Construction method for anticorrosive coating of steel structural member
By spraying a combination of coatings such as epoxy zinc-rich primer, epoxy mica intermediate paint and fire-retardant coating on the surface of the steel structure, the problem of corrosion of the steel structure is solved, the service life is significantly extended, and the safety and durability are improved, achieving Simple, fast and cost-effective anti-corrosion effect.
Patent Information
- Application Number
- CN202410805931.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-21
- Publication Date
- 2024-10-25
AI Technical Summary
Steel structures are prone to corrosion in the natural environment, resulting in reduced strength and toughness, impact on load-bearing capacity and potential safety hazards. Existing anti-corrosion measures have limited effectiveness.
An anti-corrosion coating construction method for steel structural components is adopted, which includes spraying epoxy zinc-rich primer, epoxy cloud iron intermediate paint, fire retardant paint and topcoat in sequence after surface rust removal, and repainting the nodes after installation. Through the combination of zinc powder, flake pigments and intumescent fire retardant coatings, a strong coating system is formed to isolate corrosive media.
Significantly reduce the corrosion rate of steel, extend the service life, improve the safety and durability of steel structures, use simple and fast construction methods, reduce maintenance and replacement costs, and have good cost performance and economic benefits.
Smart Images

Figure BDA0004904708230000021 
Figure BDA0004904708230000031
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of steel structure building component processing, and specifically, relates to a construction method for anti-corrosion coating of steel structure components. Background Art
[0002] With the continuous development and progress of modern construction technology, the application of steel structure buildings in the fields of industry and civil construction is becoming more and more common. However, due to the corrosion-prone nature of steel itself, effective anti-corrosion measures need to be taken during the use of steel structures to extend their service life. Steel easily reacts with oxygen, water and other chemicals in the natural environment, leading to corrosion. In addition, factors such as humidity, temperature, and salt in the environment will also accelerate the corrosion of steel. Corrosion will not only reduce the strength, toughness and ductility of steel, affecting its bearing capacity, but also destroy the integrity of the steel structure, leading to safety hazards. Summary of the invention
[0003] The purpose of the present invention is to provide a construction method for anti-corrosion coating of steel structural components to solve the potential safety hazard problem caused by the corrosion of existing steel structural components.
[0004] The purpose of the present invention is achieved through the following technical solutions:
[0005] A construction method for anti-corrosion coating of a steel structure component comprises the following steps:
[0006] S1. Surface pretreatment of engineering steel structure components;
[0007] S2. Spray epoxy zinc-rich primer, epoxy micaceous iron intermediate paint, fire retardant paint and topcoat on the engineering steel structure components in sequence;
[0008] S3. Install each steel structure component and repaint the nodes after installation.
[0009] In this application:
[0010] Epoxy zinc-rich primer contains high concentration of zinc powder. Zinc has good anti-corrosion properties, which can prevent corrosion of metal substrates and extend the service life of the coating. Especially in high temperature, high humidity and other corrosive environments, zinc will be corroded first, thereby protecting iron from erosion and playing an electrochemical protective role. At the same time, epoxy zinc-rich primer can provide good adhesion, so that the upper coating and the substrate form a strong bond, increasing the durability and stability of the coating. After spraying on the steel surface, it is firmly adhered and is not prone to falling off.
[0011] Epoxy micaceous iron intermediate paint contains flake pigments, which can play an excellent shielding effect and has a good isolation and anti-rust effect. It effectively isolates the steel surface from the external oxygen, moisture and corrosive media, and reduces the corrosion rate of the steel. Excellent adhesion ensures the stability and durability of the coating on the steel surface and reduces the risk of coating shedding. In accordance with the design specifications, the service life of the anti-corrosion coating with epoxy micaceous iron intermediate paint is higher than that of the coating with only primer and topcoat. At the same time, it provides a good adhesion foundation for subsequent coatings, enhancing the stability, durability and durability of the entire coating system.
[0012] The fire-retardant paint is applied on the epoxy micaceous iron intermediate paint layer, which has a firm and reliable adhesion and also has a good fire-retardant effect.
[0013] Finally, the surface is painted with topcoat, which is a decorative and protective paint, mainly used to change the appearance and texture of objects and protect objects from erosion by the external environment, such as sunlight, rain, wind and snow, etc., to prevent corrosion of steel structure components and further extend the service life of steel structure components.
[0014] As an implementable embodiment, the surface pretreatment in step S1 is specifically to remove rust from the surface of the steel structure component so that its surface reaches Sa2.5 level and has a roughness of 40-70 μm.
[0015] As an implementable method, the step S2 of spraying the epoxy zinc-rich primer is carried out within 3 hours after the surface pretreatment of S1 is completed; and the step S3 of repainting the nodes is carried out within 72 hours after the surface pretreatment of S1 is completed.
[0016] As an implementable embodiment, the topcoat in step S2 is acrylic topcoat or epoxy varnish.
[0017] As an implementable embodiment, the construction conditions for spraying and re-coating of S2 and S3 are: air temperature 5-35°C, relative humidity ≤85%, and substrate temperature <60°C.
[0018] As an implementable embodiment, the spraying in step S2 is performed by airless spraying with a high-pressure airless sprayer and brushing.
[0019] As an implementation method, the thickness of the epoxy zinc-rich primer is 70-80 μm, the thickness of the epoxy micaceous iron intermediate paint is 70-110 μm, and the thickness of the topcoat is 100-110 μm. The specific standards are shown in Table 1:
[0020] Table 1
[0021]
[0022]
[0023] As an implementation method, the fire retardant coating is an intumescent fire retardant coating with a spraying thickness of 2 mm and an equivalent thermal resistance of 0.25 mm. 2 ℃ / W.
[0024] Beneficial effects of the present invention:
[0025] 1. This application mainly applies an anti-corrosion coating on the surface of the steel structure. The anti-corrosion coating can effectively isolate the steel from the contact with the corrosive medium, and can prevent the corrosion of the steel by moisture, oxygen and other corrosive substances in the air, thereby significantly reducing the corrosion rate of the steel, extending the service life of the steel structure, and is conducive to ensuring and improving the safety and durability of steel structure buildings.
[0026] 2. The construction of this application is simple, fast and efficient, ensuring the quality of anti-corrosion coating construction of steel structure components; the construction cost of anti-corrosion coating is relatively low, and the coating has a long service life, which can reduce the maintenance and replacement costs of steel structures during use. Compared with other anti-corrosion methods, the present invention has better cost performance and economic benefits.
[0027] 3. This application treats steel structure components by means of primer, intermediate paint, topcoat and node paint, which can not only improve the anti-corrosion performance of the steel structure, but also improve its appearance quality. DETAILED DESCRIPTION
[0028] The following non-limiting examples serve to illustrate the invention.
[0029] Example:
[0030] A construction method for anti-corrosion coating of a steel structure component comprises the following steps:
[0031] S1. Surface pretreatment of engineering steel structure components:
[0032] (1) Rust removal on the steel surface before painting should comply with the design requirements and the provisions of the relevant national standards. The treated steel surface should be free of welding slag, welding scars, dust, oil, water and burrs.
[0033] (2) The surface of the component should be shot blasted to Sa2.5 level, that is, very thorough shot blasting and rust removal. There should be no visible grease, dirt, blocky oxide scale, rust, old paint and other impurities on the surface, and the remaining traces should only show slight spots. Rust removal on the construction site uses tools such as emery cloth, sandpaper, scraper, wire brush, hammer chisel, etc., and can also be removed by manual knocking, grinding, scraping and sweeping to remove rust, oxide scale and impurities.
[0034] (3) The surface roughness after shot blasting and rust removal should be between 40-70μm.
[0035] (4) Oil stains and dust should be removed by using diluents and sweeping the floor.
[0036] (5) After rust removal, the surface of the steel structure should be cleaned with a brush or other tools, or the rust dust and residual abrasive should be blown away with clean compressed air before proceeding to the next process.
[0037] S2. Spray epoxy zinc-rich primer, epoxy micaceous iron intermediate paint, fire retardant coating and topcoat on the engineering steel structure components in sequence, of which the topcoat is acrylic topcoat or epoxy varnish; the fire retardant coating adopts intumescent fire retardant coating, the spraying thickness is 2mm, and its equivalent thermal resistance is: 0.25m2·℃ / W. The painting in the factory adopts imported Graco BULLDOG33:1 high-pressure airless sprayer for spraying, and airless spraying and brushing are carried out on site. The thickness of indoor and outdoor coating is shown in Table 1. Key points of coating process control:
[0038] (1) Construction conditions: Temperature 5-35℃, relative humidity ≤85%. Construction is not allowed in rain, fog or heavy dust. Construction is suspended when the substrate temperature is greater than 60℃.
[0039] (2) The first coat of primer should be applied within 3 hours after surface rust removal treatment, otherwise corresponding rust removal measures are required.
[0040] (3) Before spraying, the paint must be fully stirred to ensure uniform mixing.
[0041] (4) If the previous coat of paint has been applied for too long, the surface should be roughened with water sandpaper before applying the next coat of paint to remove dust and dirt on the surface before painting to ensure interlayer adhesion.
[0042] (5) The tools used for construction should be clean and dry. The paint must not be mixed with water or other impurities. The paint should be prepared and used immediately and must be used up within 8 hours.
[0043] (6) Protective measures should be taken before the paint film dries.
[0044] (7) In order to ensure the thickness of the paint film at the edges and corners of the weld, a layer of paint should be applied manually before spraying a large area.
[0045] (8) Construction should be carried out strictly in accordance with the mixing ratio, diluent, spraying pressure, coating interval and other parameters specified in the product manual.
[0046] (9) Painters must be certified before taking up their posts, and technical personnel must provide technical briefings on painting requirements before taking up their posts.
[0047] S3. Install all steel structure components and repaint the nodes after installation; the welding parts should be painted within 72 hours after rust removal, otherwise rust removal measures must be taken first.
[0048] The above basic examples of the present invention and their further optional examples can be freely combined to form multiple embodiments, all of which are embodiments that can be adopted and claimed for protection by the present invention. In the scheme of the present invention, each optional example can be arbitrarily combined with any other basic examples and optional examples.
[0049] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A construction method for anti-corrosion coating of steel structure components, characterized in that: The following steps are involved: S1. Carry out surface pretreatment on engineering steel structure components; S2. Spray epoxy zinc-rich primer, epoxy micaceous iron intermediate paint, fire retardant paint and topcoat on the engineering steel structure components in sequence; S3. Install each steel structure component and repaint the nodes after installation.
2. The construction method of anti-corrosion coating of steel structure components according to claim 1, characterized in that: The surface pretreatment in step S1 is specifically to remove rust from the surface of the steel structure component so that the surface reaches Sa2.5 level and the roughness is 40-70 μm.
3. The construction method of anti-corrosion coating of steel structure components according to claim 1, characterized in that: The step S2 of spraying epoxy zinc-rich primer is carried out within 3 hours after the surface pretreatment of S1 is completed; the step S3 of repainting the nodes is carried out within 72 hours after the surface pretreatment of S1 is completed.
4. The construction method of anti-corrosion coating of steel structure components according to claim 1, characterized in that: The topcoat in step S2 is acrylic topcoat or epoxy varnish.
5. The construction method of anti-corrosion coating of steel structure components according to claim 1, characterized in that: The construction conditions for spraying and re-coating of S2 and S3 are: air temperature 5-35°C, relative humidity ≤85%, and substrate temperature <60°C.
6. The construction method of anti-corrosion coating of steel structure components according to claim 5 is characterized in that: The spraying in step S2 is carried out by airless spraying and brushing.
7. A construction method for anti-corrosion coating of steel structure components according to claim 6, characterized in that: The thickness of the epoxy zinc-rich primer is 70-80 μm, the thickness of the epoxy micaceous iron intermediate paint is 70-110 μm, and the thickness of the topcoat is 100-110 μm.
8. The construction method of anti-corrosion coating of steel structure components according to claim 6, characterized in that: The fire retardant coating adopts an intumescent fire retardant coating with a spraying thickness of 2 mm. Its equivalent thermal resistance is: 0.25m 2 ·℃ / W。
Citation Information
Patent Citations
Fireproof coating used for steel structure buildings, preparation method thereof and coating process
CN103788814A
Heavy duty anticorrosion coating used for coastal region steel structure, and construction technology thereof
CN106243917A
Ultrathin water-based steel structure fireproofing coating and preparation method thereof, as well as coating process
CN106590286A
Weather-resistant corrosion-resistant anticorrosive coating for steel structure surfaces and preparation method thereof
CN109554064A
Anti-corrosion coating system for outer wall of tower drum of marine wind turbine generator and coating method
CN113150642A
Cited By
Coating method of fireproof coating
CN119549377A
Manufacturing process of auxiliary truss bolting and welding combined steel truss girder
CN121321511A