Rare earth element doped carbon nitride loaded noble metal electrocatalyst as well as preparation method and application thereof

By using carbon nitride doped with rare earth elements to support precious metal electrocatalysts, the problems of poor corrosion resistance and high precious metal loading of catalysts in hydrogen fuel cells are solved, achieving high activity and stable electrocatalysts, improving fuel cell performance and reducing cost.

CN118825307APending Publication Date: 2024-10-22BEIJING NORMAL UNIV AT ZHUHAI
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202410871019.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-01
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

The poor corrosion resistance of catalysts in existing hydrogen fuel cells and the high demand for precious metal loading lead to slow kinetic cathode oxygen reduction and anode hydrogen oxidation reactions, which hinders the performance improvement and commercial application of polymer membrane hydrogen fuel cells.

Method used

A rare earth element-doped carbon nitride-supported precious metal electrocatalyst is used. The rare earth element is coordinated with the pyridinic nitrogen in the carbon nitride ring structure to optimize the electronic structure and interface combination of the catalyst and improve the loading capacity and stability of the precious metal.

Benefits of technology

Significantly improve the activity and durability of the catalyst, improve the performance of the fuel cell, enhance the utilization of precious metals, and reduce the economic cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118825307A_ABST
    Figure CN118825307A_ABST
Patent Text Reader

Abstract

The invention discloses a rare earth element doped carbon nitride loaded noble metal electrocatalyst as well as a preparation method and application thereof, and belongs to the technical field of preparation of a hydrogen oxidation reaction electrocatalyst. Rare earth element doped carbon nitride is used as a substrate, and noble metal-based nanoparticles, clusters or monatomic are loaded. The noble metal-based nanoparticles of the electrocatalyst are uniformly and stably distributed on the rare earth element-doped carbon nitride carrier, and the interface bonding strength of the noble metal and the rare earth element-doped carbon nitride carrier is greatly improved, so that the noble metal-based nanoparticles, clusters or monoatoms are uniformly dispersed in the fuel cell cathode in the electrochemical reaction process; the structure stability can be effectively kept; due to the ultrahigh stability of the rare earth element doped carbon nitride carrier, the catalyst has excellent durability, and the performance of the fuel cell is greatly improved due to higher electrocatalytic activity and excellent durability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of hydrogen oxidation reaction electrocatalyst preparation, and specifically relates to a rare earth element-doped carbon nitride-supported noble metal electrocatalyst and a preparation method and application thereof. Background Art

[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.

[0003] The electrode reactions of hydrogen fuel cells rely on high-performance electrocatalysts. Currently, polymer membrane hydrogen fuel cells (including proton exchange membrane fuel cells and anion exchange membrane fuel cells) are developing rapidly and have been commercialized, but the catalysts still have poor corrosion resistance and high demand for precious metal loading, which seriously limits the performance improvement of polymer membrane hydrogen fuel cells. The cathode oxygen reduction reaction and the anode hydrogen oxidation reaction of the 4-electron process both have slow kinetics and rely on platinum-based precious metal catalysts. In addition, the rate of hydrogen oxidation reaction under alkaline conditions is also 2-3 orders of magnitude slower than that under acidic conditions, which hinders the further development of anion exchange membrane fuel cells. Therefore, improving the activity, stability and precious metal utilization of hydrogen oxidation reaction electrocatalysts is the key to improving the performance of polymer membrane hydrogen fuel cells and their large-scale commercial application. Summary of the invention

[0004] In order to solve the deficiencies of the prior art, the purpose of the present invention is to provide a rare earth element-doped carbon nitride-loaded noble metal electrocatalyst and a preparation method and application thereof. The electrocatalyst provided by the present invention has high catalytic activity and high stability.

[0005] In order to achieve the above object, the technical solution of the present invention is:

[0006] The first aspect of the present invention provides a rare earth element doped carbon nitride supported noble metal electrocatalyst, characterized in that it comprises a substrate and an active component supported on the substrate;

[0007] The substrate is rare earth element doped carbon nitride, and the rare earth element is coordinated with the pyridine nitrogen in the carbon nitride ring structure;

[0008] The active component is a noble metal nanoparticle, cluster or single atom.

[0009] The second aspect of the present invention provides a method for preparing the rare earth element-doped carbon nitride-supported noble metal electrocatalyst, comprising the following steps:

[0010] The rare earth element-doped carbon nitride and the noble metal source are dissolved in a mixed solution of an organic solvent and water, mixed and heated for reaction, and after the reaction is completed, washed, centrifuged and dried to obtain a rare earth element-doped carbon nitride loaded with noble metal electrocatalyst;

[0011] Alternatively, rare earth element-doped carbon nitride and a noble metal source are dissolved in a mixed solution of an organic solvent and water, mixed and evaporated to obtain a precursor material; the obtained precursor material is thermally reduced in a reducing atmosphere to obtain a rare earth element-doped carbon nitride loaded with a noble metal electrocatalyst.

[0012] The third aspect of the present invention provides an application of the rare earth element-doped carbon nitride-supported noble metal electrocatalyst or the rare earth element-doped carbon nitride-supported noble metal electrocatalyst prepared by the preparation method in a hydrogen fuel cell.

[0013] The beneficial effects of the present invention are:

[0014] The present invention provides a rare earth element doped carbon nitride loaded noble metal-based electrocatalyst, which uses rare earth element doped carbon nitride as a substrate and loads noble metal-based nanoparticles, clusters or single atoms. The noble metal-based nanoparticles of the electrocatalyst are evenly and stably distributed on the rare earth element doped carbon nitride carrier, and due to the greatly improved interface bonding strength between the noble metal and the rare earth element doped carbon nitride carrier, the noble metal-based nanoparticles, clusters or single atoms can effectively maintain structural stability during the electrochemical reaction of the fuel cell cathode; due to the ultra-high stability of the rare earth element doped carbon nitride carrier, the catalyst has excellent durability, and the high electrocatalytic activity and excellent durability greatly improve the performance of the fuel cell.

[0015] The present invention adopts rare earth elements including lanthanum, cerium, praseodymium, neodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, lutetium, scandium and yttrium to dope carbon nitride carrier, rare earth elements and pyridine nitrogen in carbon nitride ring structure are coordinated, the surface charge distribution of carbon nitride carrier is optimized, it is conducive to regulating the electronic structure of precious metal platinum, and further improves the intrinsic activity of composite catalyst. At the same time, rare earth elements have a large number of d or f empty orbitals that can act as Lewis acid to selectively absorb OH - , which is beneficial to increase the OH near the active site - The concentration of lanthanum, cerium, praseodymium, neodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, lutetium, scandium and yttrium rare earth elements are doped to enhance the interface bond and interaction between carbon nitride carrier and platinum precious metal, effectively inhibit the dissolution, migration and agglomeration of platinum metal sites during the catalytic reaction, and improve the structural stability of the catalyst after long cycles.

[0016] The provided rare earth element-doped carbon nitride carrier material has the advantages of ultra-high stability, high specific surface area, and low cost, and the preparation method is simple and easy to control, which helps to reduce economic costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.

[0018] Figure 1 The XRD spectrum of the terbium-doped carbon nitride-supported platinum composite electrocatalyst prepared in Example 1 of the present invention;

[0019] Figure 2 TEM image of the terbium-doped carbon nitride-supported platinum composite electrocatalyst prepared in Example 1 of the present invention;

[0020] Figure 3 The FTIR spectrum of the terbium-doped carbon nitride-supported platinum composite electrocatalyst prepared in Example 1 of the present invention;

[0021] Figure 4 This is the LSV curve of the terbium-doped carbon nitride-supported platinum composite electrocatalyst prepared in Example 1 of the present invention;

[0022] Figure 5 This is the LSV curve of the europium-doped carbon nitride-supported palladium composite electrocatalyst prepared in Example 3 of the present invention. DETAILED DESCRIPTION

[0023] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the present invention.

[0024] All raw materials of the present invention have no particular limitation on their sources, and can be purchased from the market or prepared according to conventional methods known to those skilled in the art.

[0025] There is no particular limitation on the purity of all raw materials in the present invention. The present invention preferably uses analytically pure materials or materials of conventional purity used in the field of palladium nanoparticle synthesis.

[0026] All noun expressions, abbreviations and trademarks in the present invention are conventional noun expressions, abbreviations and trademarks in the field. Each noun expression, abbreviation and trademark is clear and unambiguous in its relevant application field, and those skilled in the art can clearly, accurately and uniquely understand it based on the noun expressions, abbreviations and trademarks.

[0027] A typical embodiment of the present invention provides a rare earth element-doped carbon nitride-supported noble metal electrocatalyst, comprising a substrate and an active component supported on the substrate;

[0028] The substrate is rare earth element doped carbon nitride, and the rare earth element is coordinated with the pyridine nitrogen in the carbon nitride ring structure;

[0029] The active component is a noble metal nanoparticle, cluster or single atom.

[0030] The present invention adopts rare earth elements (including lanthanum, cerium, praseodymium, neodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, lutetium, scandium and yttrium) to dope carbon nitride carrier, rare earth elements coordinate with pyridine nitrogen in carbon nitride ring structure, optimize the surface charge distribution of carbon nitride carrier, help to control the electronic structure of precious metal, and further improve the intrinsic activity of composite catalyst. Rare earth elements have a large number of d or f empty orbitals that can act as Lewis acid to selectively absorb OH - , which is beneficial to increase the OH near the active site - concentration, synergistically accelerating the oxidation of hydrogen and improving the activity of the composite catalyst. At the same time, the doping of rare earth elements is conducive to strengthening the interface bond and interaction between the carbon nitride carrier and the precious metal, effectively inhibiting the dissolution, migration and agglomeration of the precious metal sites during the catalytic reaction, and improving the structural stability of the catalyst after long circulation.

[0031] The rare earth element-doped carbon nitride-supported noble metal electrocatalyst provided by the present invention has the advantages of ultra-high stability, high specific surface area and low cost, and the preparation method is simple and easy to control, which helps to reduce economic costs.

[0032] In some examples of this embodiment, the rare earth element is selected from one of lanthanum, cerium, praseodymium, neodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, lutetium, scandium or yttrium, preferably terbium, dysprosium, lanthanum, europium, ytterbium, further preferably terbium, and the doping amount of the rare earth element is 1%-10%, mass percentage.

[0033] In some examples of this embodiment, the size of the noble metal particles or noble metal clusters is 1-10 nm;

[0034] The noble metal is selected from one of platinum, platinum alloy, palladium, palladium alloy, iridium or iridium alloy, and the mass percentage of the noble metal in the rare earth element-doped carbon nitride-supported noble metal electrocatalyst is 5-40wt.%.

[0035] Another typical embodiment of the present invention provides a method for preparing the above-mentioned rare earth element-doped carbon nitride-supported noble metal electrocatalyst, comprising the following steps:

[0036] The rare earth element-doped carbon nitride and the noble metal source are dissolved in a mixed solution of an organic solvent and water, mixed and heated for reaction, and after the reaction is completed, washed, centrifuged and dried to obtain a rare earth element-doped carbon nitride loaded with noble metal electrocatalyst;

[0037] Alternatively, rare earth element-doped carbon nitride and a noble metal source are dissolved in a mixed solution of an organic solvent and water, mixed and evaporated to obtain a precursor material; the obtained precursor material is thermally reduced in a reducing atmosphere to obtain a rare earth element-doped carbon nitride loaded with a noble metal electrocatalyst.

[0038] In some examples of this implementation mode, the method for preparing the rare earth element-doped carbon nitride comprises the following steps:

[0039] The carbon nitride precursor and the rare earth salt are mixed, and heat treated at 400-650°C for 2-5h in an air atmosphere with a heating rate of 2-10°C / min; after the heat treatment, the obtained product is washed and dried to obtain rare earth element-doped carbon nitride.

[0040] The carbon nitride precursor is selected from one or more of cyanamide, ammonium thiocyanate, dicyandiamide, melamine, thiourea or urea, preferably dicyandiamide. The mass ratio of the carbon nitride precursor to the rare earth salt is (8-11):1.

[0041] The rare earth salt is one of lanthanum salt, cerium salt, praseodymium salt, neodymium salt, promethium salt, samarium salt, europium salt, gadolinium salt, terbium salt, dysprosium salt, holmium salt, erbium salt, thulium salt, ytterbium salt, lutetium salt, scandium salt or yttrium salt.

[0042] Preferably, the lanthanum salt includes but is not limited to lanthanum chloride, lanthanum chloride hydrate (such as lanthanum chloride heptahydrate, lanthanum chloride hexahydrate), lanthanum sulfate, lanthanum sulfate hydrate, lanthanum nitrate, lanthanum nitrate hydrate (such as lanthanum nitrate hexahydrate), lanthanum acetate, lanthanum acetate hydrate, lanthanum carbonate, lanthanum carbonate hydrate, lanthanum acetate sesquihydrate, lanthanum bromide, lanthanum bromide hydrate, lanthanum phosphate or lanthanum phosphate hydrate.

[0043] Preferably, the cerium salt is cerium chloride heptahydrate, cerium oxalate hydrate, ammonium cerium sulfate dihydrate or cerium sulfate tetrahydrate.

[0044] Preferably, the praseodymium salt includes but is not limited to praseodymium sulfate hydrate (such as praseodymium nitrate hexahydrate), praseodymium chloride hexahydrate or praseodymium chloride.

[0045] Preferably, the neodymium salt includes but is not limited to neodymium chloride, neodymium nitrate, neodymium acetate or neodymium sulfate and hydrates thereof.

[0046] Preferably, the promethium salt includes but is not limited to promethium chloride, promethium nitrate, promethium acetate or promethium sulfate.

[0047] Preferably, the samarium salt includes but is not limited to samarium chloride, samarium nitrate, samarium acetate or samarium sulfate.

[0048] Preferably, the europium salt includes but is not limited to europium nitrate pentahydrate, europium chloride hexahydrate or europium sulfate decahydrate.

[0049] Preferably, the gadolinium salt includes but is not limited to gadolinium nitrate hexahydrate, gadolinium chloride hexahydrate or gadolinium sulfate octahydrate.

[0050] Preferably, the terbium salt includes but is not limited to terbium nitrate hexahydrate, terbium nitrate pentahydrate, terbium chloride hexahydrate or terbium sulfate octahydrate.

[0051] Preferably, the dysprosium salt includes but is not limited to dysprosium nitrate hydrate (such as dysprosium nitrate hexahydrate, dysprosium nitrate pentahydrate), dysprosium chloride hexahydrate or dysprosium sulfate octahydrate.

[0052] Preferably, the holmium salt includes but is not limited to holmium sulfate hydrate (such as holmium nitrate hexahydrate), holmium nitrate hydrate (such as holmium nitrate pentahydrate) or holmium chloride hexahydrate.

[0053] Preferably, the erbium salt includes but is not limited to erbium nitrate hexahydrate, erbium nitrate pentahydrate, erbium nitrate hydrate, erbium chloride hexahydrate or erbium sulfate hydrate.

[0054] Preferably, the thulium salt includes but is not limited to thulium nitrate hydrate (such as thulium nitrate hexahydrate, thulium nitrate pentahydrate), thulium chloride hexahydrate or thulium sulfate hydrate.

[0055] Preferably, the ytterbium salt includes but is not limited to ytterbium nitrate hydrate (ytterbium nitrate hexahydrate, ytterbium nitrate pentahydrate), ytterbium chloride hexahydrate or ytterbium sulfate octahydrate.

[0056] Preferably, the lutetium salt includes but is not limited to lutetium nitrate hydrate (such as lutetium nitrate hexahydrate, lutetium nitrate pentahydrate), lutetium chloride hexahydrate or lutetium sulfate octahydrate.

[0057] Preferably, the scandium salt includes but is not limited to scandium nitrate hydrate, scandium acetate hydrate, scandium chloride hydrate or scandium sulfate hydrate.

[0058] Preferably, the yttrium salt includes but is not limited to yttrium nitrate hydrate, yttrium acetate hydrate, yttrium phosphate, yttrium chloride hexahydrate or yttrium sulfate octahydrate.

[0059] Wherein, the mixing method includes but is not limited to distillation, freeze drying, ball milling or grinding.

[0060] The specific process of washing is: washing the obtained product in 1-3M hydrochloric acid for multiple times, preferably 1-3 times, and then washing with deionized water until neutral.

[0061] In some examples of this embodiment, the noble metal source is any one or more of a platinum salt, a palladium salt or an iridium salt.

[0062] Preferably, the platinum salt includes but is not limited to a mixture of one or more of platinum acetylacetonate, chloroplatinic acid, sodium chloroplatinate or potassium chloroplatinate in any proportion.

[0063] Preferably, the palladium salt includes but is not limited to a mixture of one or more of palladium acetylacetonate, chloropalladic acid, sodium chloropalladate or potassium chloropalladate in any proportion.

[0064] Preferably, the iridium source salt includes but is not limited to a mixture of one or more of iridium chloride and potassium chloroiridate in any proportion.

[0065] In some examples of this embodiment, in the mixed solution of the organic solvent and water, the organic solvent is alcohol or N,N-dimethylformamide, and the volume ratio of alcohol or N,N-dimethylformamide to water is (1-3):(3-5).

[0066] In order to further improve the mixing effect, the rare earth element-doped carbon nitride and the noble metal source are dissolved in a mixed solution of an organic solvent and water, and then ultrasonicated for 1-4 hours.

[0067] In some embodiments of this embodiment, the heating reaction has a reaction temperature of 60-160° C. and a reaction time of 3-7 hours. It is understandable that an oil bath or a water bath can be used for the heating reduction reaction. After the oil bath or water bath heating reaction is completed, the reaction is repeatedly washed and centrifuged with deionized water and ethanol, respectively, and vacuum dried to obtain a rare earth element-doped carbon nitride-supported noble metal electrocatalyst.

[0068] In some examples of this embodiment, the rare earth element doped carbon nitride and the noble metal source are dissolved in a mixed solution of an organic solvent and water, mixed and evaporated to dryness at 50-80° C., and then placed in an argon-hydrogen mixed atmosphere for thermal reduction. Preferably, the thermal reduction is performed at 200-600° C. to obtain a rare earth element doped carbon nitride loaded with a noble metal electrocatalyst.

[0069] A third typical embodiment of the present invention provides an application of the rare earth element-doped carbon nitride-loaded precious metal electrocatalyst or the rare earth element-doped carbon nitride-loaded precious metal electrocatalyst prepared by the preparation method in a hydrogen fuel cell.

[0070] In the rare earth element doped carbon nitride supported noble metal electrocatalyst provided by the present invention, the noble metal-based nanoparticles are evenly and stably distributed on the rare earth element doped carbon nitride carrier. Due to the greatly improved interfacial bonding strength between the noble metal and the rare earth element doped carbon nitride carrier, the noble metal-based nanoparticles, clusters or single atoms can effectively maintain structural stability during the electrochemical reaction at the cathode of the fuel cell. Due to the ultra-high stability of the rare earth element doped carbon nitride carrier, the catalyst has excellent durability, and the higher electrocatalytic activity and excellent durability greatly improve the performance of the fuel cell.

[0071] In order to enable those skilled in the art to more clearly understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below in conjunction with specific embodiments.

[0072] Example 1

[0073] A terbium-doped carbon nitride-supported platinum hydrogen oxidation reaction electrocatalyst, the preparation method specifically comprising:

[0074] (1) Preparation method of terbium-doped carbon nitride:

[0075] 3g of melamine and 0.3g of terbium nitrate hexahydrate were dissolved in a mixed solution of 30mL of ethanol and water (volume ratio of 1:1), and magnetically stirred at 60°C until the solution was completely evaporated to obtain a precursor mixture. The obtained precursor mixture was placed in a porcelain boat, placed in a tube furnace, and heated to 550°C at a heating rate of 2.5°C / min. After being kept warm for 3 hours, it was cooled to room temperature to obtain terbium-doped carbon nitride. The obtained terbium-doped carbon nitride was then centrifuged and washed twice with a 1M hydrochloric acid solution, and then repeatedly washed with deionized water until the pH was close to 7, and then placed in a blast drying oven for 10 hours to finally obtain terbium-doped carbon nitride.

[0076] (2) Preparation method of terbium-doped carbon nitride supported platinum composite electrocatalyst:

[0077] 80 mg of terbium-doped carbon nitride was dissolved in a mixed solvent of 90 mL of ethylene glycol and 120 mL of deionized water, and then 0.3 mL of a 0.1 M hexachloroplatinic acid aqueous solution was added. The resulting mixed solution was ultrasonicated for 2 hours and then heated in an oil bath at 120°C for 4 hours. After the reaction was completed, it was repeatedly washed with ethanol and water, centrifuged, and finally dried in a vacuum drying oven at 60°C to obtain a terbium-doped carbon nitride loaded with platinum (the mass fraction of platinum was about 15wt.%) composite electrocatalyst.

[0078] The terbium-doped carbon nitride carrier-supported platinum composite electrocatalyst obtained in this example was characterized by XRD. Figure 1 As shown. The average particle size of the doped carbon nitride supported platinum is about 3nm, as shown Figure 2 The Fourier transform infrared spectrum (FTIR) is shown as Figure 3 As shown, the doped carbon nitride support can be observed at 810 cm -1 There are obvious triazine ring stretching peaks at 1200-1600cm -1 There are seven azine ring stretching peaks in the range, indicating the azine ring structure of the terbium-doped carbon nitride support.

[0079] The terbium-doped carbon nitride-supported platinum composite electrocatalyst obtained in this example was subjected to a hydrogen oxidation reaction test: 2 mg of the composite catalyst prepared above was added with 100 μL of isopropanol, 384 μL of water and 16 μL of a 5 wt.% Nafion solution, and ultrasonically dispersed for 2 h to obtain a uniform slurry, and 4 mg mL -1 10 μL of the slurry was evenly dropped on the surface of a glassy carbon electrode (5 mm in diameter) and dried to obtain an electrocatalyst loading of 200 μg cm -2 The working electrode was selected as the counter electrode, the saturated calomel electrode as the reference electrode, and the 0.1M potassium hydroxide solution as the electrolyte. Hydrogen was passed at a flow rate of 300mL / min for 30min to saturate the solution with hydrogen. The working electrode was fixed in the three-electrode electrolytic cell using an electrochemical workstation and the cyclic voltammetry curve was obtained at a scan rate of 50mV / s; the working electrode speed was 400-2025r.pm / min, and the polarization curves at different speeds were obtained at a linear scan rate of 1mV / s.

[0080] After testing, the terbium-doped carbon nitride carrier-supported platinum composite electrocatalyst in this embodiment was -1 In KOH solution, the limiting current density is close to 2.97 mA cm at a rotation speed of 1600 r.pm / min. -2 ,like Figure 4 shown.

[0081] Comparative Example 1

[0082] Commercial carbon-supported platinum and graphite-phase carbon nitride-supported platinum were used as control samples. The preparation method of this comparative example was basically the same as that of Example 1, except that: the preparation of graphite-phase carbon nitride was carried out in the following specific steps: 3 g of melamine was placed in a porcelain boat, placed in a tube furnace, heated to 550° C. at a heating rate of 2.5° C. / min, kept warm for 3 hours, and cooled to room temperature to obtain graphite-phase carbon nitride. The remaining steps were the same as those of Example 1.

[0083] The prepared commercial carbon-supported platinum and graphite-phase carbon nitride-supported platinum were subjected to hydrogen oxidation reaction tests, and the test method was consistent with that of Example 1. The test results are shown in FIG. Figure 4 As shown in the figure, it can be seen that the commercial carbon-supported platinum and graphite carbon nitride-supported platinum reach 2.85 mA cm -2 and 2.63 mA cm-2 , significantly lower than 2.97 mA cm -2 .

[0084] Example 2

[0085] A dysprosium-doped carbon nitride-supported platinum hydrogen oxidation reaction electrocatalyst, the preparation method specifically comprising:

[0086] (1) Preparation method of dysprosium-doped carbon nitride:

[0087] Dissolve 4g of dicyandiamide and 0.42g of dysprosium nitrate hexahydrate in 50mL of deionized water, freeze-dry, and obtain a precursor mixture. Place the obtained precursor mixture in a porcelain boat, place it in a tube furnace, heat it to 500°C at a heating rate of 3°C / min, keep it warm for 4h, and cool it to room temperature to obtain dysprosium-doped carbon nitride. Then wash the above dysprosium-doped carbon nitride twice with a 2M hydrochloric acid solution by centrifugation, then wash it repeatedly with deionized water until the pH is close to 7, and then place it in a forced air drying oven to dry for 10h to finally obtain dysprosium-doped carbon nitride.

[0088] (2) Preparation method of dysprosium-doped carbon nitride supported platinum composite electrocatalyst:

[0089] 80 mg of dysprosium-doped carbon nitride was dissolved in a mixed solvent of 150 mL of N,N-dimethylformamide and 200 mL of deionized water, and then 0.3 mL of a 0.1 M hexachloroplatinic acid aqueous solution was added. The resulting mixed solution was ultrasonicated for 2 hours and then heated at 120°C in an oil bath for 4 hours. After the reaction was completed, it was repeatedly washed with ethanol and water, centrifuged, and finally dried in a vacuum drying oven at 60°C to obtain a dysprosium-doped carbon nitride loaded with platinum (the mass fraction of platinum was about 7 wt.%) composite electrocatalyst.

[0090] The dysprosium-doped carbon nitride carrier-supported platinum composite electrocatalyst obtained in this example was subjected to a hydrogen oxidation reaction test, and the specific steps were the same as those in Example 1.

[0091] After testing, the dysprosium-doped carbon nitride carrier-supported platinum composite electrocatalyst in this embodiment was -1 In KOH solution, the limiting current density is close to 2.97 mA cm at a rotation speed of 1600 r.pm / min. -2 ,like Figure 5 shown.

[0092] Comparative Example 2

[0093] Commercial carbon-supported platinum and graphite-phase carbon nitride-supported platinum were used as control samples. The preparation method of this comparative example was basically the same as that of comparative example 1, except that: the preparation of graphite-phase carbon nitride was carried out in the following specific steps: 4 g of dicyandiamide was placed in a porcelain boat, placed in a tube furnace, heated to 500° C. at a heating rate of 3° C. / min, kept warm for 4 hours, and cooled to room temperature to obtain graphite-phase carbon nitride. The remaining steps were the same as those of Example 2.

[0094] The commercial carbon-supported platinum and graphite-phase carbon nitride-supported platinum were subjected to hydrogen oxidation reaction tests, and the test method was consistent with that in Example 1.

[0095] The test results are as follows Figure 5 As shown in the figure, it can be seen that the commercial carbon-supported platinum and graphite carbon nitride-supported platinum reach 2.85 mA cm -2 and 2.63 mA cm -2 , significantly lower than 2.97 mA cm -2 .

[0096] Example 3

[0097] A europium-doped carbon nitride-supported palladium oxygen reduction reaction electrocatalyst, the preparation method specifically comprising:

[0098] (1) Preparation method of europium-doped carbon nitride:

[0099] Dissolve 4g of dicyandiamide and 0.42g of europium nitrate hexahydrate in 50mL of deionized water, freeze-dry, and obtain a precursor mixture. Place the obtained precursor mixture in a porcelain boat, place it in a tube furnace, and heat it to 500°C at a heating rate of 3°C / min. Keep it warm for 4 hours and then cool it to room temperature to obtain europium-doped carbon nitride. Then, wash the europium-doped carbon nitride twice with a 2M hydrochloric acid solution by centrifugation, then wash it repeatedly with deionized water until the pH is close to 7, and then place it in a forced air drying oven to dry for 10 hours to finally obtain europium-doped carbon nitride.

[0100] (3) Preparation method of europium-doped carbon nitride-supported palladium composite electrocatalyst:

[0101] 80 mg of europium-doped carbon nitride was dissolved in a mixed solvent of 150 mL of N,N-dimethylformamide and 200 mL of deionized water, and 20 mg of acetylacetonate palladium was added. The resulting solution was ultrasonically treated for 2 h until mixed uniformly, and then heated at 120 ° C in an oil bath for 4 h. After the reaction was completed, it was repeatedly washed with ethanol and water, centrifuged, and finally dried in a vacuum drying oven at 60 ° C to obtain a europium-doped carbon nitride loaded with palladium (the mass fraction of palladium is about 8 wt.%) composite electrocatalyst.

[0102] The europium-doped carbon nitride-supported palladium composite electrocatalyst obtained in this example was tested for oxygen reduction reaction:

[0103] Take 4 mg of the composite catalyst prepared above, add 200 μL of isopropanol, 768 μL of water and 32 μL of 5 wt.% Nafion solution, and disperse it ultrasonically for 2 h to obtain a uniform slurry. Take 10 μL of the slurry and drop it into a 0.196 cm 2 The surface of the glassy carbon electrode was dried in a fume hood for 2 h to obtain a loading of 0.2 mg / cm 2 The working electrode was selected as the counter electrode, the platinum wire electrode was selected as the reference electrode, the Hg / HgO electrode was selected as the reference electrode, and the 0.1M potassium hydroxide solution was selected as the electrolyte. Oxygen was passed through the solution at a flow rate of 100mL / min for 30min to saturate the solution with oxygen. The working electrode was fixed in the three-electrode electrolytic cell using an electrochemical workstation and the cyclic voltammetry curve was obtained at a scan rate of 50mV / s; the working electrode speed was 400-2025r.pm / min, and the polarization curves at different speeds were obtained at a linear scan rate of 10mV / s.

[0104] After testing, the europium-doped carbon nitride-supported palladium composite electrocatalyst in this embodiment reached a half-wave potential of 0.92 V (vs. RHE) and a limiting current density of nearly 5.7 mA / cm 2 .

[0105] Comparative Example 3

[0106] Commercial carbon-supported palladium and graphite carbon nitride-supported palladium were used as control samples. The preparation method of this comparative example was the same as that of comparative example 2.

[0107] Commercial carbon-supported palladium and graphite carbon nitride-supported palladium were tested for oxygen reduction reaction, and the test method was the same as that of Example 3. After testing, the half-wave potentials of commercial carbon-supported palladium and graphite carbon nitride-supported palladium were 0.89 and 0.86 V (vs. RHE), respectively, and the limiting current density reached 5.1 mA cm -2 and 4.8mAcm -2 , significantly lower than 5.7 mA cm -2 .

[0108] Example 4

[0109] A lanthanum-doped carbon nitride-supported iridium hydroxide oxidation reaction electrocatalyst, the preparation method specifically comprising:

[0110] (1) Preparation method of lanthanum-doped carbon nitride:

[0111] Dissolve 4g of dicyandiamide and 0.42g of lanthanum nitrate hexahydrate in 50mL of deionized water, freeze-dry, and obtain a precursor mixture. Place the obtained precursor mixture in a porcelain boat, place it in a tube furnace, and heat it to 500°C at a heating rate of 3°C / min. Keep it warm for 4 hours and then cool it to room temperature to obtain lanthanum-doped carbon nitride. Then wash the lanthanum-doped carbon nitride twice with a 2M hydrochloric acid solution by centrifugation, then wash it repeatedly with deionized water until the pH is close to 7, and then place it in a forced air drying oven for 10 hours to finally obtain lanthanum-doped carbon nitride.

[0112] (2) Preparation method of lanthanum-doped carbon nitride-supported iridium composite electrocatalyst:

[0113] 80 mg of lanthanum-doped carbon nitride was dissolved in a mixed solvent of 150 mL of isopropanol and 200 mL of deionized water, and 44 mg of potassium chloroiridate was added. The resulting solution was ultrasonically treated for 2 hours until mixed uniformly, and then heated in an oil bath at 140°C for 6 hours. After the reaction was completed, it was repeatedly washed with ethanol and water, centrifuged, and finally placed in a vacuum drying oven at 60°C for drying to obtain a lanthanum-doped carbon nitride loaded with iridium (the mass fraction of iridium was about 20wt.%) composite electrocatalyst.

[0114] The lanthanum-doped carbon nitride-supported iridium composite electrocatalyst obtained in this example was subjected to a hydrogen oxidation reaction test, and the specific test steps were the same as those in Example 1.

[0115] After testing, the lanthanum-doped carbon nitride-supported iridium composite electrocatalyst in this embodiment was -1 In KOH solution, the limiting current density is close to 2.6 mA cm at a rotation speed of 1600 r.pm / min. -2 .

[0116] Comparative Example 4

[0117] Commercial carbon-supported iridium and graphite-phase carbon nitride-supported iridium were used as control samples. The preparation method of this comparative example was basically the same as that of comparative example 2, except that the preparation of graphite-phase carbon nitride was carried out by placing 4 g of dicyandiamide in a porcelain boat, placing it in a tube furnace, heating it to 500° C. at a heating rate of 3° C. / min, and cooling it to room temperature after keeping it for 4 hours to obtain graphite-phase carbon nitride. The rest of the steps were the same as those in Example 4.

[0118] Commercial carbon-supported iridium and graphite-phase carbon nitride-supported iridium were subjected to hydrogen oxidation reaction tests, and the test method was consistent with that of Example 4.

[0119] After testing, commercial carbon-supported iridium and graphite-phase carbon nitride-supported iridium reached 2.1 mA cm -2 and 2.4 mA cm -2 , significantly lower than 2.6 mA cm -2 .

[0120] Example 5

[0121] An ytterbium-doped carbon nitride-supported platinum oxygen reduction reaction electrocatalyst, the preparation method specifically comprising:

[0122] (1) Preparation method of ytterbium-doped carbon nitride:

[0123] 4g of dicyandiamide and 0.45g of ytterbium nitrate hexahydrate were dissolved in 50mL of deionized water. After freeze drying, the above mixed precursor mixture was placed in a porcelain boat, placed in a tube furnace, and heated to 450°C at a heating rate of 2°C / min, kept warm for 3h, and cooled to room temperature to obtain ytterbium-doped carbon nitride. The above ytterbium-doped carbon nitride was then centrifugally washed twice with a 1M hydrochloric acid solution, and then repeatedly washed with deionized water until the pH was close to 7, and then placed in a blast drying oven for 10h to finally obtain ytterbium-doped carbon nitride.

[0124] (2) Preparation method of ytterbium-doped carbon nitride-supported platinum composite electrocatalyst:

[0125] 80 mg of ytterbium-doped carbon nitride was dissolved in a mixed solvent of 150 mL of N,N-dimethylformamide and 200 mL of deionized water, and then 0.9 mL of a 0.1 M hexachloroplatinic acid aqueous solution was added. The resulting mixed solution was ultrasonicated for 2 hours and then heated at 120°C in an oil bath for 6 hours. After the reaction was completed, it was repeatedly washed with ethanol and water, centrifuged, and finally dried in a vacuum drying oven at 60°C to obtain an ytterbium-doped carbon nitride loaded with platinum (the mass fraction of platinum was about 20 wt.%) composite electrocatalyst.

[0126] The ytterbium-doped carbon nitride-supported platinum composite electrocatalyst obtained in this example was tested for oxygen reduction reaction, and the test steps were the same as those in Example 2.

[0127] After testing, the half-wave potential of the Yb-doped carbon nitride supported platinum composite electrocatalyst in this embodiment is 0.91V (vs. RHE), and the limiting current density is close to 5.1mA / cm 2 .

[0128] Comparative Example 5

[0129] Commercial carbon-supported platinum and graphite phase carbon nitride-supported platinum were used as control samples. The preparation method of this comparative example was the same as that of comparative example 2.

[0130] Commercial carbon-supported platinum and graphite-phase carbon nitride-supported platinum were tested for oxygen reduction reaction using the same testing method as in Example 5.

[0131] After testing, the half-wave potentials of commercial carbon-supported platinum and graphite-phase carbon nitride-supported platinum were 0.89 and 0.85 V (vs. RHE), respectively, and the limiting current density reached 5.0 mA cm -2 and 4.8mAcm -2 , significantly lower than 5.1mAcm-2 .

[0132] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A rare earth element doped carbon nitride supported noble metal electrocatalyst, characterized in that: comprising a substrate and an active ingredient loaded on the substrate; The substrate is rare earth element doped carbon nitride, and the rare earth element is coordinated with the pyridine nitrogen in the carbon nitride ring structure; The active component is a noble metal nanoparticle, cluster or single atom.

2. The rare earth element-doped carbon nitride-supported noble metal electrocatalyst according to claim 1, characterized in that: The rare earth element is selected from one of lanthanum, cerium, praseodymium, neodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, lutetium, scandium or yttrium, and the doping amount of the rare earth element is 1%-10%, mass percentage.

3. The rare earth element-doped carbon nitride-supported noble metal electrocatalyst according to claim 1, characterized in that: The size of the noble metal particles or noble metal clusters is 1-10 nm; The noble metal is selected from one of platinum, platinum alloy, palladium, palladium alloy, iridium or iridium alloy, and the mass percentage of the noble metal in the rare earth element-doped carbon nitride-supported noble metal electrocatalyst is 5-40wt.%.

4. A method for preparing a rare earth element-doped carbon nitride-supported noble metal electrocatalyst according to any one of claims 1 to 3, characterized in that: The steps include: The rare earth element-doped carbon nitride and the noble metal source are dissolved in a mixed solution of an organic solvent and water, mixed and heated for reaction, and after the reaction is completed, washed, centrifuged and dried to obtain a rare earth element-doped carbon nitride loaded with noble metal electrocatalyst; Alternatively, rare earth element-doped carbon nitride and a noble metal source are dissolved in a mixed solution of an organic solvent and water, mixed and evaporated to obtain a precursor material; the obtained precursor material is thermally reduced in a reducing atmosphere to obtain a rare earth element-doped carbon nitride loaded with a noble metal electrocatalyst.

5. The method for preparing a rare earth element-doped carbon nitride-supported noble metal electrocatalyst according to claim 4, characterized in that: The method for preparing the rare earth element-doped carbon nitride comprises the following steps: The carbon nitride precursor and the rare earth salt are mixed, and heat treated at 400-650°C for 2-5h in an air atmosphere with a heating rate of 2-10°C / min; after the heat treatment, the obtained product is washed and dried to obtain rare earth element-doped carbon nitride.

6. The method for preparing a rare earth element-doped carbon nitride-supported noble metal electrocatalyst according to claim 5, characterized in that: The carbon nitride precursor is selected from one or more of cyanamide, ammonium thiocyanate, dicyandiamide, melamine, thiourea or urea; The rare earth salt is one of lanthanum salt, cerium salt, praseodymium salt, neodymium salt, promethium salt, samarium salt, europium salt, gadolinium salt, terbium salt, dysprosium salt, holmium salt, erbium salt, thulium salt, ytterbium salt, lutetium salt, scandium salt or yttrium salt; The mass ratio of the carbon nitride precursor to the rare earth salt is (8-11):

1.

7. The method for preparing a rare earth element-doped carbon nitride-supported noble metal electrocatalyst according to claim 4, characterized in that: The noble metal source is any one or more of platinum salt, palladium salt or iridium salt.

8. The method for preparing a rare earth element-doped carbon nitride-supported noble metal electrocatalyst according to claim 4, characterized in that: In the mixed solution of the organic solvent and water, the organic solvent is alcohol or N,N-dimethylformamide, and the volume ratio of the alcohol or N,N-dimethylformamide to water is (1-3):(3-5).

9. The method for preparing a rare earth element-doped carbon nitride-supported noble metal electrocatalyst according to claim 4, wherein the heating reaction has a reaction temperature of 60-160° C. and a reaction time of 3-7 h; Alternatively, thermal reduction is performed at 200-600°C.

10. Use of a rare earth element-doped carbon nitride-supported noble metal electrocatalyst as claimed in any one of claims 1 to 3 or a rare earth element-doped carbon nitride-supported noble metal electrocatalyst prepared by the preparation method as claimed in any one of claims 4 to 9 in a hydrogen fuel cell.

Citation Information

Cited By

  • Rare earth doped Pt-based high-entropy intermetallic compound, preparation and application

    CN119601693A

  • Nitrogen-doped alloy catalyst as well as preparation method and application thereof

    CN119674111A

  • Halogen ion intercalated spinel-graphite phase carbon nitride heterojunction catalyst as well as preparation method and application thereof

    CN121103404A

  • Visible light catalyst capable of efficiently producing hydrogen peroxide and preparation method of visible light catalyst