High-entropy MXene / LiNO3 modified all-solid-state lithium-sulfur composite positive electrode material, preparation method thereof and all-solid-state lithium-sulfur battery
By using high-entropy MXene/LiNO3-modified composite cathode materials in all-solid-state lithium-sulfur batteries, the problems of low conductivity of solid electrolytes and cathode volume expansion are solved, achieving higher charge-discharge specific capacity and cycle stability, and improving the overall performance of the battery.
Patent Information
- Application Number
- CN202410851780.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-22
AI Technical Summary
Due to the low ionic conductivity and electronic conductivity of the solid electrolyte in all-solid-state lithium-sulfur batteries, the interface resistance is large, which limits the electrochemical reaction, and the volume expansion of the positive electrode causes the electronic path to be disconnected, affecting the charge and discharge capacity and cycle stability of the battery.
An all-solid lithium-sulfur composite cathode material modified with high entropy MXene/LiNO3, including 20% to 30% elemental sulfur powder, 10% to 20% BP2000, 45% to 60% LGPS electrolyte, 5% to 10% High-entropy MXene and 1% to 5% LiNO3 are calcined and ball milled to form a conductive path and supplement lithium agent to improve electron transmission and cycle stability.
The charge-discharge specific capacity and cycle stability of the all-solid-state lithium-sulfur battery are significantly improved. High-entropy MXene provides a conductive path and LiNO3 supplements the lithium agent, which alleviates the capacity attenuation caused by dead lithium and improves the overall performance of the battery.
Smart Images

Figure CN118825232A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of functional materials and relates to an all-solid-state lithium-sulfur composite positive electrode material, and specifically relates to a high-entropy MXene / LiNO3 modified all-solid-state lithium-sulfur composite positive electrode material, a preparation method thereof and an all-solid-state lithium-sulfur battery. Background Art
[0002] Lithium-sulfur batteries have the advantages of high theoretical specific capacity, high theoretical energy density, abundant sulfur resource reserves, low electrode cost, and environmental friendliness, and have become one of the ideal choices for the new generation of energy storage devices. However, for liquid lithium-sulfur batteries, the inherent shuttle effect and safety issues have always hindered their development. As a new battery technology, all-solid-state lithium-sulfur batteries use solid electrolytes instead of liquid electrolytes, so they have many advantages. First, the decomposition temperature of solid electrolytes is higher than that of liquid electrolytes, which enhances the thermal stability of all-solid-state lithium-sulfur batteries and reduces the risk of thermal runaway. Secondly, all-solid-state lithium-sulfur batteries do not produce liquid polysulfides during the cycle. They are completely converted from solid phase S8 to solid phase Li2S and Li2S2, avoiding polysulfides, capacity reduction and safety issues caused by the shuttle effect. Finally, since all-solid-state lithium-sulfur batteries remove separators and liquid electrolytes and are directly assembled with powdered solid electrolytes, they have greater energy storage capacity than liquid lithium-sulfur batteries. Therefore, researchers gradually introduced highly safe solid electrolytes into lithium-sulfur batteries to construct all-solid-state lithium-sulfur battery systems.
[0003] However, the active material sulfur in all-solid-state lithium-sulfur batteries has low ionic conductivity and electronic conductivity. Unlike liquid lithium-sulfur batteries, where the electrolyte can infiltrate the positive electrode material to obtain good contact, all-solid-state lithium-sulfur batteries are assembled from solid powders, and solid-solid contact leads to large interfacial impedance, which limits the electrochemical reaction. In all-solid-state lithium-sulfur batteries, the electrochemical reaction of the active material occurs when ions and electrons are transferred at the three-phase interface composed of active material sulfur / lithium sulfide, solid electrolyte and conductive additives. The number of three-phase interfaces is inseparable from the conductive additives, so this puts forward new requirements for the design of carbon materials.
[0004] In addition, due to the continuous electrochemical reaction, the positive electrode will experience volume expansion, resulting in the disconnection of some ion and electron pathways, thereby generating inactive lithium (dead lithium), which ultimately affects the charge and discharge capacity and cycle stability of the battery. Therefore, the rational design of carbon materials and the timely replenishment of lithium sources have an important impact on the performance of the battery. Summary of the invention
[0005] In view of the shortcomings of the prior art, the object of the present invention is to provide a high-entropy MXene / LiNO3 modified all-solid-state lithium-sulfur composite positive electrode material, a preparation method thereof and an all-solid-state lithium-sulfur battery, which achieve higher charge and discharge specific capacity and better cycle stability.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] A high-entropy MXene / LiNO3 modified all-solid-state lithium-sulfur composite positive electrode material, wherein the raw materials, by mass percentage, include 20% to 30% elemental sulfur powder, 10% to 20% BP2000, 45% to 60% LGPS electrolyte, 5% to 10% high-entropy MXene and 1% to 5% LiNO3;
[0008] The high entropy MXene is TiVNbMoC3.
[0009] The present invention also protects a method for preparing the high-entropy MXene / LiNO3-modified all-solid-state lithium-sulfur composite positive electrode material as described above, comprising the following steps:
[0010] Step 1: Take elemental sulfur powder and BP2000 according to the mass ratio, mix and ball-mill to obtain composite powder A;
[0011] Step 2: calcining the composite powder A in a tube furnace to obtain composite powder B at a calcination temperature of 155° C. for 12 h;
[0012] Step 3: LGPS, high entropy MXene and LiNO3 are mixed with composite powder B according to the mass ratio and ball-milled to obtain a composite positive electrode material;
[0013] The steps 1 to 3 are all carried out in an argon atmosphere.
[0014] Preferably, the ball-to-material ratio of the ball milling in step 1 and step 3 is (30-40):1, the ball milling speed is 400-500 rpm / min, and the ball milling time is 8 hours.
[0015] A high-entropy MXene / LiNO3 modified all-solid-state lithium-sulfur composite positive electrode material prepared by the method as described above and an all-solid-state lithium-sulfur battery comprising the material.
[0016] The preparation method of the all-solid-state lithium-sulfur battery comprises the following steps:
[0017] In an argon atmosphere, 80-100 mg of LGPS electrolyte was weighed and placed in a solid mold, and a force of 2 Tons was applied to it for 3 minutes; then 3-5 mg of the composite positive electrode material was weighed and placed on top of the LGPS electrolyte, and a force of 3 Tons was applied for 3 minutes; finally, a pretreated lithium sheet was placed under the LGPS, and a force of 0.5 Tons was applied for about 15 seconds to obtain an all-solid-state lithium-sulfur battery.
[0018] Preferably, the pretreatment method of the lithium sheet comprises scraping off the black oxidized part on the surface with a scraper and then directly cutting it into 10 mm pieces with a punching pliers.
[0019] Compared with the prior art, the present invention has the following technical effects:
[0020] The present invention provides a path for electrons inside the positive electrode by adding high-entropy MXene (TiVNbMoC3), thereby improving the conductivity of the S positive electrode of the traditional all-solid-state lithium-sulfur battery, ensuring the electron transmission inside the positive electrode, and showing a higher discharge specific capacity; at the same time, the lithium supplement LiNO3 timely supplements the dead lithium generated by volume expansion, alleviates the excessively rapid capacity decay caused by dead lithium, and improves the cycle stability of the battery; an all-solid-state lithium-sulfur battery with a higher charge-discharge specific capacity and better cycle stability is obtained. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 The X-ray diffraction analysis patterns of the all-solid lithium-sulfur composite positive electrode materials of Example 1 and Comparative Example 1;
[0022] Figure 2 This is a SEM image of the composite positive electrode material of Comparative Example 1 before cycling;
[0023] Figure 3 This is a SEM image of the composite cathode material of Example 1 before cycling;
[0024] Figure 4 This is a SEM image of the composite positive electrode material of Comparative Example 1 after cycling;
[0025] Figure 5 This is a SEM image of the composite cathode material of Example 1 after cycling;
[0026] Figure 6 This is the in-situ impedance spectrum of the first cycle of the all-solid-state lithium-sulfur battery of Comparative Example 1;
[0027] Figure 7 This is the in-situ impedance spectrum of the first cycle of the all-solid-state lithium-sulfur battery of Example 1;
[0028] Figure 8 This is the first charge and discharge curve of the all-solid-state lithium-sulfur battery of Comparative Example 1;
[0029] Fig. 9 This is the first charge and discharge curve of the all-solid-state lithium-sulfur battery of Example 1;
[0030] Fig.10 The cycle performance diagram of the all-solid-state lithium-sulfur battery of Example 1 and Comparative Example 1 for the first 20 cycles. DETAILED DESCRIPTION
[0031] The specific contents of the present invention are further explained in detail below in conjunction with embodiments.
[0032] The raw materials used in the present invention can be prepared by those skilled in the art through published literature or purchased;
[0033] In the following embodiments, the manufacturer of BP2000 (BLACK PEARLS2000) is Guangdong Candlelight New Energy Technology Co., Ltd.;
[0034] LGPS electrolyte (Li 10 GeP2S 12 )The manufacturer is Hubei Solid New Energy Technology Co., Ltd.
[0035] Example 1
[0036] (1) Preparation of high-entropy MXene / LiNO3 modified all-solid-state lithium-sulfur composite cathode materials:
[0037] In terms of mass percentage, 20% elemental sulfur powder, 10% BP2000, 60% LGPS electrolyte, 7% high entropy MXene and 3% LiNO3 were taken;
[0038] Step 1: Mix elemental sulfur powder and BP2000 and ball-mill to obtain composite powder A; the ball-to-material ratio is 40:1, the ball milling speed is 400 rpm / min, and the ball milling time is 8 h;
[0039] Step 2: calcining the composite powder A in a tube furnace to obtain composite powder B at a calcination temperature of 155° C. for 12 h;
[0040] Step 3: LGPS, high entropy MXene and LiNO3 were mixed with composite powder B and ball-milled to obtain a composite positive electrode material; the ball-to-material ratio was 30:1, the ball milling speed was 500 rpm / min, and the ball milling time was 8 h;
[0041] (2) After scraping off the black oxidized part on the surface of the lithium sheet with a scraper, cut it directly into 10 mm pieces with a punching pliers;
[0042] (3) Preparation of all-solid-state lithium-sulfur battery: First, weigh 80-100 mg of LGPS electrolyte and place it in a solid mold, apply a force of 2 Tons to it, and maintain it for 3 minutes; then weigh 3-5 mg of composite positive electrode material and place it on top of LGPS, and apply a force of 3 Tons to maintain it for 3 minutes; finally, place a surface-treated lithium sheet under LGPS, apply 0.5 Tons, and maintain it for about 15 seconds to obtain an all-solid-state lithium-sulfur battery.
[0043] After the battery is assembled, apply a force of 0.2Tons to the entire mold, and then tighten the screws of the mold to achieve the effect of applying constant pressure to the battery.
[0044] The above steps (1) to (3) are all carried out in an inert gas Ar.
[0045] The assembled all-solid-state lithium-sulfur battery was left at room temperature for more than 2 hours and then tested.
[0046] Example 2
[0047] (1) Preparation of high-entropy MXene / LiNO3 modified all-solid-state lithium-sulfur composite cathode materials:
[0048] In terms of mass percentage, 20% elemental sulfur powder, 20% BP2000, 45% LGPS electrolyte, 10% high entropy MXene and 5% LiNO3 were taken;
[0049] Step 1: Mix elemental sulfur powder and BP2000 and ball-mill to obtain composite powder A; the ball-to-material ratio is 40:1, the ball milling speed is 400 rpm / min, and the ball milling time is 8 h;
[0050] Step 2: calcining the composite powder A in a tube furnace to obtain composite powder B at a calcination temperature of 155° C. for 12 h;
[0051] Step 3: LGPS, high entropy MXene and LiNO3 were mixed with composite powder B and ball-milled to obtain a composite positive electrode material; the ball-to-material ratio was 30:1, the ball milling speed was 500 rpm / min, and the ball milling time was 8 h;
[0052] (2) After scraping off the black oxidized part on the surface of the lithium sheet with a scraper, cut it directly into 10 mm pieces with a punching pliers;
[0053] (3) Preparation of all-solid-state lithium-sulfur battery: First, weigh 80-100 mg of LGPS electrolyte and place it in a solid mold, apply a force of 2 Tons to it, and maintain it for 3 minutes; then weigh 3-5 mg of composite positive electrode material and place it on top of LGPS, and apply a force of 3 Tons to maintain it for 3 minutes; finally, place a surface-treated lithium sheet under LGPS, apply 0.5 Tons, and maintain it for about 15 seconds to obtain an all-solid-state lithium-sulfur battery.
[0054] After the battery is assembled, apply a force of 0.2Tons to the entire mold, and then tighten the screws of the mold to achieve the effect of applying constant pressure to the battery.
[0055] The above steps (1) to (3) are all carried out in an inert gas Ar.
[0056] The assembled all-solid-state lithium-sulfur battery was left at room temperature for more than 2 hours and then tested.
[0057] Example 3
[0058] (1) Preparation of high-entropy MXene / LiNO3 modified all-solid-state lithium-sulfur composite cathode materials:
[0059] In terms of mass percentage, 30% elemental sulfur powder, 14% BP2000, 50% LGPS electrolyte, 5% high entropy MXene and 1% LiNO3 were taken;
[0060] Step 1: Mix elemental sulfur powder and BP2000 and ball-mill to obtain composite powder A; the ball-to-material ratio is 40:1, the ball milling speed is 500 rpm / min, and the ball milling time is 8 h;
[0061] Step 2: calcining the composite powder A in a tube furnace to obtain composite powder B at a calcination temperature of 155° C. for 12 h;
[0062] Step 3: LGPS, high entropy MXene and LiNO3 are mixed with composite powder B and ball-milled to obtain a composite positive electrode material; the ball-to-material ratio is 30:1, the ball milling speed is 400 rpm / min, and the ball milling time is 8 h;
[0063] (2) After scraping off the black oxidized part on the surface of the lithium sheet with a scraper, cut it directly into 10 mm pieces with a punching pliers;
[0064] (3) Preparation of all-solid-state lithium-sulfur battery: First, weigh 80-100 mg of LGPS electrolyte and place it in a solid mold, apply a force of 2 Tons to it, and maintain it for 3 minutes; then weigh 3-5 mg of composite positive electrode material and place it on top of LGPS, and apply a force of 3 Tons to maintain it for 3 minutes; finally, place a surface-treated lithium sheet under LGPS, apply 0.5 Tons, and maintain it for about 15 seconds to obtain an all-solid-state lithium-sulfur battery.
[0065] After the battery is assembled, apply a force of 0.2Tons to the entire mold, and then tighten the screws of the mold to achieve the effect of applying constant pressure to the battery.
[0066] The above steps (1) to (3) are all carried out in an inert gas Ar.
[0067] The assembled all-solid-state lithium-sulfur battery was left at room temperature for more than 2 hours and then tested.
[0068] Comparative Example 1
[0069] The composite positive electrode material of the comparative example is S: BP2000: LGPS = 3: 1: 6, and no high entropy MXene (TiVNbMoC3) lithium supplement LiNO3 is added, and the remaining steps are consistent with Example 1.
[0070] Test method:
[0071] (1) The in-situ impedance test parameters are frequency 105Hz-0.1Hz and amplitude 0.01mv;
[0072] (2) The battery cycle performance was tested using a blue power system, with the discharge voltage at 1.7 V, the charge voltage at 2.8 V, the charge and discharge current at 0.1 C, and 20 cycles.
[0073] Figure 1 The X-ray diffraction analysis patterns of the all-solid lithium-sulfur composite positive electrode materials of Example 1 and Comparative Example 1 are as follows; Figure 1 It can be seen from the XRD spectrum that the composite positive electrode powder of Example 1 shows typical characteristic peaks of elemental sulfur, LGPS, TiVNbMoC3 and LiNO3, but due to continuous ball milling, the peaks of each substance deviate from their characteristic peak positions.
[0074] Figure 2 This is a SEM image of the composite positive electrode material of Comparative Example 1 before cycling; Figure 3 is a SEM image of the composite cathode material of Example 1 before cycling; Figure 2 and Figure 3 It can be seen that the particle size of the positive electrode material in Comparative Example 1 is relatively uniform, and the particle size of the positive electrode material in Example 1 is almost the same.
[0075] Figure 4 This is a SEM image of the composite positive electrode material of Comparative Example 1 after cycling; Figure 5 is the SEM image of the composite positive electrode material after cycling of Example 1; after the battery cycle, Figure 4 It was found that cracks appeared in the positive electrode material of Comparative Example 1, which is one of the reasons for the decline in battery performance; while the positive electrode material of Example 1 in 5 is relatively complete and no obvious cracks appear.
[0076] Figure 6 This is the in-situ impedance spectrum of the first cycle of the all-solid-state lithium-sulfur battery of Comparative Example 1; Figure 7 The in-situ impedance spectrum of the first cycle of the all-solid-state lithium-sulfur battery of Example 1; Figure 6 It can be seen that the resistance of the positive electrode material in comparative example 1 increases continuously during the first cycle of discharge, and remains almost unchanged during the charging process. Figure 7 During the discharge process, the resistance did not increase, but showed signs of decreasing. This is because the addition of high entropy Mxene and LiNO3 ensured the electron transport inside the electrode.
[0077] Figure 8 This is the first charge and discharge curve of the all-solid-state lithium-sulfur battery of Comparative Example 1; Fig. 9 This is the first charge and discharge curve of the all-solid-state lithium-sulfur battery of Example 1; Figure 8 The all-solid-state lithium-sulfur battery in Comparative Example 1 only showed less than 1100 mAh g -1 The discharge capacity of Fig. 9 In the embodiment 1, the discharge capacity of the all-solid-state lithium-sulfur battery can reach about 1700 mAh g -1 The discharge specific capacity is greater than the theoretical capacity, which is due to the degradation of the electrolyte LGPS in the positive electrode also providing part of the capacity.
[0078] Fig.10 The first 20 cycles of the all-solid-state lithium-sulfur battery of Example 1 and Comparative Example 1 are shown in FIG. Fig.10 It can be seen that the all-solid-state lithium-sulfur battery of Example 1 has better cycle stability than the all-solid-state lithium-sulfur battery of Comparative Example 1.
[0079] Those skilled in the art will appreciate that the above description is only a preferred embodiment of the present invention and does not limit the present invention. Any obvious improvements made to the present invention by those skilled in the art in combination with existing knowledge shall fall within the scope of protection defined by the claims of the present invention.
Claims
1. A high entropy MXene / LiNO3 modified all-solid-state lithium-sulfur composite cathode material, characterized in that: The raw materials include, by mass percentage, 20% to 30% elemental sulfur powder, 10% to 20% BP2000, 45% to 60% LGPS electrolyte, 5% to 10% high entropy MXene and 1% to 5% LiNO3; The high entropy MXene is TiVNbMoC3.
2. A method for preparing a high-entropy MXene / LiNO3-modified all-solid-state lithium-sulfur composite cathode material as claimed in claim 1, characterized in that: The following steps are involved: Step 1: Take elemental sulfur powder and BP2000 according to the mass ratio, mix and ball-mill to obtain composite powder A; Step 2: calcining the composite powder A in a tube furnace to obtain composite powder B at a calcination temperature of 155° C. for 12 h; Step 3: LGPS, high entropy MXene and LiNO3 are mixed with composite powder B according to the mass ratio and ball-milled to obtain a composite positive electrode material; The steps 1 to 3 are all carried out in an argon atmosphere.
3. The method for preparing the high entropy MXene / LiNO3 modified all-solid lithium-sulfur composite cathode material according to claim 2, characterized in that: The ball-to-material ratio of the ball milling in step 1 and step 3 is (30-40):1, the ball milling speed is 400-500 rpm / min, and the ball milling time is 8 hours.
4. A high-entropy MXene / LiNO3 modified all-solid-state lithium-sulfur composite positive electrode material prepared by the method according to claim 2 or 3.
5. An all-solid-state lithium-sulfur battery, characterized in that: The raw materials include the high-entropy MXene / LiNO3 modified all-solid-state lithium-sulfur composite positive electrode material as described in claim 1 or 4.
6. The all-solid-state lithium-sulfur battery according to claim 5, characterized in that: The preparation method comprises the following steps: In an argon atmosphere, 80-100 mg of LGPS electrolyte was weighed and placed in a solid mold, and a force of 2 Tons was applied to it for 3 minutes; then 3-5 mg of the composite positive electrode material was weighed and placed on top of the LGPS electrolyte, and a force of 3 Tons was applied for 3 minutes; finally, a pretreated lithium sheet was placed under the LGPS, and a force of 0.5 Tons was applied for about 15 seconds to obtain an all-solid-state lithium-sulfur battery.
7. The all-solid-state lithium-sulfur battery according to claim 6, characterized in that: The pretreatment method of the lithium sheet comprises scraping off the black oxidized part on the surface with a scraper and then directly cutting it into 10 mm pieces with a punching pliers.
Citation Information
Cited By
All-solid-state lithium-sulfur battery three-dimensional elastic conductive positive electrode frame structure material and preparation method thereof
CN120300190A
Composite positive electrode for solid-state lithium-sulfur battery and preparation method of composite positive electrode
CN120955081A
A composite cathode for solid-state lithium-sulfur batteries and a method of making the same
CN120955081B
Preparation process of lithium ion battery oxide ceramic material
CN122502184A