Wear-resistant high-temperature-resistant environment-friendly anti-static film and preparation method thereof
Through specific formula and processing technology, a highly transparent wear-resistant, high-temperature-resistant, environmentally friendly and anti-static film is prepared, which solves the problem of insufficient transparency of existing films and achieves stability and transparency at high temperatures.
Patent Information
- Application Number
- CN202411085252.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-10-25
AI Technical Summary
Existing wear-resistant and high-temperature environmentally friendly anti-static films lack transparency and are unable to remain clear and transparent in high-temperature environments due to the addition of heat-resistant agents.
Use 40-60 parts by weight of polyurethane resin, 40-60 parts by weight of polyester resin, 18-22 parts by weight of hindered phenolic antioxidant, 8-12 parts by weight of auxiliary antioxidant, 25-35 parts by weight of Light stabilizer, 18-22 parts by weight of plant fiber Vitamin, 0.5-1 parts by weight of silicon nitride, 0.8-3 parts by weight of polyacrylonitrile, 2-6 parts by weight of epoxy resin and 1-5 parts by weight of dimethylacetamide, through specific stirring and Pressure treatment, combined with parallel twin-screw extrusion and plastic blown film technology to prepare films.
It improves the transparency and heat resistance of the film, inhibits oxidation reaction and light degradation, maintains the light transmittance and mechanical properties of the film, and avoids yellowing.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of chemical material product preparation, and in particular to a wear-resistant and high-temperature-resistant environmentally friendly antistatic film and a preparation method thereof. Background Art
[0002] Wear-resistant and high-temperature resistant environmentally friendly anti-static film is a special polyethylene (PE resin) film that has been specially designed and processed to withstand use in high-temperature environments. It is often used for items that need to be packaged or protected at high temperatures, such as food, electronic products, etc.
[0003] The wear-resistant and high-temperature resistant environmentally friendly antistatic film in the prior art also has the following disadvantage of insufficient transparency: due to the need to add additives such as heat-resistant agents, the transparency of the wear-resistant and high-temperature resistant environmentally friendly antistatic film may be affected and is not as clear as ordinary PE film. Summary of the invention
[0004] Based on the above shortcomings, the present invention provides a wear-resistant and high-temperature resistant environmentally friendly antistatic film and a preparation method thereof. The wear-resistant and high-temperature resistant environmentally friendly antistatic film has high transparency and is not easy to yellow. The contents of the present invention are as follows;
[0005] The first object of the present invention is to provide an environmentally friendly antistatic film that is wear-resistant and high-temperature resistant. The technical point is that, in terms of weight parts, it includes 40-60 parts by weight of polyurethane resin, 40-60 parts by weight of polyester resin, 18-22 parts by weight of hindered phenol antioxidant, 8-12 parts by weight of auxiliary antioxidant, 25-35 parts by weight of light stabilizer, 18-22 parts by weight of plant cellulose, 0.5-1 parts by weight of silicon nitride, 0.8-3 parts by weight of polyacrylonitrile, 2-6 parts by weight of epoxy resin, 1-5 parts by weight of dimethylacetamide and 1-5 parts by weight of oxidized cellulose.
[0006] In order to better realize the above technical scheme, the PE resin in the wear-resistant and high-temperature-resistant environmentally friendly antistatic film formula system of the present invention is any one of LDPE resin and LLDPE resin.
[0007] In order to better realize the above technical scheme, the hindered phenol antioxidant in the wear-resistant and high-temperature resistant environmentally friendly antistatic film formula system of the present invention is at least one of tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]pentaerythritol ester and its derivatives and N,N-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl)hexanediamine and its derivatives.
[0008] In order to better realize the above technical scheme, the auxiliary antioxidant in the wear-resistant and high-temperature-resistant environmentally friendly antistatic film formula system of the present invention is at least one of thioester type DSTP, TPL and phosphite type 168.
[0009] In order to better realize the above technical scheme, the light stabilizer in the wear-resistant and high-temperature resistant environmentally friendly antistatic film formula system of the present invention is at least one of styrene-methacrylate (2,2,6,6-tetramethylpiperidinyl), tris(2,2,6,6-methyl-4-piperidinylnitroxide) phosphite and tris(1,2,2,6,6-pentamethylpiperidinyl) phosphite.
[0010] The second object of the present invention is to provide a method for preparing a wear-resistant and high-temperature-resistant environmentally friendly antistatic film, the technical point of which is that it comprises the following steps:
[0011] Step 1, placing PE resin, hindered phenol antioxidant, auxiliary antioxidant, light stabilizer, plant cellulose and silicon nitride in a reaction kettle for stirring, the stirring temperature is controlled at 120-140° C., the stirring time is controlled at 50-70 min, then cooling to 40° C., continuing stirring for 20 min, and the stirring rate is controlled at 120-150 rpm, to obtain a mixture A;
[0012] Step 2, heating the reactor in step 1 to 150-170° C., adding polyacrylonitrile, epoxy resin, dimethylacetamide and oxidized cellulose to mixture A, pressurizing at 1.2-1.4 MPa, stirring for 70-90 min, and stirring at 200-240 rpm, and then standing and cooling to room temperature to obtain mixture B;
[0013] Step 3, filtering the mixture B obtained in step 2, introducing it into a parallel twin-screw extruder for extrusion granulation and drying to obtain a masterbatch;
[0014] Step 4, introducing the masterbatch obtained in step 3 into a plastic film blowing machine, and blowing it up with compressed air, cooling it with an air ring, and shaping it with a plate press, and then winding it up with a traction roller to obtain a wear-resistant and high-temperature resistant environmentally friendly antistatic film;
[0015] Step 5: Test the wear-resistant and high-temperature-resistant environmentally friendly antistatic film obtained in step 4, and then put it into a packaging machine for overall packaging.
[0016] Compared with the prior art, the wear-resistant and high-temperature-resistant environmentally friendly antistatic film and the preparation method thereof of the present invention can achieve the following beneficial effects:
[0017] The invention discloses a wear-resistant and high-temperature resistant environmentally friendly antistatic film, comprising PE resin, hindered phenol antioxidant, auxiliary antioxidant, light stabilizer, plant cellulose, silicon nitride, polyacrylonitrile, epoxy resin, dimethylacetamide and oxidized cellulose. The invention adds hindered phenol antioxidant to PE resin, which can effectively inhibit the oxidation reaction of polymer at high temperature, thereby improving the heat resistance and stability of the film and maintaining the light transmittance; the auxiliary antioxidant and hindered phenol antioxidant synergistically act to further enhance the antioxidant effect, and they also help to maintain the light transmittance of the PE film; the light stabilizer can effectively inhibit the degradation reaction of the polymer under light, such as the auto-oxidation reaction triggered by ultraviolet rays; the plant cellulose is a natural reinforcing agent, which can improve the heat resistance and mechanical properties of plastics; silicon nitride is a ceramic material with excellent heat resistance and chemical stability. DETAILED DESCRIPTION
[0018] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the specific embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0019] Example 1
[0020] A wear-resistant and high-temperature resistant environmentally friendly antistatic film includes 100 kg of PE resin, 20 kg of hindered phenol antioxidant, 10 kg of auxiliary antioxidant, 30 kg of light stabilizer, 20 kg of plant cellulose, 0.75 kg of silicon nitride, 1.9 kg of polyacrylonitrile, 4 kg of epoxy resin, 3 kg of dimethylacetamide and 3 kg of oxidized cellulose.
[0021] Furthermore, the PE resin in the wear-resistant and high-temperature-resistant environmentally friendly antistatic film formulation system of this embodiment is LDPE resin.
[0022] Furthermore, the hindered phenol antioxidant in the wear-resistant and high-temperature-resistant environmentally friendly antistatic film formulation system of this embodiment is pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate and its derivatives.
[0023] Furthermore, the auxiliary antioxidant in the wear-resistant and high-temperature-resistant environmentally friendly antistatic film formulation system of this embodiment is thioester-type DSTP.
[0024] Furthermore, the light stabilizer in the wear-resistant and high-temperature-resistant environmentally friendly antistatic film formulation system of this embodiment is styrene-methacrylic acid (2,2,6,6-tetramethylpiperidinyl).
[0025] According to the above formula, the preparation method of a wear-resistant and high-temperature-resistant environmentally friendly antistatic film of this embodiment includes the following steps:
[0026] Step 1, placing PE resin, hindered phenol antioxidant, auxiliary antioxidant, light stabilizer, plant cellulose and silicon nitride in a reaction kettle for stirring, the stirring temperature is controlled at 130° C., the stirring time is controlled at 60 min, then the temperature is lowered to 40° C., stirring is continued for 20 min, and the stirring rate is controlled at 135 rpm to obtain a mixture A;
[0027] Step 2, heating the reactor in step 1 to 160° C., adding polyacrylonitrile, epoxy resin, dimethylacetamide and oxidized cellulose to mixture A, pressurizing at 1.3 MPa, stirring time at 80 min, and stirring rate at 220 rpm, then standing and cooling to room temperature to obtain mixture B;
[0028] Step 3, filtering the mixture B obtained in step 2, introducing it into a parallel twin-screw extruder for extrusion granulation and drying to obtain a masterbatch;
[0029] Step 4, introducing the masterbatch obtained in step 3 into a plastic film blowing machine, and blowing it up with compressed air, cooling it with an air ring, and shaping it with a plate press, and then winding it up with a traction roller to obtain a wear-resistant and high-temperature resistant environmentally friendly antistatic film;
[0030] Step 5: Test the wear-resistant and high-temperature-resistant environmentally friendly antistatic film obtained in step 4, and then put it into a packaging machine for overall packaging.
[0031] Example 2
[0032] A wear-resistant and high-temperature resistant environmentally friendly antistatic film includes 80kg of PE resin, 18kg of hindered phenol antioxidant, 8kg of auxiliary antioxidant, 25kg of light stabilizer, 18kg of plant cellulose, 0.5kg of silicon nitride, 0.8kg of polyacrylonitrile, 2kg of epoxy resin, 1kg of dimethylacetamide and 1kg of oxidized cellulose.
[0033] Furthermore, the PE resin in the wear-resistant and high-temperature-resistant environmentally friendly antistatic film formulation system of this embodiment is LLDPE resin.
[0034] Furthermore, the hindered phenol antioxidant in the wear-resistant and high-temperature-resistant environmentally friendly antistatic film formulation system of this embodiment is N,N-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl)hexanediamine and its derivatives.
[0035] Furthermore, the auxiliary antioxidant in the wear-resistant and high-temperature-resistant environmentally friendly antistatic film formulation system of this embodiment is TPL.
[0036] Furthermore, the light stabilizer in the wear-resistant and high-temperature-resistant environmentally friendly antistatic film formulation system of this embodiment is tris(1,2,2,6,6-pentamethylpiperidinyl)phosphite.
[0037] According to the above formula, the preparation method of a wear-resistant and high-temperature-resistant environmentally friendly antistatic film of this embodiment includes the following steps:
[0038] Step 1, placing PE resin, hindered phenol antioxidant, auxiliary antioxidant, light stabilizer, plant cellulose and silicon nitride in a reaction kettle for stirring, the stirring temperature is controlled at 120° C., the stirring time is controlled at 70 min, then the temperature is lowered to 40° C., stirring is continued for 20 min, and the stirring rate is controlled at 120 rpm to obtain a mixture A;
[0039] Step 2, heating the reactor in step 1 to 150° C., adding polyacrylonitrile, epoxy resin, dimethylacetamide and oxidized cellulose to mixture A, pressurizing at 1.2 MPa, stirring time at 70 min, and stirring rate at 200 rpm, then standing and cooling to room temperature to obtain mixture B;
[0040] Step 3, filtering the mixture B obtained in step 2, introducing it into a parallel twin-screw extruder for extrusion granulation and drying to obtain a masterbatch;
[0041] Step 4, introducing the masterbatch obtained in step 3 into a plastic film blowing machine, and blowing it up with compressed air, cooling it with an air ring, and shaping it with a plate press, and then winding it up with a traction roller to obtain a wear-resistant and high-temperature resistant environmentally friendly antistatic film;
[0042] Step 5: Test the wear-resistant and high-temperature-resistant environmentally friendly antistatic film obtained in step 4, and then put it into a packaging machine for overall packaging.
[0043] Example 3
[0044] A wear-resistant and high-temperature resistant environmentally friendly antistatic film includes 120kg of PE resin, 22kg of hindered phenol antioxidant, 12kg of auxiliary antioxidant, 35kg of light stabilizer, 22kg of plant cellulose, 1kg of silicon nitride, 3kg of polyacrylonitrile, 6kg of epoxy resin, 5kg of dimethylacetamide and 5kg of oxidized cellulose.
[0045] Furthermore, the PE resin in the wear-resistant and high-temperature-resistant environmentally friendly antistatic film formulation system of this embodiment is a mixture of LDPE resin and LLDPE resin, wherein the weight ratio of LDPE resin to LLDPE resin is 1:1.
[0046] Furthermore, the hindered phenol antioxidant in the wear-resistant and high-temperature resistant environmentally friendly antistatic film formula system of this embodiment is a mixture of tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]pentaerythritol ester and its derivatives and N,N-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl)hexanediamine and its derivatives, wherein the weight ratio of tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]pentaerythritol ester and its derivatives and N,N-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl)hexanediamine and its derivatives is 1:1.
[0047] Furthermore, the auxiliary antioxidant in the wear-resistant and high-temperature-resistant environmentally friendly antistatic film formulation system of this embodiment is phosphite 168.
[0048] Furthermore, the light stabilizer in the wear-resistant and high-temperature-resistant environmentally friendly antistatic film formulation system of this embodiment is tris(1,2,2,6,6-pentamethylpiperidinyl)phosphite.
[0049] According to the above formula, the preparation method of a wear-resistant and high-temperature-resistant environmentally friendly antistatic film of this embodiment includes the following steps:
[0050] Step 1, placing PE resin, hindered phenol antioxidant, auxiliary antioxidant, light stabilizer, plant cellulose and silicon nitride in a reaction kettle for stirring, the stirring temperature is controlled at 140° C., the stirring time is controlled at 50 min, then cooling to 40° C., continuing stirring for 20 min, and the stirring rate is controlled at 150 rpm, to obtain a mixture A;
[0051] Step 2, heating the reactor in step 1 to 170° C., adding polyacrylonitrile, epoxy resin, dimethylacetamide and oxidized cellulose to mixture A, pressurizing at 1.4 MPa, stirring time at 90 min, and stirring rate at 240 rpm, then standing and cooling to room temperature to obtain mixture B;
[0052] Step 3, filtering the mixture B obtained in step 2, introducing it into a parallel twin-screw extruder for extrusion granulation and drying to obtain a masterbatch;
[0053] Step 4, introducing the masterbatch obtained in step 3 into a plastic film blowing machine, and blowing it up with compressed air, cooling it with an air ring, and shaping it with a plate press, and then winding it up with a traction roller to obtain a wear-resistant and high-temperature resistant environmentally friendly antistatic film;
[0054] Step 5: Test the wear-resistant and high-temperature-resistant environmentally friendly antistatic film obtained in step 4, and then put it into a packaging machine for overall packaging.
[0055] Comparative Example 1
[0056] The “100 kg PE resin, 20 kg hindered phenol antioxidant, 10 kg auxiliary antioxidant, 30 kg light stabilizer, 20 kg plant cellulose, 0.75 kg silicon nitride, 1.9 kg polyacrylonitrile, 4 kg epoxy resin, 3 kg dimethylacetamide and 3 kg oxidized cellulose” in Example 1 is changed to “100 kg PE resin, 30 kg hindered phenol antioxidant, 30 kg light stabilizer, 20 kg plant cellulose, 0.75 kg silicon nitride, 1.9 kg polyacrylonitrile, 4 kg epoxy resin, 3 kg dimethylacetamide and 3 kg oxidized cellulose”, and the remaining operations are the same as Example 1.
[0057] Comparative Example 2
[0058] The “100 kg PE resin, 20 kg hindered phenol antioxidant, 10 kg auxiliary antioxidant, 30 kg light stabilizer, 20 kg plant cellulose, 0.75 kg silicon nitride, 1.9 kg polyacrylonitrile, 4 kg epoxy resin, 3 kg dimethylacetamide and 3 kg oxidized cellulose” in Example 1 is changed to “100 kg PE resin, 20 kg hindered phenol antioxidant, 10 kg auxiliary antioxidant, 30 kg light stabilizer, 20.75 kg plant cellulose, 1.9 kg polyacrylonitrile, 4 kg epoxy resin, 3 kg dimethylacetamide and 3 kg oxidized cellulose”, and the remaining operations are the same as in Example 1.
[0059] Test example
[0060] The wear-resistant and high-temperature-resistant environmentally friendly antistatic films prepared in Examples 1-3 and Comparative Examples 1-2 were tested for performance. The PE films were aged at 60° C. for 48 hours, and the change rates of tensile strength and elongation at break of the PE films before and after the aging were detected. The test results are shown in Table 1:
[0061] Table 1
[0062] Tensile strength / % Elongation at break / % transparency Example 1 4.6 7.2 No yellowing Example 2 5.0 6.0 No yellowing Example 3 5.5 7.1 No yellowing Comparative Example 1 3.9 5.0 Slight yellowing Comparative Example 2 3.8 4.7 The taste turns yellow
[0063] The above description is only an embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent substitution, improvement, etc. made within the spirit and principle of the present invention should be included in the scope of the claims of the present invention.
Claims
1. A wear-resistant and high temperature resistant environmentally friendly antistatic film, characterized in that: In parts by weight, the invention comprises 40-60 parts by weight of polyurethane resin, 40-60 parts by weight of polyester resin, 18-22 parts by weight of hindered phenol antioxidant, 8-12 parts by weight of auxiliary antioxidant, 25-35 parts by weight of light stabilizer, 18-22 parts by weight of plant cellulose, 0.5-1 parts by weight of silicon nitride, 0.8-3 parts by weight of polyacrylonitrile, 2-6 parts by weight of epoxy resin, 1-5 parts by weight of dimethylacetamide and 1-5 parts by weight of oxidized cellulose, 35-45 parts by weight of modified conductive polyaniline fiber, 10-20 parts by weight of high temperature melting polyvinyl chloride, 8-15 parts by weight of polycarbonate, 3-10 parts by weight of silane coupling agent, 5-8 parts by weight of solvent oil, 12-18 parts by weight of tourmaline powder, 6-15 parts by weight of biomass carbon powder and 15-20 parts by weight of phenolic epoxy resin.
2. The wear-resistant and high-temperature-resistant environmentally friendly antistatic film according to claim 1, characterized in that: The solid content of the polyurethane resin is 44-46 wt %.
3. The wear-resistant and high-temperature-resistant environmentally friendly antistatic film according to claim 1, characterized in that: The polyester resin is at least one of polyethylene terephthalate, polybutylene terephthalate and polyarylate.
4. The wear-resistant and high-temperature-resistant environmentally friendly antistatic film according to claim 1, characterized in that: The hindered phenol antioxidant is at least one of tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]pentaerythritol ester and its derivatives and N,N-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl)hexanediamine and its derivatives.
5. The wear-resistant and high-temperature-resistant environmentally friendly antistatic film according to claim 1, characterized in that: The auxiliary antioxidant is at least one of thioester-type DSTP, TPL and phosphite 168.
6. The wear-resistant and high-temperature-resistant environmentally friendly antistatic film according to claim 1, characterized in that: The light stabilizer is at least one of styrene-methacrylate (2,2,6,6-tetramethylpiperidinyl), tris(2,2,6,6-methyl-4-piperidinylnitroxide) phosphite and tris(1,2,2,6,6-pentamethylpiperidinyl) phosphite.
7. The wear-resistant and high-temperature-resistant environmentally friendly antistatic film according to claim 1, characterized in that: The plant cellulose is any one of straw, corn cob and coconut shell.
8. A method for preparing a wear-resistant and high-temperature-resistant environmentally friendly antistatic film, characterized in that: The following steps are involved: Step 1, placing PE resin, hindered phenol antioxidant, auxiliary antioxidant, light stabilizer, plant cellulose and silicon nitride in a reaction kettle for stirring, the stirring temperature is controlled at 120-140° C., the stirring time is controlled at 50-70 min, then cooling to 40° C., continuing stirring for 20 min, and the stirring rate is controlled at 120-150 rpm, to obtain a mixture A; Step 2, heating the reactor in step 1 to 150-170° C., adding polyacrylonitrile, epoxy resin, dimethylacetamide and oxidized cellulose to mixture A, pressurizing at 1.2-1.4 MPa, stirring for 70-90 min, and stirring at 200-240 rpm, and then standing and cooling to room temperature to obtain mixture B; Step 3, filtering the mixture B obtained in step 2, introducing it into a parallel twin-screw extruder for extrusion granulation and drying to obtain a masterbatch; Step 4, introducing the masterbatch obtained in step 3 into a plastic film blowing machine, and blowing it up with compressed air, cooling it with an air ring, and shaping it with a plate press, and then winding it up with a traction roller to obtain a wear-resistant and high-temperature resistant environmentally friendly antistatic film; Step 5: Test the wear-resistant and high-temperature-resistant environmentally friendly antistatic film obtained in step 4, and then put it into a packaging machine for overall packaging.