-drain interconnection layer 530 is also oxidized, so that the material of a portion of the thickness of the protective layer 540 is converted into a metal oxide.

[0133] Since the heterostructure includes metal and metal oxide, or non-oxide metal compound and metal compound, wherein the metal or non-oxide metal compound is a conductive material, the conductive resistance of the heterostructure is small compared with the solution in which the material of the protective layer only includes metal oxide, which is beneficial to electron transmission.

[0134] As an example, in the step of forming the protective layer 540, the material of the protective layer 540 includes titanium carbide. Correspondingly, in the step of oxidizing a portion of the protective layer 540, the material of the metal oxide includes titanium oxide.

[0135] refer to Figure 6 After the reduction treatment, the source / drain capping layer 550 is filled in the groove 531 .

[0136] A source-drain capping layer 550 is filled in the groove 531, that is, the source-drain capping layer 550 is located above the source-drain interconnection layer 530. The source-drain capping layer 550 is used to protect the top of the source-drain interconnection layer 530 in the subsequent process of forming a gate contact hole plug, thereby reducing the probability of damage to the source-drain interconnection layer 530 and short circuit problems between the source-drain interconnection layer 530 and the gate structure 510.

[0137] Specifically, the step of filling the source drain capping layer 550 in the groove 531 includes: filling the groove 531 with a capping material layer (not shown); performing a planarization process to remove the protective layer 540 and the capping material layer outside the groove 531 , and the remaining capping material layer serves as the source drain capping layer 550 .

[0138] First, a cap material layer is filled in the groove 531, and then a planarization process is performed to remove the protection layer 540 and the cap material layer outside the groove 531. The remaining cap material layer is used as a source and drain cap layer, which is conducive to simplifying the process steps.

[0139] It should be noted that, in the process of reducing the surface of the source-drain interconnection layer 530, a partial thickness of the protective layer 540 is also oxidized, so that a partial thickness of the material of the protective layer 540 is converted into metal oxide. Therefore, in the step of removing the protective layer 540 and the cap material layer outside the groove 531, the protective layer 540 converted into metal oxide outside the groove is also removed.

[0140] In this embodiment, the material of the source-drain capping layer 550 includes one or more of silicon nitride, silicon carbide, silicon carbonitride, silicon carbonitride oxide, silicon nitride oxide, boron nitride and boron carbonitride. As an example, the material of the gate capping layer 512 is silicon nitride. Accordingly, the material of the source-drain capping layer 550 is silicon carbide.

[0141] refer to Figure 7In this embodiment, after the source-drain capping layer 550 is filled in the groove 531, the forming method further includes: forming one or both of a source-drain contact hole plug 561 and a gate source-drain contact hole plug 562; wherein, the step of forming the source-drain contact hole plug 561 includes: forming the source-drain contact hole plug 561 on the top of the source-drain interconnection layer 530, the source-drain contact hole plug 561 penetrates the source-drain capping layer 550 between the self-aligned sidewall layers, and is electrically connected to the source-drain interconnection layer 530; the step of forming the gate source-drain contact hole plug 562 includes: forming the gate source-drain contact hole plug 562 on the top of the adjacent gate structure 510 and the source-drain interconnection layer 530, the gate source-drain contact hole plug 562 penetrates the source-drain capping layer 550 between the self-aligned sidewall layers, and is electrically connected to the gate structure 510 and the source-drain interconnection layer 530.

[0142] The source-drain contact plugs 561 are used to realize electrical connection between the source-drain doped layer 520 and an external circuit.

[0143] The gate source-drain contact plugs 562 are used to realize electrical connection between the adjacent source-drain doped layers 520 and the gate structure 510 , and electrical connection between the adjacent source-drain doped layers 520 and the gate structure 510 and an external circuit.

[0144] It should be noted that, in the present embodiment, in the step of forming the source-drain contact hole plug 561 and the gate source-drain contact hole plug 562, a protective layer 540 is provided between the source-drain contact hole plug 561 and the source-drain interconnection layer 530, and between the gate source-drain contact hole plug 562 and the source-drain interconnection layer 530; the protective layer 540 is located between the source-drain contact hole plug 561 and the source-drain interconnection layer 530, and between the gate source-drain contact hole plug 562 and the source-drain interconnection layer 530, which is beneficial to reduce the probability of the source-drain interconnection layer 530 being damaged during the process of forming the source-drain contact hole plug 561 and the gate source-drain contact hole plug 562. In other embodiments, the protective layer may also be penetrated as needed, so that the source-drain contact hole plug and the gate source-drain contact hole plug can be in direct contact with the source-drain interconnection layer.

[0145] Specifically, the source-drain contact plug 561 and the gate source-drain contact plug 562 are made of conductive materials, for example, the conductive materials include metal materials such as tungsten, cobalt, and ruthenium.

[0146] In this embodiment, after filling the source and drain capping layer 550 in the groove 531, the formation method also includes a gate contact hole plug 563; wherein, the step of forming the gate contact hole plug 563 includes: forming the gate contact hole plug 563 on the top of the gate structure 510, the gate contact hole plug 563 passes through the gate capping layer 512 between the self-aligned sidewall layers, and is electrically connected to the gate structure 510.

[0147] The gate contact plug 563 is used to realize electrical connection between the gate structure 510 and an external circuit.

[0148] In this embodiment, the gate contact hole plug 563 is an active gate contact hole plug (Contact Over ActiveGate, COAG). Compared with the solution in which the gate contact hole plug contacts the gate structure located in the isolation area, the use of COAG is beneficial to saving chip area and further reducing the chip size.

[0149] Specifically, the gate contact hole plug 563 is made of a conductive material, for example, the conductive material includes metal materials such as tungsten, cobalt, and ruthenium.

[0150] Although the present invention is disclosed as above, the present invention is not limited thereto. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the scope defined by the claims.

Claims

1. A semiconductor structure, characterized in that: include: substrate; A gate structure, located on the substrate; Source-drain doped layers, located in the substrate on both sides of the gate structure; A source-drain interconnection layer, located at both sides of the gate structure and covering the source-drain doped layer, the source-drain interconnection layer is electrically connected to the source-drain doped layer, and the material of the top surface of the source-drain interconnection layer is the same as the material inside thereof; A source-drain capping layer, located on top of the source-drain interconnection layer; The protection layer is located between the source-drain interconnection layer and the source-drain capping layer, and the protection layer is in contact with the top surface of the source-drain interconnection layer.

2. The semiconductor structure according to claim 1, wherein: The protection layer also extends to cover the sidewalls of the source / drain capping layer, and the protection layer covering the sidewalls of the source / drain capping layer serves as a self-aligned spacer layer.

3. The semiconductor structure according to claim 2, wherein: The semiconductor structure further includes: one or both of a source-drain contact hole plug and a gate source-drain contact hole plug; wherein, The source-drain contact hole plug is located on the top of the source-drain interconnection layer, and the source-drain contact hole plug passes through the source-drain cap layer between the self-aligned sidewalls and is electrically connected to the source-drain interconnection layer; The gate source drain contact hole plug is located on the top of the adjacent gate structure and source drain interconnection layer, and the gate source drain contact hole plug passes through the source drain cap layer between the self-aligned sidewall layers and is electrically connected to the gate structure and the source drain interconnection layer.

4. The semiconductor structure according to claim 1, wherein: The material of the protective layer includes one or more of metal, non-oxide metal compound and metal oxide.

5. The semiconductor structure according to claim 1, wherein: The protection layer includes a first sub-protection layer located on the surface of the source-drain interconnection layer and a second sub-protection layer covering the first sub-protection layer. The material of the first sub-protection layer includes metal oxide, and the material of the second sub-protection layer includes metal or non-oxide metal compound.

6. The semiconductor structure according to claim 5, characterized in that The material of the first sub-protection layer includes titanium oxide, and the material of the second sub-protection layer includes titanium carbide.

7. The semiconductor structure according to claim 1, wherein: Along the normal direction of the top surface of the substrate, the thickness of the protection layer located on the top of the source-drain interconnection layer ranges from 10 angstroms to 100 angstroms.

8. A method for forming a semiconductor structure, characterized in that: include: Providing a substrate, wherein a gate structure is formed on the substrate, source-drain doped layers are formed in the substrate on both sides of the gate structure, a source-drain interconnection layer covering the source-drain doped layers is formed on the substrate on the side of the gate structure, and the source-drain interconnection layer is electrically connected to the source-drain doped layers; Removing a portion of the source-drain interconnection layer along a normal direction of the top surface of the substrate to form a groove between adjacent gate structures; forming a protection layer covering the source-drain interconnection layer at the bottom of the groove; After forming the protection layer, performing reduction treatment on the surface of the source-drain interconnection layer to achieve deoxidation; After the reduction treatment, a source-drain capping layer is filled in the groove.

9. The method for forming a semiconductor structure according to claim 8, wherein: In the step of forming the protective layer, the material of the protective layer includes a metal or a non-oxide metal compound; During the reduction treatment of the surface of the source-drain interconnection layer, a partial thickness of the protective layer on the surface of the source-drain interconnection layer is also oxidized to convert a partial thickness of the protective layer into metal oxide.

10. The method for forming a semiconductor structure according to claim 9, wherein: In the step of forming the protective layer, the material of the protective layer includes titanium carbide; In the step of performing oxidation treatment on a partial thickness of the protective layer, the material of the metal oxide includes titanium oxide.

11. The method for forming a semiconductor structure according to claim 8, wherein: In the step of forming the protection layer, the protection layer also covers the sidewalls of the groove, and the protection layer located on the sidewalls of the groove is used as a self-aligned spacer layer.

12. The method for forming a semiconductor structure according to claim 11, wherein: After the source-drain capping layer is filled in the groove, the forming method further comprises: forming one or both of source-drain contact hole plugs and gate source-drain contact hole plugs; wherein, The step of forming the source-drain contact hole plug comprises: forming a source-drain contact hole plug on the top of the source-drain interconnection layer, wherein the source-drain contact hole plug penetrates the source-drain cap layer between the self-aligned spacer layers and is electrically connected to the source-drain interconnection layer; The step of forming the gate source drain contact hole plug comprises: forming a gate source drain contact hole plug on the top of the adjacent gate structure and source drain interconnection layer, the gate source drain contact hole plug penetrates the source drain cap layer between the self-aligned sidewall layers, and is electrically connected to the gate structure and the source drain interconnection layer.

13. The method for forming a semiconductor structure according to claim 8, wherein: In the step of forming the protection layer, the protection layer also covers the sidewalls of the groove and the top of the gate structure outside the groove; The step of filling the source-drain capping layer in the groove comprises: filling the capping material layer in the groove; A planarization process is performed to remove the protective layer and the cap material layer outside the groove, and the remaining cap material layer is used as a source and drain cap layer.

14. The method for forming a semiconductor structure according to claim 8, wherein: After forming the groove and before forming the protective layer, the forming method further includes: performing oxidation treatment on the source-drain interconnection layer at the bottom of the groove so that the top surface of the source-drain interconnection layer is oxidized into an oxide layer; In the step of forming the protective layer, the protective layer covers the oxide layer; In the process of performing reduction treatment on the surface of the source-drain interconnection layer, the oxide layer is also reduced to reduce the oxide layer to the source-drain interconnection layer.

15. The method for forming a semiconductor structure according to claim 14, wherein: In the step of oxidizing the source-drain interconnection layer at the bottom of the groove, the thickness of the oxide layer is in a range of 10 angstroms to 50 angstroms along the normal direction of the top surface of the substrate.

16. The method for forming a semiconductor structure according to any one of claims 8 to 14, characterized in that: In the step of performing reduction treatment on the surface of the source-drain interconnection layer, the reaction gas includes hydrogen, and the gas flow rate of the hydrogen is 10 standard ml / min to 100 standard ml / min.

17. The method for forming a semiconductor structure according to claim 8, wherein: In the step of forming the protection layer, along the normal direction of the top surface of the substrate, the thickness of the protection layer located on the top of the source-drain interconnection layer ranges from 10 angstroms to 100 angstroms.

18. The method for forming a semiconductor structure according to claim 8, wherein: The process of removing a portion of the thickness of the source-drain interconnection layer includes an atomic layer etching process.

19. The method for forming a semiconductor structure according to claim 18, wherein: The process parameters of the atomic layer etching process include: the etching gas includes chlorine gas and hexafluoroacetylacetone gas, or the etching gas includes oxygen and hexafluoroacetylacetone gas, the pressure of the etching chamber is 10 mTorr to 500 mTorr, the gas flow rate of hexafluoroacetylacetone gas is 10 standard ml / min to 500 standard ml / min, the gas flow rate of chlorine gas is 10 standard ml / min to 500 standard ml / min, the gas flow rate of oxygen is 10 standard ml / min to 500 standard ml / min, and the etching time is 5 seconds to 50 seconds.