High-strength saturated paper tube base paper and preparation process thereof

By using a combination of softened water and specific auxiliary materials such as cationic polyacrylamide and polyethyleneimine, the absorption capacity and surface smoothness of the paper tube base paper are improved, and the problem of insufficient absorption capacity of the existing paper tube base paper is solved. High strength and high cleanliness paper tube preparation is achieved.

CN118835482AActive Publication Date: 2024-10-25ZHONGTIAN PAPER

Patent Information

Application Number
CN202411235095.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-10-25
Estimated Expiration
2044-09-04

AI Technical Summary

Technical Problem

The existing paper tube base paper has low resin absorption capacity and low absorption uniformity. As a result, the surface smoothness and cleanliness of the paper tube prepared after hot extrusion are not high, and it cannot meet the high requirements of optical grade films for film rolled paper tubes.

Method used

Demineralized water that has undergone water softening treatment is used to prepare paper pulp, and cationic polyacrylamide is added as a dry strength agent and polyethylenimine as a wet strength agent in the process. Through specific process steps and material combinations, the absorption capacity of the paper tube is improved. and surface smoothness.

Benefits of technology

It achieves high absorption capacity and absorption uniformity on the surface of the paper tube, ensures the smoothness and cleanliness of the paper tube surface after hot extrusion, meets the requirements of optical grade films, and improves the strength and stability of the paper tube.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118835482A_ABST
    Figure CN118835482A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of papermaking, and particularly relates to high-strength saturated paper tube base paper and a preparation process thereof. The preparation process of the high-strength saturated paper tube body paper comprises the following steps: softening with clear water, preparing paper pulp, mixing the pulp, adding auxiliary materials and papermaking. The quantification of the high-strength saturated paper tube raw paper is 200 + / -5g / m < 2 >, 240 + / -5g / m < 2 > or 280 + / -5g / m < 2 >, the longitudinal dry tensile index is greater than or equal to 130N. M / g, the longitudinal wet tensile strength is greater than or equal to 30N. M / g, the longitudinal ring crush index is greater than or equal to 17N. M / g, the interlayer bonding strength is greater than or equal to 300J / m < 2 >, the burst index is greater than or equal to 3.2 Kpa. M < 2 > / g, the smoothness is greater than or equal to 10s, the moisture is 6.2-6.8%, the water absorption height is greater than or equal to 70mm / 10min, and the banner quantification difference is less than or equal to 1.2%. The high-strength saturated paper tube raw paper has the beneficial effects that the high-strength saturated paper tube raw paper has extremely high absorption capacity and absorption uniformity on resin when being used for preparing a paper tube, so that the surface smoothness of the paper tube prepared after the resin is extruded is high.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of papermaking, and in particular relates to a high-strength saturated paper tube base paper and a preparation process thereof. Background Art

[0002] At present, paper tubes are increasingly used in different industries and fields, and the materials in different fields have more and more performance requirements for paper tubes. Among them, optical-grade films have higher requirements for film-rolled paper tubes. Because the main processing technology of optical-grade films is coating, if there are stripes on the surface of the film-rolled paper tube during coating, there will be coating leaks, which will then produce waste products. Therefore, optical-grade films have extremely high requirements for the smoothness of the surface of the film-rolled paper tube; and optical films have high requirements for cleanliness, so the base paper and production process of the film-rolled paper tube need to be kept clean; at the same time, the film-rolled paper tube of the optical film is prepared by coating the surface with resin and then hot extruding, but the existing paper tube base paper has low absorption capacity and absorption uniformity for resin, which makes the surface smoothness of the paper tube prepared after hot extrusion low. Therefore, it is necessary to develop a high-strength saturated paper tube base paper that can ensure the smoothness and cleanliness of the paper tube surface. Summary of the invention

[0003] In view of the above problems, the present invention provides a high-strength saturated paper tube base paper and a preparation process thereof.

[0004] The present invention relates to a preparation process of high-strength saturated paper tube base paper, and the specific steps are as follows: a. Softening of clean water: Soften clean water to obtain softened water; b. Preparing pulp: using the softened water to pulp the mixed wood pulp, and then entering the pre-beating pool after pulping. The pulp in the pre-beating pool is screened by a pressure screen, purified by a slag remover, and concentrated, and then refined by a double disc mill, and then enters the post-beating pool; c. Slurry adjustment: the slurry in the post-beating tank enters the slurry preparation tank after concentration adjustment, and the slurry in the slurry preparation tank enters the pre-scaling tank after secondary concentration adjustment; d. Adding auxiliary materials: dry strength agent and wet strength agent are added to the slurry in the pre-sieving tank in sequence, and then pumped to the white water tower and the slurry pump in sequence through the slurry pump, and a penetrant is added before the slurry pump; e. Papermaking: After adding auxiliary materials, the pulp passes through the headbox, wire section, press section, drying section, and calender in sequence. After calendering, it is wound and rewound, and after packaging, high-strength saturated paper tube base paper is obtained.

[0005] Preferably, in step a, the clean water is softened by using Na2CO3; the hardness of the softened water is 50-70 mg / L.

[0006] Preferably, in step b, the mixed wood pulp is a mixture of 20-30 mass parts of unbleached sulfate coniferous wood pulp and 70-80 mass parts of unbleached sulfate broadleaf wood pulp; the pulping concentration is 4.0-5.0%; the refining concentration is 5.5-6.5%, the refining beating degree is 30-40°SR, and the pulp inlet pressure is 0.15-0.20 MPa.

[0007] Preferably, in step b, the pressure screen is a single-drum outflow rotor pressure screen, which adopts a one-stage two-stage arrangement; the slag remover is a high-pressure differential conical slag remover, which adopts a one-stage three-stage arrangement, is used in series, and is installed in a vertical column.

[0008] Preferably, in the step c, after the slurry in the post-beating tank is concentrated, it is pumped to the slurry preparation tank via a slurry lifting pump, and the slurry concentration in the slurry preparation tank is 4.5-5.0%; after the slurry in the slurry preparation tank is concentrated for the second time, it is pumped to the pre-sweeping tank via a slurry lifting pump, and the slurry concentration in the pre-sweeping tank is 3.0-3.5%.

[0009] Preferably, in step d, the dry strength agent is cationic polyacrylamide, which is diluted 10 times by an online dilution device and then continuously added to the pre-scraping tank; the wet strength agent is polyethyleneimine, which is continuously added to the pre-scraping tank by a metering pump; and the penetrant is a surface-active penetrant, which is continuously added in front of the slurry pump by a metering pump.

[0010] Preferably, in step d, the amount of the dry strength agent added is 30-35 kg per ton of paper; the amount of the wet strength agent added is 1.8-2.2 kg per ton of paper.

[0011] Preferably, in steps b, c, d and e, the clean water used is treated in step a.

[0012] Preferably, before implementing steps b, c, d and e, the preparation system is thoroughly rinsed with the softened water.

[0013] The present invention also relates to a high-strength saturated paper tube base paper, which is prepared by using the high-strength saturated paper tube base paper preparation process, wherein the basis weight of the high-strength saturated paper tube base paper is 200±5g / ㎡, 240±5g / ㎡ or 280±5g / ㎡; The high-strength saturated paper tube base paper has a longitudinal dry tensile index of ≥130 N·m / g, a longitudinal wet tensile strength of ≥30 N·m / g, and a longitudinal ring compression index of ≥17 N·m / g; The interlayer bonding strength of the high-strength saturated paper tube base paper is ≥300 J / ㎡, and the bursting index is ≥3.2 Kpa·㎡ / g; The high-strength saturated paper tube base paper has a smoothness of ≥10s and a moisture content of 6.2-6.8%; The water absorption height of the high-strength saturated paper tube base paper is ≥70mm / 10min, and the cross-section quantitative difference is ≤1.2%.

[0014] Compared with the prior art, the advantages and positive effects of the present invention are: (1) The clean water used in the preparation process of the high-strength saturated paper tube base paper is replaced by softened water that has undergone specific treatment, and the hardness of the softened water is controlled within a specific range, thereby preventing impurities in the clean water from entering the paper tube base paper. As a result, the high-strength saturated paper tube base paper has extremely high absorption capacity and absorption uniformity for the resin when preparing the paper tube, so that the paper tube obtained after the resin is extruded has excellent surface smoothness and cleanliness; (2) The preparation process of the high-strength saturated paper tube base paper uses cationic polyacrylamide as a dry strength agent, which can avoid the dependence of the dry strength agent on the cationic promoter, thereby using aluminum sulfate and polyaluminum chloride to reduce the absorbency of the base paper. Therefore, the high-strength saturated paper tube base paper improves the dry strength while ensuring that the absorption capacity and absorption uniformity of the resin are not affected, so that the surface smoothness and strength of the prepared tube paper are relatively high; (3) The preparation process of the high-strength saturated paper tube base paper uses polyethyleneimine as a wet strength agent, which can produce wet strength without aging, effectively reducing the risk of paper breaking in the wet end of the paper machine and improving the stability of the high-strength saturated paper tube base paper during preparation; (4) The raw material of the high-strength saturated paper tube base paper is a mixture of unbleached kraft coniferous wood pulp and unbleached kraft broadleaf wood pulp. Since the raw material is 100% wood pulp, the fiber quality is uniform and stable, so the high-strength saturated paper tube base paper has high cleanliness, good uniformity and high smoothness. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] In order to more clearly illustrate the technical solution of the embodiment of the present invention, the following is a brief introduction to the drawings required for describing the embodiment: Figure 1 This is a process flow chart for preparing the high-strength saturated paper tube base paper provided in Example 1. DETAILED DESCRIPTION

[0016] In order to more clearly understand the above-mentioned objects, features and advantages of the present invention, the present invention is further described below with reference to the accompanying drawings and embodiments.

[0017] In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention may also be implemented in other ways than those described herein. Therefore, the present invention is not limited to the specific embodiments of the following disclosure.

[0018] Example 1 The following is combined with Figure 1The present invention is further described as follows: a process for preparing a high-strength saturated paper tube base paper; the specific steps are as follows: a. Softening of clean water: Soften clean water to obtain softened water; b. Preparation of pulp: Use softened water to pulp the mixed wood pulp, and then enter the pre-beating pool. The pulp in the pre-beating pool is screened by a pressure screen, purified by a slag remover, and concentrated, and then refined by a double disc mill. After refining, it enters the post-beating pool; c. Slurry preparation: The slurry in the post-beating tank enters the slurry preparation tank after concentration adjustment. The slurry in the slurry preparation tank enters the pre-scaling tank after secondary concentration adjustment. d. Adding auxiliary materials: dry strength agent and wet strength agent are added to the slurry in the forewater pool in sequence, and then pumped to the white water tower and flushing pump in sequence through the slurry pump, and the penetrant is added before the flushing pump; e. Papermaking: After adding auxiliary materials, the pulp passes through the headbox, wire section, press section, drying section, and calender in sequence. After calendering, it is wound and rewound, and after packaging, high-strength saturated paper tube base paper is obtained.

[0019] In step a, Na2CO3 is used to soften the clean water; the hardness of the softened water is 50 mg / L.

[0020] In step b, the mixed wood pulp is a mixture of 30 parts by mass of unbleached sulfate coniferous pulp and 70 parts by mass of unbleached sulfate broadleaf pulp; the pulping concentration is 5.0%; the refining concentration is 6.5%, the refining beating degree is 40°SR, and the pulp inlet pressure is 0.18Mpa.

[0021] In step b, the pressure screen is a single-drum outflow rotor pressure screen, which adopts a one-stage two-stage arrangement; the slag remover is a high-pressure differential conical slag remover, which adopts a one-stage three-stage arrangement, is used in series, and is installed in a vertical column.

[0022] In step c, after the slurry in the post-beating tank is adjusted in concentration, it is pumped to the slurry mixing tank by the slurry lifting pump, and the slurry concentration in the slurry mixing tank is 5.0%; after the slurry in the slurry mixing tank is adjusted in concentration for the second time, it is pumped to the pre-sweeping tank by the slurry lifting pump, and the slurry concentration in the pre-sweeping tank is 3.5%.

[0023] In step d, the dry strength agent is cationic polyacrylamide, which is diluted 10 times by an online dilution device and continuously added to the pre-slurry tank; the wet strength agent is polyethyleneimine, which is continuously added to the pre-slurry tank by a metering pump; the penetrant is a surfactant penetrant, which is continuously added in front of the slurry pump by a metering pump.

[0024] In step d, the amount of dry strength agent added is 32 kg per ton of paper; the amount of wet strength agent added is 2.0 kg per ton of paper.

[0025] In steps b, c, d and e, the clean water used is treated in step a.

[0026] Before implementing steps b, c, d, and e, the preparation system is thoroughly rinsed with softened water.

[0027] The main indicators of the high-strength saturated paper tube base paper prepared by the above-mentioned preparation process were tested, and the results are shown in Table 1.

[0028] Table 1 The "Standard Value" column in Table 1 is the standard value of each indicator of high-strength saturated paper tube base paper.

[0029] The "Test Value" column in Table 1 is the average test value of each index of the high-strength saturated paper tube base paper after multiple tests.

[0030] From Table 1, we can conclude that: The basis weight of the above-mentioned high-strength saturated paper tube base paper is 202g / ㎡; the moisture content is 6.6%; the smoothness is 13.5s; the longitudinal ring compression index is 18.2N·m / g; the interlayer bonding strength is 341J / ㎡; the longitudinal dry tensile index is 132N·m / g; the longitudinal wet tensile strength is 33N·m / g; the bursting index is 3.27Kpa·㎡ / g; the water absorption height is 78mm / 10min, and the cross-sectional basis weight difference is 1.13%.

[0031] The basis weight, moisture content, smoothness, longitudinal ring compression index, interlayer bonding strength, longitudinal dry tensile index, longitudinal wet tensile index, bursting index, water absorption height and cross-sectional basis weight difference of the high-strength saturated paper tube base paper all meet the standard requirements, and it is proved that the high-strength saturated paper tube base paper has a high absorption capacity, as well as high smoothness, dry strength and wet strength.

[0032] The above description is only a preferred embodiment of the present invention and does not limit the present invention in other forms. Any technician familiar with the profession may use the technical content disclosed above to change or modify it into an equivalent embodiment with equivalent changes for application in other fields. However, any simple modification or equivalent change made to the above embodiment based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A process for preparing high-strength saturated paper tube base paper, characterized in that: The specific steps are as follows: a. Softening of clean water: Soften clean water to obtain softened water; b. Preparing pulp: using the softened water to pulp the mixed wood pulp, and then entering the pre-beating pool after pulping. The pulp in the pre-beating pool is screened by a pressure screen, purified by a slag remover, and concentrated, and then refined by a double disc mill, and then enters the post-beating pool; c. Slurry adjustment: the slurry in the post-beating tank enters the slurry preparation tank after concentration adjustment, and the slurry in the slurry preparation tank enters the pre-scaling tank after secondary concentration adjustment; d. Adding auxiliary materials: dry strength agent and wet strength agent are added to the slurry in the pre-sieving tank in sequence, and then pumped to the white water tower and the slurry pump in sequence through the slurry pump, and a penetrant is added before the slurry pump; e. Papermaking: After adding auxiliary materials, the pulp passes through the headbox, wire section, press section, drying section, and calender in sequence. After calendering, it is wound and rewound, and after packaging, high-strength saturated paper tube base paper is obtained.

2. The process for preparing high-strength saturated paper tube base paper according to claim 1, characterized in that: In the step a, the clean water is softened by using Na2CO3; the hardness of the softened water is 50-70 mg / L.

3. The process for preparing high-strength saturated paper tube base paper according to claim 1, characterized in that: In the step b, the mixed wood pulp is a mixture of 20 to 30 parts by mass of unbleached kraft coniferous wood pulp and 70 to 80 parts by mass of unbleached kraft broadleaf wood pulp; the pulping concentration is 4.0 to 5.0%; the refining concentration is 5.5 to 6.5%, the refining beating degree is 30 to 40°SR, and the pulp inlet pressure is 0.15 to 0.20 MPa.

4. The process for preparing high-strength saturated paper tube base paper according to claim 1, characterized in that: In step b, the pressure screen is a single-drum outflow rotor pressure screen, which adopts a one-stage two-stage arrangement; the slag remover is a high-pressure differential conical slag remover, which adopts a one-stage three-stage arrangement, is used in series, and is installed in a vertical column.

5. The process for preparing high-strength saturated paper tube base paper according to claim 1, characterized in that: In the step c, after the slurry in the post-beating tank is adjusted in concentration, it is pumped to the slurry preparation tank through a slurry lifting pump, and the slurry concentration in the slurry preparation tank is 4.5-5.0%; after the slurry in the slurry preparation tank is adjusted in concentration for the second time, it is pumped to the pre-sweeping tank through a slurry lifting pump, and the slurry concentration in the pre-sweeping tank is 3.0-3.5%.

6. The process for preparing high-strength saturated paper tube base paper according to claim 1, characterized in that: In the step d, the dry strength agent is cationic polyacrylamide, which is diluted 10 times by an online dilution device and then continuously added to the pre-scraping tank; the wet strength agent is polyethyleneimine, which is continuously added to the pre-scraping tank by a metering pump; the penetrant is a surface-active penetrant, which is continuously added in front of the slurry pump by a metering pump.

7. The process for preparing high-strength saturated paper tube base paper according to claim 1, characterized in that: In the step d, the amount of the dry strength agent added is 30-35 kg per ton of paper; the amount of the wet strength agent added is 1.8-2.2 kg per ton of paper.

8. The process for preparing high-strength saturated paper tube base paper according to claim 1, characterized in that: In steps b, c, d and e, the clean water used is treated by step a.

9. The process for preparing high-strength saturated paper tube base paper according to claim 1, characterized in that: Before implementing the steps b, c, d and e, the preparation system is thoroughly rinsed with the softened water.

10. A high-strength saturated paper tube base paper, characterized in that: The high-strength saturated paper tube base paper is prepared by the preparation process of the high-strength saturated paper tube base paper according to any one of claims 1 to 9, wherein the basis weight of the high-strength saturated paper tube base paper is 200±5g / ㎡, 240±5g / ㎡ or 280±5g / ㎡; The high-strength saturated paper tube base paper has a longitudinal dry tensile index of ≥130 N·m / g, a longitudinal wet tensile strength of ≥30 N·m / g, and a longitudinal ring compression index of ≥17 N·m / g; The interlayer bonding strength of the high-strength saturated paper tube base paper is ≥300 J / ㎡, and the bursting index is ≥3.2 Kpa·㎡ / g; The high-strength saturated paper tube base paper has a smoothness of ≥10s and a moisture content of 6.2-6.8%; The water absorption height of the high-strength saturated paper tube base paper is ≥70mm / 10min, and the cross-section quantitative difference is ≤1.2%.

Citation Information

Patent Citations

  • Cultural paper

    CN102978998A

  • Method for making lignocellulosic paper and paper products

    CN108138439A

  • High-voltage cable paper with high insulating property and tightness and production method thereof

    CN108735403A

  • Surface layer polishing base paper and preparation process thereof

    CN113089358A

  • Preparation method of decorative base paper with uniformly distributed titanium dioxide

    CN117306298A

Cited By

  • Device for improving drying efficiency through online punching of raw paper of paper tube