Preparation method of aluminum alloy micro-arc oxidation-chemical plating Ni / P electromagnetic shielding coating
By performing micro-arc oxidation and electroless Ni/P plating on the aluminum alloy surface, combined with stearic acid modification, the problem of insufficient electromagnetic shielding performance of the aluminum alloy micro-arc oxidation coating was solved, and efficient electromagnetic shielding performance improvement and Enhanced long-term stability, suitable for applications in complex environments.
Patent Information
- Application Number
- CN202410972067.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2044-07-19
AI Technical Summary
Existing aluminum alloy micro-arc oxidation coatings have deficiencies in electromagnetic shielding performance and are difficult to effectively apply in complex environments, and conductive nanoparticles are difficult to construct a complete conductive network in the electrolyte.
Micro-arc oxidation technology is used to grow a porous alumina coating in situ on the surface of the aluminum alloy, and electroless Ni/P plating is performed on the coating surface, combined with stearic acid modification to enhance the magnetism and conductivity of the coating, thereby improving the electromagnetic Shielding performance.
The electromagnetic shielding performance of the aluminum alloy micro-arc oxidation coating is significantly improved. The self-corrosion current density reaches 6.054×10-8A/cm2, and the electromagnetic shielding efficiency is higher than 60dB, which meets the application in harsh environments and is improved through stearic acid modification. improve the long-term stability of the coating.
Smart Images

Figure CN118835243A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of aluminum alloy surface protective coatings, and in particular to a method for preparing an aluminum alloy micro-arc oxidation-chemical Ni / P electromagnetic shielding coating. Background Art
[0002] With the rapid development of wireless communication technology, electromagnetic waves as a medium for information transmission have been integrated into people's lives. However, the electromagnetic radiation pollution generated by electromagnetic waves has a serious impact on communication security, human health and the ecological environment. Therefore, the prevention and control of electromagnetic radiation problems have become increasingly important. The development of efficient electromagnetic interference shielding materials can effectively reduce electromagnetic wave pollution.
[0003] Aluminum alloy, as the matrix of electromagnetic shielding materials, has the characteristics of low density and high strength. The mechanical properties, wear resistance and corrosion resistance can be effectively improved by preparing micro-arc oxidation porous coatings. However, the high insulation of micro-arc oxidation coatings will have a certain impact on the dielectric loss of electromagnetic waves. In order to improve the electromagnetic shielding performance of ceramic coatings, it is necessary to introduce conductive and magnetic particles into the coatings. Magnetic metal particles have excellent conductivity and magnetic loss properties, which can effectively improve the electromagnetic shielding performance and increase the absorption loss efficiency. However, it is difficult to construct a complete conductive network by adding conductive nanoparticles to the electrolyte. Therefore, it is crucial to combine the micro-arc oxidation process with other processes to improve the electromagnetic shielding performance.
[0004] CN 105039981 A discloses a method for improving the performance of lamp radiators. The patent prepares a heat dissipation composite coating by preparing micro-arc oxidation and spraying graphene. The graphene spraying aqueous solvent is used, but the dispersion of graphene in the solvent is very poor and it is easy to agglomerate, which has limited effect on improving the conductivity of the coating. CN 107460515 A discloses a method for preparing a micro-arc oxidation-chemical nickel plating composite coating. The process first micro-arc oxidation on the surface of an aluminum alloy to form a micro-arc oxidation ceramic coating, and then chemically plating nickel to form a composite coating, which improves the wear and corrosion resistance of the aluminum alloy and enables the composite coating to have a certain conductivity. However, the coating cannot effectively improve the electromagnetic shielding performance and is difficult to apply in a complex service environment.
[0005] Therefore, designing a coating with excellent electromagnetic shielding performance has important research value and significance. Summary of the invention
[0006] The purpose of the present invention is to improve the electromagnetic shielding performance of aluminum alloy micro-arc oxidation coatings, and to provide a method for preparing aluminum alloy micro-arc oxidation-chemical Ni / P electromagnetic shielding coatings. The present invention first uses micro-arc oxidation technology to in-situ grow a porous aluminum oxide coating on the surface of the aluminum alloy to improve the corrosion resistance and mechanical properties of the aluminum alloy; and chemically plates Ni / P on the surface of the coating to improve the magnetism and conductivity of the aluminum oxide ceramic coating, and improve the electromagnetic shielding performance of the coating. Finally, the coating surface is modified by stearic acid to enhance the long-term stability of the electromagnetic shielding coating. The present invention improves the electromagnetic shielding performance of aluminum alloy micro-arc oxidation coatings, meeting the application of aluminum alloys in the field of electromagnetic shielding under harsh environments.
[0007] To achieve the above object, the present invention is implemented according to the following technical solutions:
[0008] A method for preparing an aluminum alloy micro-arc oxidation-chemical plating Ni / P electromagnetic shielding coating, the method comprising the following steps:
[0009] Step 1: The aluminum alloy sample is treated with 400#~2000# sandpaper and then ultrasonically cleaned with anhydrous ethanol and acetone for 10~20min respectively;
[0010] Step 2: placing the aluminum alloy sample in an alkaline electrolyte and preparing the micro-arc oxidation coating using a double-pulse DC power supply;
[0011] Among them, the alkaline electrolyte contains Na 2 SiO 3 9H 2 O、(NaPO 3 ) 6 and NaOH aqueous solution, Na 2 SiO 3 9H 2 O concentration is 5-30 g / L, (NaPO 3 ) 6 The concentration is 2-15 g / L, and the NaOH concentration is 0.5-5 g / L;
[0012] Current density is 1~20A / dm 2 , frequency is 100-1000Hz, duty cycle is 10-50%, time is 5-30min, electrolyte temperature is controlled at 20-50℃;
[0013] Step 3: Immerse the micro-arc oxidation sample obtained in step 2 in a sensitizing solution for 1 to 5 minutes, and rinse the remaining liquid with deionized water; the sensitizing solution is composed of 1 to 3 g / L SnCl 2 ;
[0014] Step 4: Activate the sample in the activation solution for 20 to 50 seconds, and rinse the remaining liquid with deionized water; the composition of the activation solution is 0.5 to 1 g / L PdCl 2 ;
[0015] Step 5: Then, reduce the sample in the reducing solution for 10 to 90 seconds, take it out and rinse the remaining liquid with deionized water; the reducing solution is composed of 10 to 40 g / L NaH 2 PO 2 ·H 2 O;
[0016] Step 6: Finally, chemical plating is performed in a water bath; the chemical plating solution is 10-40 g / L NiSO 4 6H 2 O, 10~50g / LNaH 2 PO 2 ·H 2 O, 10-30 g / L NH 4 Cl, 10~40g / LC 4 H 5 Na 3 O 7 , 0.001~1g / L CH 4 N 2 S; pH is 9-11; bath temperature is 70-90°C, time is 5-60min;
[0017] Step 7: Soak the workpiece obtained in step 6 in a stearic acid ethanol solution, the concentration of the stearic acid ethanol solution is 0.1-1 mol / L, the solution temperature is 50-70°C, the soaking time is 1-8h, and the composite coating is obtained after taking out and drying.
[0018] The aluminum alloy is specifically 6061 aluminum alloy, 7075 aluminum alloy or 1060 aluminum alloy;
[0019] The self-corrosion potential of the composite coating is -0.502 to -0.444 V, and the self-corrosion current density is 3.718×10 -6 ~6.054×10 -8 A / cm 2 The electromagnetic shielding effectiveness in the X-band (8.2-12.4 GHz) is 45-70 dB.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] 1. The present invention firstly adopts the micro-arc oxidation process to in-situ generate porous Al on the surface of aluminum alloy 2 O 3The ceramic coating has a metallurgical bond with the substrate and alumina, which has high bonding strength and enhances the corrosion resistance of the aluminum alloy. After chemical plating of Ni / P on the surface of the micro-arc oxidation coating, the electromagnetic shielding performance is significantly improved.
[0022] 2. The aluminum alloy micro-arc oxidation-chemical Ni / P electromagnetic shielding composite coating of the present invention has excellent electromagnetic shielding performance, and the electromagnetic shielding effectiveness is higher than 60dB, which is higher than the commercial standard; it has excellent corrosion resistance (self-corrosion current density is 6.054×10 -8 A / cm 2 ). And after being modified with stearic acid, the long-term stability of the electromagnetic shielding performance of the coating is increased.
[0023] 3. The coating prepared by the present invention has excellent comprehensive performance, can be applied to a variety of complex environments, and has good application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to more clearly illustrate the technical solutions of the exemplary embodiments of the present invention, the following briefly introduces the drawings required to describe the embodiments. Obviously, the drawings introduced are only drawings of a part of the embodiments to be described in the present invention, rather than all the drawings. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0025] Figure 1 It is a flow chart of the method for preparing the aluminum alloy micro-arc oxidation-chemical plating Ni / P electromagnetic shielding coating in Example 1 of the present invention;
[0026] Figure 2 is a SEM image of the aluminum alloy micro-arc oxidation-chemical Ni / P electromagnetic shielding composite coating (P1) in Example 1 of the present invention and the micro-arc oxidation treatment (MAO) in Comparative Example 1; wherein, Figure 2 (a) Surface morphology of micro-arc oxidation coating; Figure 2 (b) Surface morphology of aluminum alloy micro-arc oxidation-chemical plating Ni / P electromagnetic shielding composite coating;
[0027] Figure 3 is an XRD diagram of the aluminum alloy micro-arc oxidation electromagnetic shielding composite coating (P1) in Example 1 of the present invention and after micro-arc oxidation treatment (MAO) in Comparative Example 1; wherein, Figure 3 (a) is the XRD pattern of micro-arc oxidation coating; Figure 3 (b) is the XRD pattern of aluminum alloy micro-arc oxidation-chemical plating Ni / P electromagnetic shielding composite coating;
[0028] Figure 4 Polarization curves of the aluminum alloy micro-arc oxidation-chemical Ni / P electromagnetic shielding composite coating (P1) in Example 1 of the present invention and the micro-arc oxidation treatment (MAO) in Comparative Example 1;
[0029] Figure 5 The electromagnetic shielding stability of the aluminum alloy micro-arc oxidation-chemical plating Ni / P electromagnetic shielding composite coating (P1) in Example 3 of the present invention and the unmodified electromagnetic shielding coating (P2) in Comparative Example 2 after immersion for 96 hours. DETAILED DESCRIPTION
[0030] The present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention, rather than to limit the scope of protection of the present invention.
[0031] Example 1
[0032] 1. A method for preparing an aluminum alloy micro-arc oxidation-chemical plating Ni / P electromagnetic shielding coating, comprising the following steps:
[0033] Step 1: The size is 10.20×22.32×1mm 3 The 6061 aluminum alloy was treated with 400#, 1000#, and 2000# sandpapers in turn, and ultrasonically cleaned with anhydrous ethanol and acetone for 20 min respectively;
[0034] Step 2: Place the aluminum alloy sample in a solution containing 15 g / L Na 2 SiO 3 9H 2 O, 5g / L (NaPO 3 ) 6 The micro-arc oxidation coating was prepared by double pulse DC power supply in alkaline electrolyte containing 1g / L NaOH. The electrical parameters of the micro-arc oxidation process are: current density of 10A / dm 2 , frequency is 500Hz, duty cycle is 30%, time is 10min, and electrolyte temperature is controlled at 30℃.
[0035] Step 3: Immerse the micro-arc oxidation sample obtained in step 2 in the sensitizing solution for 1 min, and rinse the residual liquid with deionized water; the sensitizing solution composition is 1g / L SnCl 2 ;
[0036] Step 4: Activate the sample in the activation solution for 20 seconds and rinse the remaining liquid with deionized water. The composition of the activation solution is 0.5g / L PdCl 2 ;
[0037] Step 5: Then, the sample was reduced in the reducing solution for 60 seconds, and the residual liquid was rinsed with deionized water after removal. The reducing solution was composed of 30 g / L NaH 2 PO 2 ·H 2 O.
[0038] Step 6: Perform chemical plating in a water bath. The chemical plating solution is 30g / L NiSO 4 6H 2 O, 20g / LNaH 2 PO 2 ·H 2 O, 15 g / L NH 4 Cl, 20g / LC 4 H 5 Na 3 O 7 , 0.003g / L CH 4 N 2 S; pH is 9; bath temperature is 70°C; time is 10 min.
[0039] Step 7: Soak the sample obtained in step 6 in a stearic acid ethanol solution, the concentration of the stearic acid ethanol solution is 0.5 mol / L, the solution temperature is 60° C., the soaking time is 3 h, and after drying, an electromagnetic shielding composite coating is obtained.
[0040] 2. Sample testing
[0041] The surface morphology of aluminum alloy micro-arc oxidation-chemical Ni / P electromagnetic shielding composite coating and micro-arc oxidation coating was observed by focused ion beam scanning electron microscopy (such as Figure 2 The micro-arc oxidation coating consists of crater-shaped micropores. After chemical plating, nickel particles are evenly attached to the surface of the ceramic coating. Figure 3 The diffraction peak of nickel was observed (as shown in the figure), confirming that magnetic nickel particles existed in the coating.
[0042] The electrochemical corrosion test of the sample was carried out using an electrochemical workstation. The self-corrosion potential of the composite coating obtained in this embodiment was -0.495 V, and the self-corrosion current density was 2.359×10 -6 A / cm 2 Compared with the samples only subjected to micro-arc oxidation, the self-corrosion potential shifted positively, the self-corrosion current density decreased, and the corrosion resistance improved (e.g. Figure 4 shown).
[0043] The electromagnetic shielding effectiveness in the X-band (8.2-12.4 GHz) was tested using a vector network analyzer and the result was 54.8 dB, which is 20 dB higher than the commercial standard.
[0044] Example 2
[0045] The other steps are the same as those in Example 1, except that the chemical plating time in step 6 is 30 min;
[0046] The self-corrosion potential is -0.480 V and the self-corrosion current density is 2.902×10-7 A / cm 2 The electromagnetic shielding effectiveness in the X-band (8.2-12.4 GHz) is 58.4 dB, which is 20 dB higher than the commercial standard.
[0047] Example 3
[0048] The other steps are the same as those in Example 1, except that the chemical plating time in step 6 is 60 minutes.
[0049] The self-corrosion potential is -0.444V and the self-corrosion current density is 6.054×10 -8 A / cm 2 The electromagnetic shielding effectiveness in the X-band (8.2-12.4 GHz) is 68.6 dB, which is higher than the commercial standard (20 dB). After immersion in a 3.5 wt. % NaCl solution for 96 hours, the electromagnetic shielding performance is 59.3 dB, with strong stability (such as Figure 5 shown).
[0050] Comparative Example 1
[0051] The other steps are the same as those in Example 1, except that steps 3, 4, 5, 6, and 7 are removed, that is, the aluminum alloy workpiece is only subjected to micro-arc oxidation treatment.
[0052] The self-corrosion potential is -0.671 V and the self-corrosion current density is 3.872×10 -7 A / cm 2 The electromagnetic shielding effectiveness in the X-band (8.2-12.4 GHz) is 29.5 dB, which is higher than the commercial standard (20 dB).
[0053] Comparative Example 2
[0054] The other steps are the same as those in Example 3, except that step 7 is removed, i.e., the composite coating is not modified with stearic acid.
[0055] The self-corrosion potential is -0.455 V and the self-corrosion current density is 7.650×10 -7 A / cm 2 The electromagnetic shielding effectiveness in the X-band (8.2-12.4 GHz) is 68.5 dB, which is higher than the commercial standard (20 dB). After immersion in a 3.5 wt. % NaCl solution for 96 h, the electromagnetic shielding performance is 41.7 dB, and the stability is poor.
[0056] Note that the above are only preferred embodiments of the present invention and the technical principles used. Those skilled in the art will understand that the present invention is not limited to the specific embodiments described herein, and that various obvious changes, readjustments and substitutions can be made by those skilled in the art without departing from the scope of protection of the present invention. Therefore, although the present invention has been described in more detail through the above embodiments, the present invention is not limited to the above embodiments, and may include more other embodiments without departing from the concept of the present invention, and the scope of the present invention is determined by the scope of the appended claims.
[0057] Matters not covered by the present invention are known technologies.
Claims
1. A method for preparing an aluminum alloy micro-arc oxidation-chemical Ni / P electromagnetic shielding coating, characterized in that the method comprises the following steps: Step 1: Grind and clean the aluminum alloy sample; Step 2: placing the aluminum alloy sample in an alkaline electrolyte and preparing a micro-arc oxidation coating using a double-pulse DC power supply; in, Alkaline electrolyte contains Na 2 SiO 3 9H 2 O、(NaPO 3 ) 6 and NaOH aqueous solution, Na 2 SiO 3 9H 2 O concentration is 5-30 g / L, (NaPO 3 ) 6 The concentration is 2-15 g / L, and the NaOH concentration is 0.5-5 g / L; Current density is 1~20A / dm 2 , frequency is 100-1000Hz, duty cycle is 10-50%, time is 5-30min, electrolyte temperature is controlled at 20-50℃; Step 3: Immerse the micro-arc oxidation sample obtained in step 2 in a sensitizing solution for 1 to 5 minutes, and rinse the remaining liquid with deionized water; the sensitizing solution is composed of 1 to 3 g / L SnCl 2 ; Step 4: Activate the sample in the activation solution for 20 to 50 seconds, and rinse the remaining liquid with deionized water; the composition of the activation solution is 0.5 to 1 g / L PdCl 2 ; Step 5: Then, reduce the sample in the reducing solution for 10 to 90 seconds, take it out and rinse the remaining liquid with deionized water; the reducing solution is composed of 10 to 40 g / L NaH 2 PO 2 ·H 2 O; Step 6: Perform chemical plating in a water bath; the chemical plating solution is 10-40g / L NiSO 4 6H 2 O, 10~50g / LNaH 2 PO 2 ·H 2 O, 10-30 g / L NH 4 Cl, 10~40g / LC 4 H 5 Na 3 O 7 , 0.001~1g / L CH 4 N 2 S; pH is 9-11; bath temperature is 70-90°C, time is 5-60min; Step 7: Soak the workpiece obtained in step 6 in a stearic acid ethanol solution, the concentration of the stearic acid ethanol solution is 0.1-1 mol / L, the solution temperature is 50-70° C., the soaking time is 1-8 hours, and the composite coating is obtained after taking out and drying.
2. The method for preparing the aluminum alloy micro-arc oxidation-chemical Ni / P electromagnetic shielding coating according to claim 1, Its characteristics are The aluminum alloy is specifically 6061 aluminum alloy, 7075 aluminum alloy or 1060 aluminum alloy.
3. The method for preparing an aluminum alloy micro-arc oxidation-chemical plating Ni / P electromagnetic shielding coating as described in claim 1 is characterized in that the polishing is performed by water polishing with 400# to 2000# sandpaper; and the cleaning is performed by ultrasonic cleaning with anhydrous ethanol and acetone in sequence for 10 to 20 minutes.
4. The method for preparing an aluminum alloy micro-arc oxidation-chemical Ni / P electromagnetic shielding coating as claimed in claim 1, wherein the self-corrosion potential of the composite coating is -0.502 to -0.444 V, and the self-corrosion current density is 3.718×10 -6 ~6.054×10 -8 A / cm 2 The electromagnetic shielding effectiveness in the X-band (8.2-12.4 GHz) is 45-70 dB.
Citation Information
Patent Citations
Method for improving fatigue strength after microarc oxidation of aluminium alloy
CN101914798A
Aluminum product and preparation method thereof
CN103144370A
Preparation method for aluminum alloy micro-arc oxidation-electroless nickel-plating composite coating
CN107460515A
Method for preparing aluminum-based layered shielding material
CN108930053A
Wheel surface oxidation-resistant treatment method
CN109487270A
Cited By
Method for preparing super-hydrophobic coating on surface of aluminum alloy
CN119663393A
High-voltage aluminum bar for new energy automobile and preparation method of high-voltage aluminum bar
CN120221160A
A high-pressure aluminum bar for new energy vehicles and its preparation method
CN120221160B