Method for regulating and controlling carbon content in aluminum nitride, product and application

Through ball milling of glucose alcohol solution and aluminum nitride powder and high-temperature heat treatment, the problem of difficult dispersion of carbon black in adjusting the carbon content in aluminum nitride was solved, high-quality preparation of aluminum nitride was achieved, the process was simplified, and the carbon content was improved. Accuracy and uniformity, meeting the requirements of standard samples.

CN118833784AActive Publication Date: 2024-10-25SHANDONG NON METALLIC MATERIAL RESEARCH INSTITUTE
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411086336.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-10-25
Estimated Expiration
2044-08-08

AI Technical Summary

Technical Problem

Existing methods for adjusting the carbon content in aluminum nitride are difficult to disperse and easy to agglomerate, resulting in poor carbon content uniformity and inability to meet the requirements of standard samples. The process is cumbersome and time-consuming, affecting the accuracy of aluminum nitride.

Method used

Glucose alcohol solution and aluminum nitride powder are used for ball milling, followed by drying and high-temperature heat treatment. Through this method, the carbon content in aluminum nitride can be controlled, the process flow can be simplified, and the accuracy and uniformity of the carbon content can be improved.

Benefits of technology

This method can achieve uniform dispersion of glucose without adding a dispersant, simplify the process, reduce costs, control the carbon content in aluminum nitride powder in small batches, improve the uniformity and accuracy of aluminum nitride, and meet the requirements of standard samples.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004985281760000091
    Figure BDA0004985281760000091
Patent Text Reader

Abstract

The invention belongs to the field of aluminum nitride preparation, and discloses a method for regulating and controlling the carbon content in aluminum nitride, a product and application, and the method comprises the following steps: mixing a glucose alcohol solution with aluminum nitride powder, and carrying out ball milling to obtain uniformly mixed slurry; drying the slurry to obtain dry powder; and carrying out heat treatment on the dry powder in a vacuum or inert atmosphere to regulate and control the carbon content in the aluminum nitride. The problems that when the carbon content is regulated and controlled in the preparation process of the aluminum nitride powder, carbon black is often used as a carbon source, the carbon source is not easy to disperse and easy to agglomerate, the use amount of the carbon source is large, and the uniformity of the obtained aluminum nitride powder cannot meet the requirement are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of aluminum nitride preparation, and specifically relates to a method for regulating the carbon content in aluminum nitride, a product and an application. Background Art

[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.

[0003] Standard samples, sometimes called standard substances, are materials or substances with one or more sufficiently uniform and well-defined characteristic values, which are used to calibrate measuring devices, evaluate measuring methods or assign values ​​to materials. It can be a pure or mixed gas, fluid or solid. ISO Guide 30:1992 also gives the definition of certified standard samples: standard samples with certificates, one or more characteristic values ​​of which are determined by established traceability procedures, so that they can be traced back to accurately reproduced measurement units used to express the characteristic values, and each standard value is accompanied by an uncertainty with a given confidence level. Standard samples are widely used in measurement quality assurance, product quality management, evaluation of measurement methods, and the scientific formulation and effective implementation of regulations. In recent years, standard samples are playing an increasingly important role in the construction of a market economy, requiring more and more varieties of standard samples with higher and higher quality.

[0004] Among them, aluminum nitride (AI N) has a high thermal conductivity (theoretically up to 320w·m -1 K -1 ), good insulation (>10"Q·cm), low dielectric constant (8.0 at 1MHz test conditions) and dielectric loss (dielectric loss angle tanδ=10 -4 ), and the thermal expansion coefficient that matches silicon (3.2×10 -6 K -1 ), good chemical stability and non-toxicity, etc., good chemical stability and non-toxicity, etc., have a wide range of applications in semiconductors, electric vacuum and other fields, and are also key materials for electronic components in automotive electronics, aerospace and military defense. The different carbon content of aluminum nitride changes the properties of aluminum nitride. Aluminum nitride with different carbon contents is used in different fields. Therefore, it is of great significance to regulate the carbon content in aluminum nitride and obtain standard samples of aluminum nitride with corresponding carbon content.

[0005] At present, the commonly used method for adjusting the carbon content in aluminum nitride is to adjust the amount of raw material carbon black added during the preparation of aluminum nitride, so as to achieve the purpose of adjusting the carbon content. Since carbon black is difficult to disperse and easy to agglomerate, measures need to be taken to fully mix it. For example, patent CN 117800737A discloses a high-purity aluminum nitride powder and a batch preparation method thereof, wherein a dispersant and a binder are added to a mixture of carbon black and aluminum nitride, and dry grinding and wet grinding are performed to obtain a precursor slurry, and high-temperature nitriding treatment and decarburization treatment are combined to obtain a high-purity aluminum nitride powder. This method is often used in workshops for batch production, and carbon black is dispersed by adding an auxiliary agent. The amount of carbon black used is large, and multiple operations such as dry grinding and wet grinding are performed. The operation steps for carbon black dispersion are cumbersome and time-consuming, and the amount of carbon black used is large. The carbon black slurry is easy to adhere to the inner wall of the dry grinding container and the high-temperature furnace, thereby affecting the accuracy of the carbon content in the aluminum nitride. At the same time, the uniformity of the carbon black slurry is poor, and the uniformity of the obtained aluminum nitride cannot meet the requirements of the standard sample. Summary of the invention

[0006] In order to solve the deficiencies of the prior art, the purpose of the present invention is to provide a method, product and application for regulating the carbon content in aluminum nitride. The method provided by the present invention solves at least one of the above problems.

[0007] In a first aspect, the present invention provides a method for regulating the carbon content in aluminum nitride, comprising:

[0008] The glucose alcohol solution is mixed with aluminum nitride powder and ball milled to obtain a uniformly mixed slurry;

[0009] Drying the slurry to obtain dry powder;

[0010] The dry powder is heat treated under vacuum or inert atmosphere to adjust the carbon content in aluminum nitride.

[0011] Preferably, the heat treatment temperature is 600-1500° C., and the holding time is 15-60 min.

[0012] Preferably, the inert atmosphere is one of nitrogen or argon.

[0013] Preferably, the glucose alcohol solution is an absolute ethanol solution of glucose.

[0014] Preferably, the mass ratio of glucose alcohol solution to aluminum nitride powder is 40.99:0.1-0.3.

[0015] Preferably, after the glucose alcohol solution is mixed with the aluminum nitride powder, ball milling is performed, and the ball milling speed is 250-350r / min; further preferably, the ball-to-material ratio is 3-5:1, and the ball milling time is 20-28h. Further preferably, the ball milling is wet ball milling.

[0016] Preferably, the drying is vacuum drying at a drying temperature of 35-45°C.

[0017] In a second aspect, the present invention provides aluminum nitride prepared by the method described in the first aspect.

[0018] A third aspect is the use of the method described in the first aspect in the preparation of aluminum nitride.

[0019] The beneficial effects achieved by one or more technical solutions of the present invention are as follows:

[0020] 1. The present invention mixes glucose and aluminum nitride by mixing and ball-milling a glucose alcohol solution with aluminum nitride powder and then drying the mixture, thereby improving the uniformity of the mixture of glucose and aluminum nitride powder. At the same time, the glucose can be evenly dispersed without adding dispersants or other additives. After heat treatment, high-quality aluminum nitride can be obtained. The treatment method is helpful to improve the accuracy and uniformity of the carbon content in aluminum nitride. The treatment method is simple, the process flow is simple, the equipment requirements are not high, the cost is low, and the carbon content in aluminum nitride powder can be regulated in small batches.

[0021] 2. Since the accuracy of the carbon content that needs to be regulated in the process of introducing carbon source into aluminum nitride is high, a carbon source soluble in ethanol is selected, and glucose alcohol solution is used to mix with aluminum nitride for ball milling. After the glucose is evenly mixed with aluminum nitride, it is first carbonized and then dissolved into aluminum nitride. At the same time, the wet ball milling method is more conducive to the uniform dispersion of glucose alcohol solution and aluminum nitride powder, and then heat treatment is carried out to further improve the uniformity of aluminum nitride. DETAILED DESCRIPTION

[0022] In view of the fact that carbon black is often used as a carbon source when regulating the carbon content in the existing preparation process of aluminum nitride powder, the carbon source is not easy to disperse and is easy to agglomerate, the amount of carbon source used is relatively large, and the uniformity of the obtained aluminum nitride powder cannot meet the requirements, the present invention proposes a method, product and application for regulating the carbon content in aluminum nitride.

[0023] A typical embodiment of the present invention provides a method for regulating the carbon content in aluminum nitride, comprising: mixing a glucose alcohol solution with aluminum nitride powder, ball milling, and obtaining a uniformly mixed slurry; drying the slurry to obtain a dry powder; and heat treating the dry powder under vacuum or an inert atmosphere at a heat treatment temperature of 600 to 1500°C and a holding time of 15 to 60 minutes, thereby achieving regulation of the carbon content in aluminum nitride.

[0024] Since the addition of C into AlN is a p-type substitution, the original lattice undergoes a slight deformation after the addition, and its geometric parameters and electronic structure also change. After the addition, the mean free path of phonons can be effectively increased, thereby improving the lattice thermal conductivity of intrinsic AlN.

[0025] Another embodiment of the present invention provides aluminum nitride, which is prepared by the method described in the first aspect.

[0026] A third embodiment of the present invention provides the use of the method described in the first aspect in preparing aluminum nitride.

[0027] The following will describe the implementation methods of the present invention in detail in conjunction with specific embodiments, so that the implementation process of how the present invention applies technical means to solve technical problems and achieve technical effects can be fully understood and implemented accordingly.

[0028] Unless otherwise specified, the technical means used in the examples are conventional means well known to those skilled in the art, and the reagents and products used are all commercially available.

[0029] Example 1

[0030] Add glucose to anhydrous ethanol and stir evenly to obtain a 0.125wt% glucose alcohol solution:

[0031] Aluminum nitride powder with a purity of 99% and glucose alcohol solution were mixed in a weight ratio of 0.3:40.99, added into a ball mill and mixed for 24 hours at a ball mill speed of 300 r / min and a ball-to-material ratio of 4:1;

[0032] Place the mixed slurry in a vacuum drying oven at 40°C for vacuum drying. Stop drying when the slurry turns into powder.

[0033] The dried powder is placed in a corundum crucible for heat treatment at a temperature of 1000° C. for 45 minutes in a vacuum atmosphere to obtain treated aluminum nitride powder.

[0034] Example 2

[0035] Add glucose to anhydrous ethanol and stir evenly to obtain a 0.175wt% glucose alcohol solution:

[0036] Aluminum nitride powder with a purity of 99% and glucose alcohol solution were mixed in a weight ratio of 0.3:40.99, added into a ball mill and mixed for 24 hours at a ball mill speed of 300 r / min and a ball-to-material ratio of 4:1;

[0037] Place the mixed slurry in a vacuum drying oven at 40°C for vacuum drying. Stop drying when the slurry turns into powder.

[0038] The dried powder is placed in a corundum crucible for heat treatment at a temperature of 1000° C. for 45 minutes in a vacuum atmosphere to obtain treated aluminum nitride powder.

[0039] Example 3

[0040] Add glucose to anhydrous ethanol and stir evenly to obtain a 0.225wt% glucose alcohol solution:

[0041] Aluminum nitride powder with a purity of 99% and glucose alcohol solution were mixed in a weight ratio of 0.2:40.99, added into a ball mill and mixed for 24 hours at a ball mill speed of 300 r / min and a ball-to-material ratio of 4:1;

[0042] Place the mixed slurry in a vacuum drying oven at 40°C for vacuum drying. Stop drying when the slurry turns into powder.

[0043] The dried powder is placed in a corundum crucible for heat treatment at a temperature of 1000° C. for 45 minutes in a vacuum atmosphere to obtain treated aluminum nitride powder.

[0044] Example 4

[0045] Add glucose to anhydrous ethanol and stir evenly to obtain a 0.275wt% glucose alcohol solution:

[0046] Aluminum nitride powder with a purity of 99% and glucose alcohol solution were mixed in a weight ratio of 0.2:40.99, added into a ball mill and mixed for 24 hours at a ball mill speed of 300 r / min and a ball-to-material ratio of 4:1;

[0047] Place the mixed slurry in a vacuum drying oven at 40°C for vacuum drying. Stop drying when the slurry turns into powder.

[0048] The dried powder is placed in a corundum crucible for heat treatment at a temperature of 1000° C. for 45 minutes in a vacuum atmosphere to obtain treated aluminum nitride powder.

[0049] Example 5

[0050] Add glucose to anhydrous ethanol and stir evenly to obtain a 0.325wt% glucose alcohol solution:

[0051] Aluminum nitride powder with a purity of 99% and glucose alcohol solution were mixed in a weight ratio of 0.1:40.99, added into a ball mill and mixed for 24 hours at a ball mill speed of 300 r / min and a ball-to-material ratio of 4:1;

[0052] Place the mixed slurry in a vacuum drying oven at 40°C for vacuum drying. Stop drying when the slurry turns into powder.

[0053] The dried powder is placed in a corundum crucible for heat treatment at a temperature of 1000° C. for 45 minutes in a vacuum atmosphere to obtain treated aluminum nitride powder.

[0054] Example 6

[0055] Add glucose to anhydrous ethanol and stir evenly to obtain a 0.375wt% glucose alcohol solution:

[0056] Aluminum nitride powder with a purity of 99% and glucose alcohol solution were mixed in a weight ratio of 0.1:40.99, added into a ball mill and mixed for 24 hours at a ball mill speed of 300 r / min and a ball-to-material ratio of 4:1;

[0057] Place the mixed slurry in a vacuum drying oven at 40°C for vacuum drying. Stop drying when the slurry turns into powder.

[0058] The dried powder is placed in a corundum crucible for heat treatment at a temperature of 1000° C. for 45 minutes in a vacuum atmosphere to obtain treated aluminum nitride powder.

[0059] Example 7

[0060] Add glucose to anhydrous ethanol and stir evenly to obtain a 0.325wt% glucose alcohol solution:

[0061] Aluminum nitride powder with a purity of 99% and glucose alcohol solution were mixed in a weight ratio of 0.1:40.99, added into a ball mill and mixed for 28 hours, the ball mill speed was 250r / min, and the ball-to-material ratio was 3:1;

[0062] Place the mixed slurry in a vacuum drying oven at 35°C for vacuum drying. Stop drying when the slurry turns into powder.

[0063] The dried powder was placed in a corundum crucible for heat treatment at a temperature of 600° C. for 60 min in a nitrogen atmosphere to obtain treated aluminum nitride powder.

[0064] Example 8

[0065] Add glucose to anhydrous ethanol and stir evenly to obtain a 0.375wt% glucose alcohol solution:

[0066] Aluminum nitride powder with a purity of 99% and glucose alcohol solution were mixed in a weight ratio of 0.1:40.99, and added into a ball mill for ball milling for 20 hours. The ball mill speed was 350 r / min, and the ball-to-material ratio was 5:1.

[0067] Place the mixed slurry in a vacuum drying oven at 45°C for vacuum drying. Stop drying when the slurry turns into powder.

[0068] The dried powder was placed in a corundum crucible for heat treatment at a temperature of 1500° C. for a holding time of 45 min and an argon atmosphere to obtain treated aluminum nitride powder.

[0069] The aluminum nitride powder obtained by the treatment of Examples 1-8 was tested for element content, and the changes in carbon element in the aluminum nitride powder were shown in Table 1.

[0070] Table 1 Changes in carbon content before and after treatment (in mass percentage)

[0071]

[0072] It can be seen from Table 1 and Examples 1-6 that the higher the concentration of the glucose solution, the higher the carbon content in the aluminum nitride. Therefore, the carbon content in the final aluminum nitride can be regulated by controlling the concentration of the glucose solution.

[0073] The preparation method of the present invention performs high-temperature and normal-pressure heat treatment on AlN powder doped with C, so that the original AlN lattice undergoes slight deformation, and its geometric parameters and electronic structure also change. The incorporation of C can effectively increase the mean free path of phonons, thereby improving the lattice thermal conductivity of intrinsic AlN and further improving the performance of aluminum nitride.

[0074] Comparative Example 1

[0075] The difference from Example 1 is that glucose is replaced by sucrose, and the sucrose alcohol solution is mixed with aluminum nitride powder, and the remaining steps are the same.

[0076] The aluminum nitride powder obtained by the above treatment was tested for element content. The results showed that sucrose was almost insoluble in ethanol and the carbon content of the aluminum nitride powder after treatment was almost unchanged.

[0077] Comparative Example 2

[0078] The difference from Example 1 is that the glucose alcohol solution is replaced by a 0.125 wt % glucose aqueous solution, the sucrose alcohol solution is mixed with aluminum nitride powder, and the remaining steps are the same.

[0079] The aluminum nitride powder obtained by the above treatment was tested for element content. The results showed that although the carbon content of the treated aluminum nitride powder increased, most of the aluminum nitride was oxidized to aluminum oxide. This was due to the long-term grinding of aluminum nitride in an aqueous solution, which led to the violent hydrolysis of aluminum nitride.

[0080] Since aluminum nitride will hydrolyze when in contact with water, resulting in aluminum nitride being hydrolyzed and oxidized to aluminum oxide, anhydrous ethanol is selected as the solvent. Since the amount of carbon source introduced is very small, glucose carbon source soluble in ethanol is selected to make the raw materials mixed more evenly.

[0081] Since glucose is first carbonized and then dissolved into aluminum nitride after being evenly mixed, the carbon content is very trace, and direct addition will cause uneven mixing of the raw materials. Therefore, it is chosen to dissolve glucose in alcohol, mix the alcohol solution with aluminum nitride powder, and then perform heat treatment to make it more uniform.

[0082] Comparative Example 3

[0083] This comparative example is Example 1 of patent CN 117800737 A, comprising the following steps:

[0084] S1: 1200g of aluminum oxide and 530g of carbon black were put into a horizontal ball mill for dry grinding for 20min at a speed of 30r / min, and then 6800g of water, 8.5g of acrylic copolymer dispersant, 46.5g of polyethylene glycol, 40g of polyvinyl alcohol mixed binder and 6g of sintering aid were added, and wet grinding was performed for 60min at a speed of 80r / min to obtain a precursor slurry, and a precursor granulated powder with a particle size of about 100μm was obtained by spray granulation;

[0085] S2: Feed the precursor granulated powder obtained in S1 to the large-bellied tube of the high-temperature rotary furnace through an automatic feeder; evacuate the high-temperature rotary furnace, and when the vacuum reaches 97kpa, maintain the pressure for 20 minutes, and introduce nitrogen until the pressure in the furnace reaches a slightly positive pressure. Repeat the above gas washing operation twice, and then start the furnace heating program. Rise the temperature at a rate of 10℃ / min to 1550℃, keep warm for 4h, the furnace tube speed is 2r / min, and the nitrogen flow rate is 150L / h; high-temperature nitridation is performed to obtain gray aluminum nitride powder containing trace amounts of carbon;

[0086] S3: The gray aluminum nitride powder obtained in S2 is sent to a decarburization rotary furnace at 650°C for 3 hours for air decarburization, and then crushed by a jet mill to obtain high-purity aluminum nitride powder.

[0087] The target carbon content of the obtained high-purity aluminum nitride was 300 ppm, the actual carbon content was 270 ppm, the error was 10%, and the uniformity was 3.17.

[0088] Comparative Example 4

[0089] This comparative example is an adjustment of Example 1 of patent CN 117800737 A. Since the patent is a batch production step, the raw materials of this scheme are adjusted in equal proportions. The specific steps are as follows:

[0090] S1: 120g of alumina and 53g of carbon black were put into a horizontal ball mill and dry-milled for 20min at a speed of 30r / min, and then 680g of water, 0.85g of acrylic copolymer dispersant, 4.65g of polyethylene glycol, 4g of polyvinyl alcohol mixed binder and 0.6g of sintering aid were added, and wet-milled for 60min at a speed of 80r / min to obtain a precursor slurry, which was spray-granulated to obtain a precursor granulated powder with a particle size of about 100μm;

[0091] The precursor granulated powder is placed in a corundum crucible for heat treatment at a temperature of 1000° C. for a holding time of 45 minutes and an argon atmosphere to obtain treated aluminum nitride powder.

[0092] The target carbon content of the aluminum nitride powder obtained in Comparative Example 3 is expected to be 400 ppm. After testing, the actual carbon content of the obtained aluminum nitride powder is 467 ppm, the error is 16.75%, and the uniformity is 3.77.

[0093] It can be seen from the embodiments and comparative example 3 that the nitrogen content of aluminum nitride of the present invention is more accurately regulated and has better uniformity. Comparative example 3 actually regulates the carbon content in aluminum nitride in batches in the production workshop, while the present invention prepares standard samples of aluminum nitride in the laboratory and applies the batch preparation method to the laboratory. As shown in comparative example 4, due to the poor dispersibility of carbon black, even if it is dispersed, the uniformity of the obtained aluminum nitride still cannot meet the requirements of the standard sample. At the same time, the carbon black slurry is easy to adhere to the container wall. Due to adhesion loss, residue and other reasons, the accuracy of regulating the nitrogen content of the aluminum nitride powder is affected.

[0094] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for regulating the carbon content in aluminum nitride, characterized in that: include: The glucose alcohol solution is mixed with aluminum nitride powder and ball milled to obtain a uniformly mixed slurry; Drying the slurry to obtain dry powder; The dry powder is heat treated under vacuum or inert atmosphere to adjust the carbon content in aluminum nitride.

2. The method for regulating the carbon content in aluminum nitride according to claim 1, characterized in that: The heat treatment temperature is 600-1500°C, and the holding time is 15-60 minutes.

3. The method for regulating the carbon content in aluminum nitride according to claim 1, characterized in that: The inert atmosphere is one of nitrogen or argon; Alternatively, the glucose alcohol solution is a solution of glucose in anhydrous ethanol.

4. The method for regulating the carbon content in aluminum nitride according to claim 1, characterized in that: The mass ratio of glucose alcohol solution to aluminum nitride powder is 40.99:0.1-0.

3.

5. The method for controlling the carbon content in aluminum nitride according to claim 1, characterized in that: After the glucose alcohol solution and the aluminum nitride powder are mixed, ball milling is performed, and the ball milling speed is 250-350r / min; more preferably, the ball-to-material ratio is 3-5:1, and the ball milling time is 20-28h.

6. The method for regulating the carbon content in aluminum nitride according to claim 1, characterized in that: The ball milling is wet ball milling.

7. The method for controlling the carbon content in aluminum nitride according to claim 1, characterized in that: The drying is vacuum drying at a temperature of 35-45°C.

8. Aluminum nitride, characterized in that: The aluminum nitride is prepared by the method for regulating the carbon content in aluminum nitride as described in any one of claims 1 to 7.

9. Use of the method for regulating the carbon content in aluminum nitride according to any one of claims 1 to 7 in the preparation of aluminum nitride.

Citation Information

Patent Citations

  • Aluminum nitride powder and preparation method thereof

    CN117776735A