Polyurethane adhesive composition and use thereof

Through the combination of phosphate modified polyol and vegetable oil modified polyol in the two-component polyurethane adhesive composition with NCO-terminated polyurethane prepolymer, the problems of aluminum alloy substrate bonding and moisture absorption are solved, and the battery pack is improved. Adhesion strength and production stability.

CN118829673APending Publication Date: 2024-10-22DOW GLOBAL TECHNOLOGIES LLC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280092251.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2022-03-25
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

Existing polyurethane adhesives are difficult to effectively combine with aluminum alloy substrates in battery assembly, and they easily absorb moisture, leading to the formation of solid skin and reduced NCO content, affecting the reaction feed ratio and production stability.

Method used

A two-component polyurethane adhesive composition is used, including a phosphate-modified polyol and a vegetable oil-modified polyol and an NCO-terminated polyurethane prepolymer. By controlling the mixing ratio and additive combination, a reactive liquid intermediate is formed to improve Bond strength and moisture resistance.

Benefits of technology

It achieves good adhesion to the aluminum alloy substrate, reduces moisture absorption and solid skin formation, improves the stability of the reaction feed ratio and bonding strength, and ensures the production continuity and quality of the battery pack.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005003149320000041
    Figure BDA0005003149320000041
  • Figure BDA0005003149320000042
    Figure BDA0005003149320000042
  • Figure BDA0005003149320000111
    Figure BDA0005003149320000111
Patent Text Reader

Abstract

There is provided a polyurethane adhesive composition comprising (a) a polyol component comprising a phosphate-modified polyol and a vegetable oil-modified polyol, and (b) an isocyanate component comprising an NCO-terminated polyurethane prepolymer, the NCO-terminated polyurethane prepolymer comprising a polyol component comprising a phosphate-modified polyol and a vegetable oil-modified polyol, and the polyol component comprising an NCO-terminated polyurethane prepolymer, the polyol component comprising an NCO-terminated polyurethane prepolymer, the vegetable oil-modified polyol comprising an NCO-terminated polyurethane prepolymer, and the isocyanate component comprising an NCO-terminated polyurethane prepolymer. The polyurethane prepolymer is the reaction product of (i) a polyester polyol based on a dimer acid and an aromatic dicarboxylic acid and (ii) an isocyanate monomer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to an adhesive composition, and more particularly to a two-component polyurethane adhesive composition. Background Art

[0002] The ability to mass produce battery packs in an economical manner has been revolutionary over the past few years and has driven the adoption of electric vehicles (EVs) around the world. Due to their low cost, low volatility, high bulk strength and toughness, polyurethane adhesives have become a popular solution for battery pack assembly, where the battery cells are bonded to the cooling plate.

[0003] The bonding substrates used for battery pack assembly mainly include aluminum alloys, PET films, polycarbonates, etc., among which Al alloy-Al alloy bonding is the most important one. However, due to the high surface energy and the absence of organic chemical groups on the surface of Al alloys, effective bonding between Al alloys is difficult. On the other hand, the moisture resistance of polyurethane components (including polyol parts and isocyanate parts) is another important industrial need. This is because both the polyol part and the isocyanate part can easily absorb moisture. For the isocyanate part, the absorbed moisture causes a decrease in the NCO content and the formation of a solid skin starting from the top of the component. Therefore, the reduced NCO content will make the feed ratio between the reaction groups incorrect, and the thick skin will usually block the storage tank and / or the distribution channel, causing product defects and production interruptions, respectively. For the polyol part, after mixing and distributing the polyol part with the isocyanate part, the absorbed moisture may bring significant bubbles to the cured adhesive.

[0004] Therefore, there remains a need for polyurethane adhesive compositions that provide good moisture resistance, bond strength, and cost effectiveness. Summary of the invention

[0005] In one aspect, the present disclosure provides a polyurethane adhesive composition, comprising:

[0006] (a) a polyol component comprising a phosphate-modified polyol and a vegetable oil-modified polyol, and

[0007] (b) an isocyanate component comprising an NCO-terminated polyurethane prepolymer which is the reaction product of (i) a polyester polyol based on a dimer acid and an aromatic dicarboxylic acid and (ii) an isocyanate monomer.

[0008] In a further aspect, the present disclosure provides an isocyanate agent for use in a polyurethane adhesive composition, the isocyanate agent comprising an NCO-terminated polyurethane prepolymer, the NCO-terminated polyurethane prepolymer being the reaction product of (i) a polyester polyol based on a dimer acid and an aromatic dicarboxylic acid and (ii) an isocyanate monomer.

[0009] In a further aspect, the present disclosure provides a method of using the polyurethane adhesive composition described herein, the method comprising:

[0010] (a) providing a polyurethane adhesive composition as described herein, wherein a polyol component and an isocyanate component are provided separately from each other;

[0011] (b) contacting a polyol component with an isocyanate component to form a curable mixture;

[0012] (c) applying the curable mixture to a first substrate to which at least a second substrate will be bonded;

[0013] (d) contacting a second substrate with the first substrate such that at least a portion of the curable mixture is sandwiched between the first substrate and the second substrate; and

[0014] (e) curing the curable mixture, or causing it to cure.

[0015] In a further aspect, the present disclosure provides use of the polyurethane adhesive composition described herein in a battery pack.

[0016] It is to be understood that both the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the invention, as claimed. DETAILED DESCRIPTION

[0017] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the invention belongs. In addition, all publications, patent applications, patents, and other references mentioned herein are incorporated by reference.

[0018] As disclosed herein, “and / or” means “and, or as an alternative.” Unless otherwise indicated, all ranges are inclusive.

[0019] As disclosed herein, all percentages referred to herein are by weight and temperatures are in °C unless otherwise stated.

[0020] A. Polyurethane Adhesive Composition

[0021] In one aspect, the present disclosure provides a polyurethane adhesive composition, comprising:

[0022] (a) a polyol component comprising at least one phosphate-modified polyol and at least one vegetable oil-modified polyol, and

[0023] (b) an isocyanate component comprising an NCO-terminated polyurethane prepolymer which is the reaction product of (i) a polyester polyol based on a dimer acid and an aromatic dicarboxylic acid and (ii) an isocyanate monomer.

[0024] The polyurethane adhesive composition described herein is a two-component composition. As used herein, the term "two-component" means that the composition is provided in separate parts before reacting them. For example, the polyol component and the isocyanate component of the composition can be prepared, stored, transported and supplied separately, and soon or immediately combined, for example, in a mixer, to form a reactive mixture. It is expected that when the two components contact, the curing reaction begins, wherein the polyol group reacts with the isocyanate group to form a urethane chain segment. The reactive polyurethane composition formed by contacting the two components can be referred to as a "reactive liquid intermediate" or a "reactive mixture".

[0025] The mixing ratio between the polyol component and the isocyanate component is not strictly limited. In some exemplary embodiments, the isocyanate component and the polyol component may have an NCO / OH molar ratio of 0.9:1 to 1.95:1, such as 1:1 to 1.9:1, or 1.05:1 to 1.85:1. In some exemplary embodiments, the isocyanate component and the polyol component may be combined in a volume ratio of about 1:1, such as 1:1.2 to 1:0.8, 1:1.1 to 1:0.9, or 1:1.05 to 1:0.95.

[0026] Typically, the polyurethane adhesive composition is solvent-free.

[0027] (A) Polyol component

[0028] The polyol component of the polyurethane adhesive composition includes at least one phosphate ester-modified polyol and at least one vegetable oil-modified polyol.

[0029] In addition to the phosphate-modified polyol and the vegetable oil-modified polyol, the polyol component may further comprise one or more additional polyols.

[0030] The polyol component may optionally include one or more additives, such as plasticizers, flame retardants, adhesion promoters, rheology modifiers, fillers, or any combination thereof.

[0031] Typically, the polyol component described herein is solvent-free. As used herein, the term "solvent-free" means that the adhesive composition (e.g., up to 100% solid) can be applied without an organic solvent or an aqueous carrier. In some embodiments of the present disclosure, the adhesive composition comprises less than 4 wt %, less than 3 wt %, less than 2 wt %, less than 1 wt %, less than 0.5 wt %, less than 0.2 wt %, less than 0.1 wt %, less than 100 ppm (by weight), less than 50 ppm (by weight), less than 10 ppm (by weight), less than 1 ppm (by weight) of any organic or inorganic solvent or water, or does not contain any organic or inorganic solvent or water.

[0032] Phosphate modified polyols

[0033] At least one phosphate-modified polyol (eg, phosphate ester polyol) is included in the polyol component.

[0034] Typically, the at least one phosphate-modified polyol can function as an adhesion promoter in the polyol component.

[0035] As used herein, "phosphate-modified polyol" refers to a compound having two or more hydroxyl groups and one or more structures (I):

[0036]

[0037] Included in Structure I are structures in which one or more of the acidic hydrogen atoms have been abstracted. An acidic hydrogen atom is a hydrogen atom attached to an oxygen atom that is attached to a phosphorus atom. When one or more acidic hydrogens are abstracted, the phosphate group is an anion.

[0038] In some embodiments, the polyol component may include one or more phosphate-modified polyols represented by structure (II):

[0039]

[0040] Where R 1 Is a trivalent group, such as C1-C 16 (For example, C1-C 10 , C1-C8 or C1-C6) trivalent groups (e.g., C1-C 16 A and B are each independently a direct bond or a divalent group, such as C1-C 16 (For example, C1-C 10 , C1-C8 or C1-C6) divalent group (e.g., C1-C 16 alkylene), provided that A and B are not both direct bonds. In addition to the side groups shown in structure (II), R1 , A and B each independently may or may not have one or more additional -OH side groups, and R 1 , A and B each independently may or may not have one or more additional side groups of structure (I). Any two or more of the -OH group and the group of structure (I) may or may not be attached to R 1 Preferably, each -OH group and each group of structure (I) is connected to R 1 , A and B. In some embodiments, the phosphate-modified polyol is a polyether-based polyol. In some embodiments, the phosphate-modified polyol is a polyether-based polyurethane polyol.

[0041] Phosphate ester polyols can be prepared from trifunctional propylene glycol, polyphosphoric acid, and polyisocyanate. Commercially available examples of trifunctional propylene glycol suitable for use according to the present disclosure include polyisocyanate sold under the trade name VORANOL TM CP-450, VORANOL TM CP-260, VORANOL TM CP-755 and VORANOL TM CP-1055 is a product sold, each of which can be obtained from The Dow Chemical Company. In some embodiments, the phosphoric acid content of the phosphate polyol is less than 4% by weight based on the weight of the phosphate polyol, or 0% to 3% by weight based on the weight of the phosphate polyol, or 1.5% to 2.5% by weight based on the weight of the phosphate polyol. In some embodiments, the phosphate polyol has a viscosity of less than 40,000 cps at 25°C or less than 30,000 cps at 25°C, as measured by the method of ASTM D2196. In some embodiments, the phosphate polyol has a hydroxyl equivalent of less than 330 g / mol. In some embodiments, the phosphate polyol has a trifunctional polyether polyol with an equivalent weight of less than 2,000 g / mol from 0% to 100% by weight based on the weight of the phosphate polyol.

[0042] In some embodiments, the polyol component comprises 1% to 50%, eg, 2% to 40%, 3% to 30%, 3% to 15%, or 3% to 10%, by weight of the polyol component, of the phosphate-modified polyol.

[0043] In some embodiments, at least one phosphate-modified polyol contained in the polyol component has an average number of hydroxyl groups of not less than 80 mg KOH / g. In some embodiments, at least one phosphate-modified polyol contained in the polyol component has an average number of hydroxyl groups of no more than 800 mg KOH / g. In some embodiments, at least one phosphate-modified polyol contained in the polyol component has an average number of hydroxyl groups within a numerical range obtained by combining any two of the following endpoints: 80 mg KOH / g, 100 mg KOH / g, 150 mg KOH / g, 200 mg KOH / g, 300 mg KOH / g, 400 mg KOH / g, 500 mg KOH / g, 600 mg KOH / g, 700 mg KOH / g, 800 mg KOH / g. In some embodiments, the at least one phosphate-modified polyol included in the polyol component has an average number of hydroxyl groups of 80 to 800 mg KOH / g, 100 to 600 mg KOH / g, 150 to 500 mg KOH / g, or 200 to 400 mg KOH / g.

[0044] Vegetable oil modified polyols

[0045] At least one vegetable oil-modified polyol is included in the polyol component.

[0046] Typically, at least one vegetable oil-modified polyol can function as a hydrophobicity-imparting agent in the polyol component.

[0047] As used herein, "vegetable oil modified polyol" refers to a polyether polyol based on a vegetable oil, a polyester polyol based on a vegetable oil, a polyurethane polyol based on a vegetable oil, or a mixture thereof having an average hydroxyl group functionality of not less than 2. In a preferred embodiment, the polyol modified by a vegetable oil comprises a polyurethane polyol and a short-chain polyether polyol (such as Voranol CP 450). In an exemplary embodiment, the polyol modified by a vegetable oil does not include a polyolefin polyol (such as a polybutadiene polyol). Suitable polyester polyols for use include, but are not limited to, diols and optionally polyols (e.g., triols, tetraols) and dicarboxylic acids and optionally polycarboxylic acids (e.g., tricarboxylic acids, tetracarboxylic acids) or hydroxycarboxylic acids or lactones. Polyurethane polyols can be synthesized using isocyanates as chain extenders and hydroxyl groups as end groups. In some embodiments, the polyol modified by a vegetable oil comprises a polyol modified by castor oil. In some embodiments, the polyol modified by a vegetable oil comprises a polyurethane polyol modified by castor oil.

[0048] The polyol component comprises from 1% to 99%, e.g., from 2% to 90%, from 3% to 80%, from 5% to 30%, from 5% to 20%, or from 5% to 10%, by weight of the polyol component, of a vegetable oil-modified polyol.

[0049] Additional polyols

[0050] In addition to the described phosphate-modified polyols and vegetable oil-modified polyols, the polyol component may further comprise one or more additional polyols, for example one or more selected from polyester polyols, polyether polyols, polyetherester polyols, polycarbonate polyols, polyurethane polyols, and combinations thereof.

[0051] In some embodiments, the polyol component includes one or more polyether polyols. In some embodiments, the one or more polyether polyols included in the polyol component have an average hydroxyl group number of not less than 80 mg KOH / g. In some embodiments, the one or more polyether polyols included in the polyol component have an average hydroxyl group number of no more than 800 mg KOH / g. In some embodiments, the one or more polyether polyols included in the polyol component have an average hydroxyl group number within a numerical range obtained by combining any two of the following endpoints: 80 mg KOH / g, 100 mg KOH / g, 150 mg KOH / g, 200 mg KOH / g, 300 mg KOH / g, 400 mg KOH / g, 500 mg KOH / g, 600 mg KOH / g, 700 mg KOH / g, 800 mg KOH / g. In some embodiments, the one or more polyether polyols included in the polyol component have an average number of hydroxyl groups of 80 to 800, 100 to 600, 150 to 500, or 200 to 400 mg KOH / g.

[0052] In some embodiments, the one or more additional polyols included in the polyol component have an average hydroxyl group functionality of no more than 4. In some embodiments, the one or more additional polyols included in the polyol component have an average hydroxyl group functionality of no less than 2. In some embodiments, the one or more additional polyols in the polyol component have an average hydroxyl group functionality within the range of values ​​obtained by combining any two of the following endpoints: 2, 2.5, 3, 3.5, and 4. In some embodiments, the additional polyols have an average hydroxyl group functionality of 2 to 4 or 2 to 3.

[0053] In some embodiments, the additional polyol comprises one or more hydrophobic polyols, such as castor oil.

[0054] Optional additional additives

[0055] The polyol component may optionally contain one or more additional agents that serve a particular function or purpose.

[0056] For example, one or more additional agents selected from the group consisting of chain extenders (eg, short chain diols), moisture scavengers, catalysts, flame retardants, rheology modifiers, fillers, additional adhesion promoters, and any combination thereof may be further included in the polyol component.

[0057] In some embodiments, the polyol component may include one or more chain extenders (e.g., short chain glycols) or crosslinkers. Chain extenders or crosslinkers refer to small molecular weight alcohols with a hydroxyl functionality ≥ 2. Examples are 1,2-methylene glycol, 1,4-butanediol, glycerol, etc. In an exemplary embodiment, the polyol component may include 0% to 10% chain extenders by weight of the polyol component.

[0058] In some embodiments, the polyol component may include one or more moisture scavengers. Moisture scavengers absorb moisture from the environment before they react with NCO-containing groups in the adhesive, thereby helping to solve the bubble formation problem. Common moisture scavengers in polyurethane adhesives are molecular sieves. In an exemplary embodiment, the polyol component may include 0% to 10% moisture scavenger by weight of the polyol component.

[0059] In some embodiments, the polyol component may include one or more catalysts to adjust the reaction kinetics to meet process requirements. Loading more catalyst helps to establish initial bond strength, but shortens the pot life. A well-balanced catalyst package is an organometallic catalyst, including a catalyst containing Zn, Bi and Sn. In an exemplary embodiment, the polyol component may include 0% to 3% catalyst by weight of the polyol component.

[0060] In some embodiments, the polyol component may include one or more flame retardants. The flame retardant can help improve the fire resistance of the battery cell when exposed to an electrical short circuit. In an exemplary embodiment, the polyol component may include 0% to 20% flame retardant by weight of the polyol component.

[0061] In some embodiments, the polyol component may include one or more rheology modifiers. Rheology modifiers are often included in adhesive formulations to provide thixotropic properties required for different applications. Rheology modification can be provided by physical association, such as fumed silica, or chemical reaction, such as amines and NCO. In an exemplary embodiment, the polyol component may include 0% to 10% rheology modifier by weight of the polyol component.

[0062] In some embodiments, the polyol component may include one or more fillers. Fillers are added to the adhesive to provide lower cost, thermal conductivity, etc. They can be selected from silica, calcium carbonate, kaolin, talc, aluminum hydroxide, aluminum oxide, boron nitride, etc. with or without surface modification. In an exemplary embodiment, the polyol component may include 0% to 95% filler by weight of the polyol component.

[0063] In some embodiments, the polyol component may include one or more additional adhesion promoters. Additional adhesion promoters are those adhesion promoters other than the phosphate-modified polyols described herein. In an exemplary embodiment, the polyol component may include 0% to 10% of the additional adhesion promoter by weight of the polyol component.

[0064] (B) Isocyanate component

[0065] The isocyanate component of the polyurethane adhesive composition comprises an NCO-terminated polyurethane prepolymer which is the reaction product of (i) a polyester polyol based on dimer acid and aromatic dicarboxylic acid ("DADPP") and (ii) an isocyanate monomer.

[0066] As used herein, "dimer acid and aromatic dicarboxylic acid based polyester polyol," "dimer acid and aromatic dicarboxylic acid based polyester polyol," or "DADPP" refers to a polyester polyol derived from (e.g., prepared from) a reactive mixture of at least one dimer acid, at least one aromatic dicarboxylic acid, and at least one polyol.

[0067] When "dimer acid" is mentioned herein, derivatives of dimer acid are also included, such as compounds produced by replacing hydrogen atoms in dimer acid molecules with another atom or atomic group (such as halogen or amino group), including halides, anhydrides, esters, salts, amides, etc. of dimer acid. Similarly, when "aromatic dicarboxylic acid" is mentioned herein, derivatives of aromatic dicarboxylic acid are also included, such as compounds produced by replacing hydrogen atoms in aromatic dicarboxylic acid molecules with another atom or atomic group (such as halogen or amino group), including halides, anhydrides, esters, salts, amides, etc. of aromatic dicarboxylic acid.

[0068] Typically, the isocyanate components described herein are solvent-free.

[0069] The isocyanate component may optionally include one or more additives such as plasticizers, flame retardants, adhesion promoters, rheology modifiers, fillers, or any combination thereof.

[0070] NCO-terminated polyurethane prepolymer

[0071] The NCO-terminated polyurethane prepolymer included in the isocyanate component is the reaction product of at least one polyester polyol and at least one isocyanate monomer, wherein the at least one polyester polyol comprises DADPP as described herein.

[0072] Typically, the NCO terminated polyurethane prepolymer is prepared by using 35 to 95 weight percent isocyanate and 5 to 65 weight percent DADPP, based on the weight of the reactive mixture.

[0073] The polyol used to prepare the NCO-terminated polyurethane prepolymer preferably does not contain a phosphorus-containing polyol, because the present inventors have found that the inclusion of a phosphorus-containing polyol may impair its hydrophobicity by increasing the moisture sensitivity of the isocyanate side.

[0074] The isocyanate component comprises 5% to 100% of the NCO-terminated polyurethane prepolymer, based on the weight of the isocyanate component. For example, the content of the NCO-terminated polyurethane prepolymer in the isocyanate component is within the range obtained by combining any two of the following endpoints: 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, 97%, 98%, 99% and 100%. In some embodiments, the isocyanate component comprises from 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, or 45% to 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, 97%, 98%, 99% or 100% NCO terminated polyurethane prepolymer by weight of the isocyanate component.

[0075] It should be understood that the NCO terminated polyurethane prepolymer is an intermediate between the monomer and the final polymer.

[0076] DADPP

[0077] The DADPP useful for preparing the NCO-terminated polyurethane prepolymer is prepared from a reactive mixture of at least one dimer acid, at least one aromatic dicarboxylic acid, and at least one polyol.

[0078] The present inventors have found that polyester polyols based on dimer acids can provide low viscosity and, more importantly, hydrophobicity to the isocyanate component. In addition, incorporation of aromatic dicarboxylic acids can not only reduce costs, but also improve bond strength to the polyester polyol. In this regard, it is not desirable to include aliphatic dicarboxylic acids due to the poor hydrophobicity and bond strength that may result. For example, DADPP is not prepared from any adipic acid due to the non-hydrophobicity of adipic acid.

[0079] DADPP is generally a condensation product of diols and optionally polyols (e.g., triols, tetraols), and is a condensation product of dimer acid and aromatic dicarboxylic acid or its derivatives. The hydroxyl groups of DADPP will further react with isocyanates to produce polyurethane prepolymers.

[0080] In some embodiments, DADPP is prepared via a one-step process where all acid and alcohol are charged in one pot and reacted in one step.

[0081] In some embodiments, the weight ratio of aromatic dicarboxylic acid to dimer acid is >0 and <4.2. In some embodiments, the weight ratio of aromatic dicarboxylic acid to dimer acid is >0 and <3. In some embodiments, the weight ratio of aromatic dicarboxylic acid to dimer acid is >0 and <2.5. In some embodiments, the weight ratio of aromatic dicarboxylic acid to dimer acid is >0 and <2.0. In some embodiments, the weight ratio of aromatic dicarboxylic acid to dimer acid is >0 and <1.5. In some embodiments, the weight ratio of aromatic dicarboxylic acid to dimer acid is >0 and <1. In some embodiments, the weight ratio of aromatic dicarboxylic acid to dimer acid is >0 and <0.6.

[0082] Dimer acid

[0083] The "dimer acid" that can be used to prepare DADPP can be a dicarboxylic acid compound obtained by reacting a fatty acid having one, two, three or four olefinic double bonds and 14 to 22 (e.g., 16 to 20) carbon atoms (hereinafter referred to as "unsaturated fatty acid A") with a fatty acid having one, two, three or four olefinic double bonds and 14 to 22 (e.g., 16 to 20) carbon atoms (hereinafter referred to as "unsaturated fatty acid B") at a double bond in a dimerization reaction. In one embodiment, the unsaturated fatty acid A has two olefinic double bonds and 14 to 22 (e.g., 16 to 20) carbon atoms, and the unsaturated fatty acid B has one or two olefinic double bonds and 14 to 22 (e.g., 16 to 20) carbon atoms. The non-limiting examples of suitable unsaturated fatty acids A include tetradecadienoic acid, hexadecadienoic acid, octadecadienoic acid (such as linoleic acid), eicosadienoic acid, docosadienoic acid, octadecatrienoic acid (such as linolenic acid), eicosatetraenoic acid (such as arachidonic acid) and combinations thereof. The non-limiting examples of suitable unsaturated fatty acids B include the above examples, as well as tetradecenoic acid (crude oleic acid, spermaceti acid, myristoleic acid), hexadecenoic acid (such as palmitoleic acid), octadecenoic acid (such as oleic acid, elaidic acid and vaccenic acid), eicosenoic acid (such as gadoleic acid) and docosenoic acid (such as erucic acid, setoleic acid and brassene acid) and combinations thereof.

[0084] The obtained dimer acid may be a mixture of dimer acids whose structures differ depending on the bonding site or isomerization of the double bond.

[0085] In some embodiments, the dimer acid useful for preparing the NCO-terminated polyurethane prepolymer may be selected from the group consisting of an acyclic dimer acid, a cyclic dimer acid, an aromatic dimer acid, a polycyclic dimer acid, and any combination thereof.

[0086] For example, an acyclic dimer acid may be represented by structure (A) or (B):

[0087]

[0088] The cyclic dimer acid can be represented by the structure (C):

[0089]

[0090] Aromatic dimer acids can be represented by structure (D):

[0091]

[0092] The polycyclic dimer acid can be represented by the structure (E):

[0093]

[0094] In some embodiments, the dimer acid can be a C36 dimer acid. In other embodiments, the C36 dimer acid has structure (A).

[0095] In one embodiment, the dimer acid is unsaturated. An "unsaturated dimer acid" includes at least one carbon-carbon double bond. For example, structure (A) is an unsaturated dimer acid. A non-limiting example of a suitable dimer acid is ATUREX-1001 (CAS 61788-89-4), available from Aturex Group.

[0096] In one embodiment, the dimer acid has an acid value of from 150 mg KOH / g, or 160 mg KOH / g, or 170 mg KOH / g, or 180 mg KOH / g, or 190 mg KOH / g, or 194 mg KOH / g to 200 mg KOH / g, or 210 mg KOH / g, or 220 mg KOH / g, or 230 mg KOH / g, or 240 mg KOH / g, or 250 mg KOH / g. In another embodiment, the dimer acid has an acid value of from 150 mg KOH / g to 250 mg KOH / g, or from 180 mg KOH / g to 220 mg KOH / g, or from 190 mg KOH / g to 200 mg KOH / g.

[0097] In one embodiment, the dimer acid has structure (A) and has an acid value of 150 to 250 mg KOH / g, or 180 to 220 mg KOH / g, or 190 to 200 mg KOH / g.

[0098] In some embodiments, the DADPP comprises 5% to 80%, eg, 10% to 75%, 15% to 70%, or 20% to 65%, of at least one dimer acid, based on the weight of the DADPP.

[0099] In some embodiments, the NCO-terminated polyurethane prepolymer comprises from 1% to 20%, eg, from 2% to 18%, from 3% to 17%, or from 3% to 15%, by weight of the prepolymer, of at least one dimer acid.

[0100] Aromatic dicarboxylic acids

[0101] The aromatic dicarboxylic acid that can be used to prepare DADPP is not a dimer acid as described above. In other words, the aromatic dicarboxylic acid is structurally different and / or compositionally different from the dimer acid in the reaction mixture.

[0102] In some embodiments, the aromatic dicarboxylic acid comprises a carboxyl group directly attached to an aromatic ring. In some embodiments, the aromatic dicarboxylic acid does not comprise an olefinic bond.

[0103] In some embodiments, the aromatic dicarboxylic acid can be selected from the group consisting of phthalic acid, isophthalic acid, terephthalic acid, and any combination thereof. In some embodiments, the aromatic dicarboxylic acid comprises isophthalic acid.

[0104] In some embodiments, the DADPP comprises 5% to 80%, eg, 10% to 70%, 12% to 60%, or 15% to 55%, of at least one aromatic dicarboxylic acid, based on the weight of the DADPP.

[0105] In some embodiments, the NCO terminated polyurethane prepolymer comprises from 0.5% to 20%, eg, from 1% to 18%, from 2% to 15%, or from 3% to 12%, by weight of the prepolymer, of at least one aromatic dicarboxylic acid.

[0106] Polyols

[0107] The polyol that can be used to prepare DADPP can be selected from the group consisting of diols, triols, tetraols, and combinations thereof.

[0108] As used herein, the term "polyol" refers to a compound having two or more hydroxyl groups. When a polyol has exactly two hydroxyl groups, it is a "diol," when it has exactly three hydroxyl groups, it is a "triol," when it has exactly four hydroxyl groups, it is a "tetraol," when it has exactly five hydroxyl groups, it is a "pentanol," and so on.

[0109] Non-limiting examples of suitable diols include 3-methyl 1,5-pentanediol (MPD); 2-methyl-1,3-propanediol (MPG); ethylene glycol; butanediol; diethylene glycol (DEG); triethylene glycol; polyalkylene glycols, such as polyethylene glycol and polypropylene glycol; 1,2-propylene glycol; 1,3-propylene glycol; 1,3-butanediol; 1,4-butanediol; 1,6-hexanediol; and neopentyl glycol (NPG). In some embodiments, the polyol includes a diol. In other embodiments, the diol includes MPG and / or 1,6-hexanediol.

[0110] A non-limiting example of a suitable triol is trimethylolpropane (TMP).

[0111] In some embodiments, the one or more polyols used to prepare DADPP have an average hydroxyl group functionality of no more than 4. In some embodiments, the one or more polyols used to prepare DADPP have an average hydroxyl group functionality of no less than 2. In some embodiments, the one or more polyols used to prepare DADPP have an average hydroxyl group functionality within the range of values ​​obtained by combining any two of the following endpoints: 2, 2.5, 3, 3.5, and 4. In some embodiments, the one or more polyols used to prepare DADPP have an average hydroxyl group functionality of 2 to 4, for example, 2 to 3.

[0112] Isocyanate monomer

[0113] Isocyanate monomers useful in preparing the NCO-terminated polyurethane prepolymer may include various unmodified or modified monomeric isocyanates.

[0114] As used herein, an "isocyanate monomer" or "monomeric isocyanate" is any compound containing two or more isocyanate groups.

[0115] Compounds having isocyanate groups, such as isocyanate monomers, can be characterized by the parameter "% NCO" or "-NCO content", which is the amount of isocyanate groups by weight of the compound. In some embodiments, the isocyanate monomer has a free -NCO content of between 15% and 40%, e.g., between 18% and 35%, by weight of the isocyanate monomer.

[0116] Examples of monomeric aromatic isocyanates suitable for use in accordance with the present disclosure include, but are not limited to, isomers of methylene diphenyl diisocyanate ("MDI") such as 4,4-MDI, 2,4-MDI and 2,2'-MDI, or modified MDI such as carbodiimide-modified MDI or allophanate-modified MDI; isomers of toluene diisocyanate ("TDI") such as 2,4-TDI, 2,6-TDI, naphthalene diisocyanate ("N-TDI") and 2,6-T ... DI") such as 1,5-NDI, m- and p-phenylene diisocyanate, chlorophenylene-2,4-diisocyanate, diphenylene-4,4'-diisocyanate, 3,3'-dimethyl-4,4'-diphenyl-diisocyanate, 3-methyldiphenyl-methane-4,4'-diisocyanate, diphenyl ether diisocyanate, 2,4,6-triisocyanate toluene, 2,4,4'-triisocyanate diphenyl ether, and combinations thereof.

[0117] In some embodiments, the isocyanate monomer may be selected from the group consisting of MDI, TDI, IPDI, HMDI, and any combination thereof. In some embodiments, MDI is included for better mechanical properties. Types of MDI include linear MDI, such as 4,4'-MDI, 2,2'-MDI, carbodiimide-modified MDI, and mixtures thereof. Polymeric MDI can also be used to adjust mechanical properties, but is not preferred because it is found to be more sensitive to moisture (e.g., compared to carbodiimide-containing isocyanates).

[0118] In some embodiments, one or more of the included isocyanate monomers are carbodiimide-modified. In some embodiments, the isocyanate monomers include carbodiimide-modified MDI.

[0119] Optional additional additives

[0120] The isocyanate component may optionally contain one or more additional agents for a particular function or purpose.

[0121] For example, one or more additional agents selected from the group consisting of plasticizers, flame retardants, other adhesion promoters, rheology modifiers, fillers, and any combination thereof may be further included in the isocyanate component.

[0122] In some embodiments, the isocyanate component may include one or more plasticizers to reduce skinning that builds up during application of the isocyanate component. In an exemplary embodiment, the isocyanate component may include 0% to 20% plasticizer by weight of the isocyanate component.

[0123] In some embodiments, the isocyanate component may include one or more flame retardants to improve fire resistance. In an exemplary embodiment, the isocyanate component may include 0% to 20% of the flame retardant, based on the weight of the isocyanate component.

[0124] In some embodiments where the isocyanate component is used as the isocyanate component in the polyurethane adhesive composition, the isocyanate component may include one or more adhesion promoters to increase adhesion between substrates. In an exemplary embodiment, the isocyanate component may include 0% to 10% of other adhesion promoters by weight of the isocyanate component. In embodiments where the isocyanate component is used as the isocyanate component in the polyurethane adhesive composition as described herein, the adhesion promoter included in the isocyanate component is different from the phosphate-modified polyol as described herein.

[0125] In some embodiments, the isocyanate component may include one or more rheology modifiers to provide thixotropic properties required for different applications. Rheology modification can be provided by physical association, such as fumed silica, or chemical reaction, such as amine and NCO. In an exemplary embodiment, fumed silica with a hydrophobic surface treatment can be used as a rheology modifier in the isocyanate component. In an exemplary embodiment, the isocyanate component can include 0% to 10% of the rheology modifier by weight of the isocyanate component.

[0126] In some embodiments, the isocyanate component may include one or more fillers to further reduce cost, thermal conductivity, etc. The filler may be selected from silica, calcium carbonate, kaolin, talc, aluminum hydroxide, aluminum oxide, boron nitride, etc. with or without surface modification. In an exemplary embodiment, the isocyanate component may include 0% to 95% filler based on the weight of the isocyanate component.

[0127] B. Isocyanate Reagents

[0128] In one aspect, the present disclosure provides an isocyanate reagent comprising an NCO-terminated polyurethane prepolymer that is the reaction product of (i) a polyester polyol based on dimer acid and aromatic dicarboxylic acid ("DADPP") and (ii) an isocyanate monomer.

[0129] The isocyanate reagent comprises or is one isocyanate component among the isocyanate components, or a mixture of isocyanate components, as described above in the "(B) Isocyanate Component" section, and is prepared, packaged, stored, and transported as an independent product.

[0130] In some embodiments, an isocyanate reagent is used in a polyurethane adhesive composition. For example, an isocyanate reagent can be used as an isocyanate component in a polyurethane adhesive composition according to the present disclosure, which can be mixed and reacted with a polyol component to produce a polyurethane adhesive.

[0131] C. Application of polyurethane adhesive composition

[0132] In a further aspect, the present disclosure provides a method of using the polyurethane adhesive composition as described herein, the method comprising:

[0133] (a) providing a polyurethane adhesive composition comprising the described polyol component and isocyanate component;

[0134] (b) contacting a polyol component with an isocyanate component to form a curable mixture;

[0135] (c) applying the curable mixture to a first substrate to which at least a second substrate will be bonded;

[0136] (d) contacting a second substrate with the first substrate such that at least a portion of the curable mixture is sandwiched between the first substrate and the second substrate; and

[0137] (e) curing the curable mixture, or causing it to cure.

[0138] In some embodiments, the curable mixture can be cured at room temperature (about 25° C.) for several days (e.g., 3 to 10 days). In some embodiments, the curable mixture can be subjected to pressure or heat (e.g., at a temperature of 30° C. to 90° C., such as 30° C. to 60° C.) to accelerate curing.

[0139] The material or type of the substrates (eg, first and second substrates) to be treated with the polyurethane adhesive composition is not limited. In an exemplary embodiment, the first substrate may be one or more battery cells, and the second substrate may be a cooling plate.

[0140] In a further aspect, the present application provides use of the described polyurethane adhesive composition in a battery pack.

[0141] Example

[0142] Some embodiments of the present invention will now be described in the following examples, in which all parts and percentages are by weight unless otherwise indicated.

[0143] raw materials

[0144] Table 1. Raw materials used in this ICD

[0145]

[0146]

[0147]

[0148] Synthesis process

[0149] Synthesis of Dimer Acid-Based Polyester Polyol-1 (DA-1):

[0150] 100g 1,6-hexanediol, 353g ATUREX-1001 were loaded into a 500ml glass reactor and mixed thoroughly. The mixture was heated to 100°C. When the raw materials were converted into liquids, stirring was started. The temperature was controlled at an appropriate location and monitored throughout the process. If the top temperature of the glass condenser rises to above 103°C, the cooling of the reactor was started as quickly as possible. When the reaction temperature rises to 220°C and the top temperature drops below 100°C, vacuum is slowly applied to 30mm Hg within 30 minutes. The acid value was checked every 30 minutes. A certain amount of catalyst Tyzor TBT was added until the acid value of the reaction system was less than 10. The catalyst was added and the reaction system was kept under 30mm Hg vacuum for more than 1 hour until the OH value reached the theoretical value. The temperature was cooled to 60°C-70°C and the final product as a polyester polyol based on dimer acid was collected.

[0151] Synthesis of Dimer Acid-Based Polyester Polyol-2 (DA-2):

[0152] 100g of 2-methyl-1,3-propanediol and 467.5g of ATUREX-1001 were charged into a 500ml glass reactor and mixed thoroughly. The mixture was heated to 100°C. When the raw materials were converted into liquids, stirring was started. The temperature was controlled at an appropriate location and monitored throughout the process. If the top temperature of the glass condenser rises to above 103°C, the cooling of the reactor was started as quickly as possible. When the reaction temperature rises to 220°C and the top temperature drops below 100°C, vacuum is slowly applied to 30mm Hg within 30 minutes. The acid value was checked every 30 minutes. A certain amount of catalyst Tyzor TBT was added until the acid value of the reaction system was less than 10. The catalyst was added and the reaction system was kept under 30mm Hg vacuum for more than 1 hour until the OH value reached the theoretical value. The temperature was cooled to 60°C-70°C and the final product as a polyester polyol based on dimer acid was collected.

[0153] Synthesis of polyester polyols based on dimer acid / adipic acid (DAAP):

[0154] 100g 2-methyl-1,3-propanediol, 54.3g ATUREX-1001, 129.9g adipic acid were charged into a 500ml glass reactor and mixed thoroughly. The mixture was heated to 100°C. When the raw materials were converted into liquids, stirring was started. The temperature was controlled at an appropriate location and monitored throughout the process. If the top temperature of the glass condenser rises to above 103°C, the cooling of the reactor was started as quickly as possible. When the reaction temperature rises to 220°C and the top temperature drops below 100°C, vacuum is slowly applied to 30mm Hg within 30 minutes. The acid value was checked every 30 minutes. A certain amount of catalyst TyzorTBT was added until the acid value of the reaction system was less than 10. The catalyst was added and the reaction system was kept under 30mm Hg vacuum conditions for more than 1 hour until the OH value reached the theoretical value. The temperature was cooled to 60°C to 70°C, and the final product as a polyester polyol based on dimer acid was collected.

[0155] Synthesis of Dimer Acid / Isophthalic Acid-Based Polyester Polyol-1 (DAIA-1):

[0156] 100g 2-methyl-1,3-propanediol, 36.7g ATUREX-1001, 152.4g isophthalic acid are charged into a 500ml glass reactor and mixed thoroughly. The mixture is heated to 100°C. When the raw materials are converted into liquids, stirring is started. The temperature is controlled at an appropriate location and monitored throughout the process. If the top temperature of the glass condenser rises to above 103°C, the cooling of the reactor is started as quickly as possible. When the reaction temperature rises to 220°C and the top temperature drops below 100°C, vacuum is slowly applied to 30mm Hg within 30 minutes. Check the acid value every 30 minutes. Add a certain amount of catalyst Tyzor TBT until the acid value of the reaction system is less than 10. Add the catalyst and keep the reaction system under 30mm Hg vacuum conditions for more than 1 hour until the OH value reaches the theoretical value. The temperature is cooled to 60°C to 70°C, and the final product as a polyester polyol based on dimer acid is collected.

[0157] Synthesis of Dimer Acid / Isophthalic Acid-Based Polyester Polyol-2 (DAIA-2):

[0158] 100g 2-methyl-1,3-propanediol, 68.2g ATUREX-1001, 141.4g isophthalic acid are charged into a 500ml glass reactor and mixed thoroughly. The mixture is heated to 100°C. When the raw materials are converted into liquids, stirring is started. The temperature is controlled at an appropriate location and monitored throughout the process. If the top temperature of the glass condenser rises to above 103°C, the cooling of the reactor is started as quickly as possible. When the reaction temperature rises to 220°C and the top temperature drops below 100°C, vacuum is slowly applied to 30mm Hg within 30 minutes. Check the acid value every 30 minutes. Add a certain amount of catalyst Tyzor TBT until the acid value of the reaction system is less than 10. Add the catalyst and keep the reaction system under 30mm Hg vacuum conditions for more than 1 hour until the OH value reaches the theoretical value. The temperature is cooled to 60°C to 70°C, and the final product as a polyester polyol based on dimer acid is collected.

[0159] Synthesis of Dimer Acid / Isophthalic Acid-Based Polyester Polyol-3 (DAIA-3):

[0160] 100g 2-methyl-1,3-propanediol, 107.7g ATUREX-1001, 127.6g isophthalic acid are charged into a 500ml glass reactor and mixed thoroughly. The mixture is heated to 100°C. When the raw materials are converted into liquids, stirring is started. The temperature is controlled at an appropriate location and monitored throughout the process. If the top temperature of the glass condenser rises to above 103°C, the cooling of the reactor is started as quickly as possible. When the reaction temperature rises to 220°C and the top temperature drops below 100°C, vacuum is slowly applied to 30mm Hg within 30 minutes. Check the acid value every 30 minutes. Add a certain amount of catalyst Tyzor TBT until the acid value of the reaction system is less than 10. Add the catalyst and keep the reaction system under 30mm Hg vacuum conditions for more than 1 hour until the OH value reaches the theoretical value. The temperature is cooled to 60°C to 70°C, and the final product as a polyester polyol based on dimer acid is collected.

[0161] Synthesis of Dimer Acid / Isophthalic Acid-Based Polyester Polyol-4 (DAIA-4):

[0162] 100g 2-methyl-1,3-propanediol, 175.2g ATUREX-1001, 103.8g isophthalic acid are charged into a 500ml glass reactor and mixed thoroughly. The mixture is heated to 100°C. When the raw materials are converted into liquids, stirring is started. The temperature is controlled at an appropriate location and monitored throughout the process. If the top temperature of the glass condenser rises to above 103°C, the cooling of the reactor is started as quickly as possible. When the reaction temperature rises to 220°C and the top temperature drops below 100°C, vacuum is slowly applied to 30mm Hg within 30 minutes. Check the acid value every 30 minutes. Add a certain amount of catalyst Tyzor TBT until the acid value of the reaction system is less than 10. Add the catalyst and keep the reaction system under 30mm Hg vacuum conditions for more than 1 hour until the OH value reaches the theoretical value. The temperature is cooled to 60°C to 70°C, and the final product as a polyester polyol based on dimer acid is collected.

[0163] Synthesis of Dimer Acid / Isophthalic Acid-Based Polyester Polyol-5 (DAIA-5):

[0164] 100g 2-methyl-1,3-propanediol, 255.4g ATUREX-1001, 75.6g isophthalic acid are charged into a 500ml glass reactor and mixed thoroughly. The mixture is heated to 100°C. When the raw materials are converted into liquids, stirring is started. The temperature is controlled at an appropriate location and the temperature is monitored throughout the process. If the top temperature of the glass condenser rises to above 103°C, the cooling of the reactor is started as quickly as possible. When the reaction temperature rises to 220°C and the top temperature drops below 100°C, vacuum is slowly applied to 30mm Hg within 30 minutes. Check the acid value every 30 minutes. Add a certain amount of catalyst Tyzor TBT until the acid value of the reaction system is less than 10. Add the catalyst and keep the reaction system under 30mm Hg vacuum conditions for more than 1 hour until the OH value reaches the theoretical value. The temperature is cooled to 60°C to 70°C, and the final product as a polyester polyol based on dimer acid is collected.

[0165] Synthesis of castor oil modified polyols (polyurethane polyols):

[0166] Polyurethane polyol was synthesized in a 1,000 ml glass reactor according to the conventional polyurethane prepolymer preparation process. 12 g of ISONATE OP 50 was charged into the reactor and kept at 60° C. under nitrogen protection, and then 44 g of castor oil and 44 g of VORANOL P 400 were charged into the reactor to mix with ISONATE OP 50. The temperature was slowly raised to 80° C. and maintained for 2 hours. Finally, the polyurethane polyol was charged into a well-sealed container with nitrogen protection for further use.

[0167] Synthesis of NCO-terminated prepolymer of DA-1 (Pre-DA1):

[0168] 75g of ISONATE 143L was charged into a 1,000ml glass reactor and kept at 60°C under nitrogen protection, and then 25g of DA-1 was charged into the reactor to mix with ISONATE 143L. The temperature was slowly raised to 80°C and maintained for 2 to 3 hours until the NCO content reached the theoretical value. Finally, the prepolymer was charged into a well-sealed container with nitrogen protection for further application.

[0169] Synthesis of NCO-terminated prepolymer of DA-2 (Pre-DA2):

[0170] 75g of ISONATE 143L was charged into a 1,000ml glass reactor and kept at 60°C under nitrogen protection, and then 25g of DA-2 was charged into the reactor to mix with ISONATE 143L. The temperature was slowly raised to 80°C and maintained for 2 to 3 hours until the NCO content reached the theoretical value. Finally, the prepolymer was charged into a well-sealed container with nitrogen protection for further application.

[0171] Synthesis of NCO-terminated prepolymer of DAAP (Pre-DAAP):

[0172] 75g of ISONATE 143L was charged into a 1,000ml glass reactor and kept at 60°C under nitrogen protection, and then 25g of DAAP was charged into the reactor to mix with ISONATE 143L. The temperature was slowly raised to 80°C and maintained for 2 to 3 hours until the NCO content reached the theoretical value. Finally, the prepolymer was charged into a well-sealed container with nitrogen protection for further application.

[0173] Synthesis of NCO-terminated prepolymer of DAIA-1 (Pre-DAIA1):

[0174] 75g of ISONATE 143L was charged into a 1,000ml glass reactor and kept at 60°C under nitrogen protection, and then 25g of DAIA-1 was charged into the reactor to mix with ISONATE 143L. The temperature was slowly raised to 80°C and maintained for 2 to 3 hours until the NCO content reached the theoretical value. Finally, the prepolymer was charged into a well-sealed container with nitrogen protection for further application.

[0175] Synthesis of NCO-terminated prepolymer of DAIA-2 (Pre-DAIA2):

[0176] 75g of ISONATE 143L was charged into a 1,000ml glass reactor and kept at 60°C under nitrogen protection, and then 25g of DAIA-2 was charged into the reactor to mix with ISONATE 143L. The temperature was slowly raised to 80°C and maintained for 2 to 3 hours until the NCO content reached the theoretical value. Finally, the prepolymer was charged into a well-sealed container with nitrogen protection for further application.

[0177] Synthesis of NCO-terminated prepolymer of DAIA-3 (Pre-DAIA3):

[0178] 75g of ISONATE 143L was charged into a 1,000ml glass reactor and kept at 60°C under nitrogen protection, and then 25g of DAIA-3 was charged into the reactor to mix with ISONATE 143L. The temperature was slowly raised to 80°C and maintained for 2 to 3 hours until the NCO content reached the theoretical value. Finally, the prepolymer was charged into a well-sealed container with nitrogen protection for further application.

[0179] Synthesis of NCO-terminated prepolymer of DAIA-4 (Pre-DAIA4):

[0180] 75g of ISONATE 143L was charged into a 1,000ml glass reactor and kept at 60°C under nitrogen protection, and then 25g of DAIA-4 was charged into the reactor to mix with ISONATE 143L. The temperature was slowly raised to 80°C and maintained for 2 to 3 hours until the NCO content reached the theoretical value. Finally, the prepolymer was charged into a well-sealed container with nitrogen protection for further application.

[0181] Synthesis of NCO-terminated prepolymer of DAIA-5 (Pre-DAIA5):

[0182] 75g of ISONATE 143L was charged into a 1,000ml glass reactor and kept at 60°C under nitrogen protection, and then 25g of DAIA-5 was charged into the reactor to mix with ISONATE 143L. The temperature was slowly raised to 80°C and maintained for 2 to 3 hours until the NCO content reached the theoretical value. Finally, the prepolymer was charged into a well-sealed container with nitrogen protection for further application.

[0183] All prepolymers were successfully synthesized.

[0184] Formulations and Effects

[0185] The isocyanate reagents (used as Part B in the polyurethane adhesive compositions) were formulated as shown in Table 2, all of which met the moisture resistance requirements.

[0186] Table 2. Part B formulations tested (tack-free time ≥ 8.0 h, required)

[0187]

[0188]

[0189] E-01 and E-02 show good hydrophobicity, but their cost is high. In addition, the adhesive strength of E-02 is not satisfactory, as will be described in detail later.

[0190] A comparison was made between E02 to E03 and E04 to E08 and it was found that:

[0191] (1) When the weight ratio of isophthalic acid / dimer acid is >0 and <0.6, the hydrophobicity of the isocyanate moiety is improved.

[0192] (2) When the weight ratio of isophthalic acid / dimer acid is >0.6 and <4.2, the hydrophobicity of the isocyanate moiety deteriorates but is still acceptable.

[0193] (3) When the weight ratio of isophthalic acid / dimer acid is ≥ 4.2, the hydrophobicity of the isocyanate moiety is unacceptable.

[0194] (4) If isophthalic acid is changed to an aliphatic dicarboxylic acid (carbon number ≤ 6), the hydrophobicity of the isocyanate portion is unacceptable even if the dicarboxylic acid / dimer acid ratio is < 4.2.

[0195] A polyurethane adhesive composition was further prepared.

[0196] The adhesive formulations are summarized in Table 3, with details in the corresponding examples of Part A and Part B. Adhesive applicators are mostly obtained with a volume mixing ratio of 1:1. To ensure that the adhesive is fully cured, the stoichiometric ratio of 2K polyurethane adhesives is usually set in the range of 1.05 to 1.85. Therefore, formulations are designed to meet these requirements. The volume mixing ratio and stoichiometric ratio are calculated and listed in Table 3.

[0197] Table 3. Adhesive Examples

[0198]

[0199]

[0200] Note: Com. – comparative example; Inv. – example of the present invention. Lap shear strength ≥ 8.5 MPa and cross tensile strength

[0201] ≥12.5MPa is preferred Com.01-Com.03 as comparative examples show

[0202] (1) Compositions based on pure dimer acid polyester are costly and may impair bond strength (E-02)

[0203] (2) Prepolymers of polyesters based on adipic acid and dimer acid impair the bonding strength (Com.03)

[0204] Comparing Com.04 with Inv.01 to 04, it was found that when the weight ratio of isophthalic acid / dimer acid was ≥ 4.2, the hydrophobicity of the isocyanate portion was unacceptable. In addition, the adhesive strength may be significantly impaired.

[0205] Comparing Com. 01 to 02 with 01 to 04, it was found that the cross tensile strength was greatly increased when the weight ratio of isophthalic acid / dimer acid was <4.2.

[0206] Comparing Com.03 with Inv.01, the weight ratio between the dicarboxylic acid and the dimer acid is the same, however, both the hydrophobicity and the adhesive strength are deteriorated.

[0207] Methods and tests

[0208] Part B isocyanate prepolymer was prepared according to the following procedure:

[0209] Step 1: Place the NCO-terminated prepolymer into a container; then, add other liquid components

[0210] (DINP, IPPP, Z-6040, etc.).

[0211] Step 2: Apply vacuum and mix at medium agitation for 30 minutes;

[0212] Step 3: Charge alumina into a container; apply vacuum after incorporating the powder; mix at a high stirring rate for 30 minutes;

[0213] Step 4: Charge the fumed silica into a container; apply vacuum after incorporating the powder; mix at a high stirring rate for 1 hour;

[0214] Step 5 Set the temperature bath to 80°C; keep mixing at a moderate to low stirring rate for 30 minutes to maintain this temperature;

[0215] Step 6 Set the temperature bath to 20°C to cool to <40°C;

[0216] Test the tack-free time according to the following procedure: (ASTM C679-03)

[0217] Take 10 g of Part B and place it in a 50 ml plastic beaker, and place the beaker in an oven at 45% humidity and 23°C. Start time recording. Periodically take out the beaker and gently touch the surface of Part B with a plastic stick. As the reaction between Part B and moisture increases, the surface viscosity increases. When the surface of Part B is no longer sticky, stop time recording. Record this duration as the tack-free time of Part B.

[0218] Prepare Part A polyol mixture according to the following procedure:

[0219] Step 1: Charge castor oil, polyurethane polyol, CP450 and BDO into a container. Step 2: Heat to 80°C; apply vacuum and mix at medium stirring speed for 1 hour to degas. Step 3: Charge ATH into a container and apply vacuum after incorporating the powder; mix at high stirring speed for 15 minutes;

[0220] Step 4: Charge molecular sieve 3A into a container; apply vacuum after incorporating the powder; mix at a high stirring rate for 15 minutes;

[0221] Step 5: Charge H-18 into a container; apply vacuum after incorporating the powder; mix at a high stirring rate for 1 hour;

[0222] Step 6 Cool to <40°C.

[0223] Use the following procedure to make the overlap test specimen: (GB / T7124)

[0224] 1. A substrate was made of 3003 aluminum alloy with a size of 25 mm × 12.5 mm.

[0225] 2. Clean the substrate surface by wiping with ethanol.

[0226] 3. Mask the bonding area of ​​25 mm x 12 mm by using pressure sensitive tape.

[0227] 4. Combine Part A and Part B of the adhesive and place in a high speed mixer at 1,000 rpm for 1 minute to ensure thorough mixing.

[0228] 5. Apply 0.5g to 1.5g of adhesive in the bonding area of ​​the substrate. Place two copper wires with a diameter of 0.25mm to control the thickness of the adhesive.

[0229] 6. Along the length direction, stack another masked substrate with the same bonding area in head-to-head contact. Compress and tighten the bonding surface with two side-by-side clamps.

[0230] 7. Allow the adhesive to cure at 25°C for 7 days.

[0231] The butt joint test specimens were made based on the following procedure: (GB / T6329)

[0232] 1. The base material diameter was made by 3003 aluminum alloy with the size of 60mm height and 15mm diameter.

[0233] 2. Clean the substrate surface by wiping with ethanol.

[0234] 3. Combine Part A and Part B of the adhesive and place in a high speed mixer at 1,000 rpm for 1 minute to ensure thorough mixing.

[0235] 4. Apply 0.5g to 1g of adhesive on the flat surface of the substrate. Place two copper wires with a diameter of 1.00mm to control the thickness of the adhesive.

[0236] 5. Stack another clean substrate with the flat surfaces bonded together. Hold the stacked substrates vertically so that the bonding surfaces can be constantly fastened by gravity.

[0237] 6. Allow the adhesive to cure at 25°C for 7 days.

[0238] The test specimens were assembled on the fixture of an Instron testing machine and the shear strength of the lap joint and the tensile strength of the butt joint were tested at a strain rate of 5 mm / min.

Claims

1. A polyurethane adhesive composition, comprising: (a) a polyol component, the polyol component comprising a phosphate-modified polyol and a vegetable oil-modified polyol, and (b) an isocyanate component comprising an NCO-terminated polyurethane prepolymer which is the reaction product of (i) a polyester polyol based on a dimer acid and an aromatic dicarboxylic acid and (ii) an isocyanate monomer.

2. The polyurethane adhesive composition according to claim 1, wherein the polyurethane adhesive composition is solvent-free.

3. The polyurethane adhesive composition of claim 1, wherein the polyester polyol based on dimer acid and aromatic dicarboxylic acid is prepared from a reactive mixture of at least one dimer acid, at least one aromatic dicarboxylic acid and at least one polyol.

4. The polyurethane adhesive composition according to claim 3, wherein the weight ratio of the at least one aromatic dicarboxylic acid to the at least one dimer acid is >0 and <4.

2.

5. The polyurethane adhesive composition of claim 3, wherein the at least one dimer acid is selected from the group consisting of an acyclic dimer acid, a cyclic dimer acid, an aromatic dimer acid, a polycyclic dimer acid, and any combination thereof.

6. The polyurethane adhesive composition of claim 3, wherein the at least one aromatic dicarboxylic acid is selected from the group consisting of phthalic acid, isophthalic acid, terephthalic acid, and any combination thereof.

7. The polyurethane adhesive composition of claim 1, wherein the polyol component comprises 1% to 50% of the phosphate ester modified polyol and 1% to 99% of the vegetable oil modified polyol, based on the weight of the polyol component. 8 . The polyurethane adhesive composition of claim 1 , wherein the isocyanate component and the polyol component have an NCO / OH molar ratio of 0.9:1 to 1.95:

1.

9. An isocyanate agent for use in a polyurethane adhesive composition, the isocyanate agent comprising an NCO-terminated polyurethane prepolymer, the NCO-terminated polyurethane prepolymer being the reaction product of (i) a polyester polyol based on a dimer acid and an aromatic dicarboxylic acid and (ii) an isocyanate monomer.

10. A method of using the polyurethane adhesive composition according to claim 1, the method comprising: (a) providing the polyurethane adhesive composition according to claim 1; (b) contacting the polyol component with the isocyanate component to form a curable mixture; (c) applying the curable mixture to a first substrate to which at least a second substrate will bond; (d) contacting the second substrate with the first substrate such that at least a portion of the curable mixture is sandwiched between the first substrate and the second substrate; as well as (e) curing the curable mixture, or causing it to cure.

11. Use of the polyurethane adhesive composition according to claim 1 in a battery pack.