Super-hydrophilic ultrathin vapor chamber

By using a modified polyacrylic acid fullerene super hydrophilic coating on a super hydrophilic ultra-thin vapor chamber, the problem of low efficiency of traditional heat dissipation components under high power and high heat flux density is solved, and efficient heat exchange and Ultra-thin heat dissipation effect of vapor chamber.

CN118836718APending Publication Date: 2024-10-25SUZHOU REHAN TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411126185.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

Traditional heat dissipation components cannot effectively solve the heat transfer problem when facing high power and high heat flux density, and the heat dissipation performance of super hydrophilic vapor chambers suffers from continuous attenuation and slow reflow of working fluid.

Method used

A super hydrophilic and ultra-thin soaking plate is designed, which uses an evaporation plate, a sealing frame and a condensation plate to form a closed cavity. The cavity is filled with liquid working fluid, and the bottom and side walls of the condensation plate are equipped with dense inverted square-shaped reflux blocks and reflux columns. , the surface is coated with a modified polyacrylic acid fullerene super-hydrophilic coating to improve the liquid return speed and heat transfer efficiency.

Benefits of technology

Through the use of modified polyacrylic acid fullerene super-hydrophilic coating, the liquid return speed and heat transfer efficiency are significantly improved, achieving efficient heat exchange and ultra-thin heat dissipation effect of the vapor chamber.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118836718A_ABST
    Figure CN118836718A_ABST
Patent Text Reader

Abstract

The super-hydrophilic ultrathin vapor chamber comprises an evaporation plate, a frame sealing frame and a condensation plate, the condensation plate and the evaporation plate are fixedly connected to the upper side and the lower side of the frame sealing frame respectively, a closed cavity is formed in the evaporation plate, the frame sealing frame and the condensation plate, and the cavity is filled with a liquid working medium. A plurality of densely arranged backflow blocks are fixedly connected to the bottom side wall of the condensation plate, each backflow block is arranged in an inverted quadrangular shape, the bottom end of each backflow block is fixedly connected with a backflow column, the bottom end of each backflow column is fixedly connected to the upper side of the evaporation plate, and the side walls of the backflow blocks and the side walls of the backflow columns are coated with super-hydrophilic coatings. The super-hydrophilic coating comprises a bottom layer and a surface layer. The super-hydrophilic coatings based on the modified polyacrylic fullerene are arranged on the surfaces of the backflow block and the backflow column, so that the liquid backflow speed can be increased, the heat transfer efficiency is improved, heat exchange is accelerated, the overall structure is simple, and ultrathin and efficient heat dissipation of the vapor chamber can be achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of vapor chambers, and in particular to a super-hydrophilic ultra-thin vapor chamber. Background Art

[0002] With the rapid development of electronics, IT, communications, LED, solar energy and other industries, the heating power of the electronic components used is also increasing, and the heat flux density has increased significantly. It is difficult to solve the related heat transfer problems using traditional heat dissipation components.

[0003] Traditional heat dissipation mostly adopts a heat source plus heat sink cooling mode, dissipating heat through heat exchange between the heat sink and the air. However, due to limitations in structural space, material heat transfer characteristics, heat dissipation module weight, structural strength and reliability, traditional heat dissipation modes cannot meet heat dissipation requirements when encountering high power and high heat flux density.

[0004] The super-hydrophilic heat spreader is a vacuum cavity with a microstructure on the inner wall. It has become the development trend of integrated heat dissipation structure for high-power LEDs due to its high thermal conductivity, good temperature uniformity, thin thickness and easy integration. However, the heat dissipation performance of the heat sink still has problems such as continuous attenuation of heat dissipation capacity and slow reflux of working fluid. Summary of the invention

[0005] The present invention provides a super-hydrophilic ultra-thin vapor chamber to solve the problems raised in the above background technology.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] A super-hydrophilic ultra-thin heat spreader, comprising an evaporation plate, a sealing frame, and a condensation plate, wherein the condensation plate and the evaporation plate are fixedly connected to the upper and lower sides of the sealing frame respectively, and a closed cavity is formed inside the evaporation plate, the sealing frame, and the condensation plate, and the cavity is filled with a liquid working medium; a plurality of densely arranged reflux blocks are fixedly connected to the bottom side wall of the condensation plate, each of the reflux blocks is arranged in an inverted quadrangular shape, a reflux column is fixedly connected to the bottom end of each reflux block, and the bottom end of the reflux column is fixedly connected to the upper side of the evaporation plate; the side walls of the reflux blocks and the reflux columns are coated with a super-hydrophilic coating, and the super-hydrophilic coating comprises a bottom layer and a surface layer.

[0008] As a further improvement of the technical solution: the bottom layer is composed of the following components: 10-15 parts of cationic monomer, 5-10 parts of photoinitiator, 1-2 parts of crosslinking agent, and 80-100 parts of solvent.

[0009] As a further improvement of the technical solution: the surface layer is composed of the following ingredients: 8-15 parts of modified polyacrylic acid fullerene, 10-12 parts of photosensitive semiconductor, 6-9 parts of surfactant, and 80-100 parts of ethanol.

[0010] As a further improvement of the technical solution: the preparation steps of the modified polyacrylic acid fullerene include: dissolving fullerene, diisobutyronitrile and acrylic acid in toluene, then reacting for 24 hours under light-proof conditions, then evaporating the solution under reduced pressure and dissolving the product in anhydrous N,N-dimethylformamide, filtering to remove insoluble matter, and then dialyzing in anhydrous ethanol, using a semipermeable membrane to remove small molecular compounds with a molecular weight of less than 1000, and obtaining modified polyacrylic acid fullerene after removing anhydrous ethanol.

[0011] As a further improvement of the technical solution: the method of coating the super hydrophilic coating on the surface of the reflux block and the reflux column comprises the following steps:

[0012] 1) adding the cationic monomer and the crosslinking agent into a solvent and stirring them uniformly at room temperature to obtain a solution A;

[0013] 2) preparing a dispersion of modified polyacrylic acid fullerene and ethanol, adding a surfactant and stirring after ultrasonic stirring, then adding a photosensitive semiconductor, and continuing stirring at 50-80° C. for 2-10 hours to obtain a solution B;

[0014] 3) Add photoinitiator to solution A, mix well and apply to the surface of reflux block and reflux column, irradiate with ultraviolet light for 1-3 seconds for pre-curing, then apply solution B, irradiate with ultraviolet light for 1-3 seconds after coating to complete curing.

[0015] As a further improvement of the technical solution: the cationic monomer is a combination of one or more of dimethyldiallylammonium chloride, acryloyloxyethyldimethylbenzylammonium chloride, methacryloyloxyethyltrimethylammonium chloride, and acryloyloxyethyltrimethylammonium chloride.

[0016] As a further improvement of the technical solution: the photoinitiator is a combination of one or more of benzophenone, 2,4-dihydroxybenzophenone, α-aminoalkylphenone, and benzoin dimethyl ether.

[0017] As a further improvement of the technical solution: the surfactant is a combination of one or more of sodium dodecyl sulfate, octadecyltrimethylammonium bromide, and hexadecyltrimethylammonium bromide.

[0018] As a further improvement of the technical solution: the reflux block and the reflux column are both made of copper.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] The present invention can improve the liquid reflux speed, increase the heat transfer efficiency, accelerate the heat exchange by arranging a super-hydrophilic coating based on modified polyacrylic acid fullerene on the surface of the reflux block and the reflux column, and the overall structure is simple, which can realize ultra-thin and efficient heat dissipation of the heat spreader.

[0021] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention and implement it according to the contents of the specification, the following is a detailed description of the preferred embodiments of the present invention in conjunction with the accompanying drawings. The specific implementation of the present invention is given in detail by the following embodiments and their accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] The drawings described herein are used to provide a further understanding of the present invention and constitute a part of this application. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0023] Figure 1 A schematic diagram of the structure of a super-hydrophilic ultra-thin vapor chamber proposed by the present invention;

[0024] Figure 2 It is a schematic diagram of the structure of the dense reflux block on the surface of the condensation plate in the present invention;

[0025] Figure 3 A schematic diagram of the front cross-sectional structure of a super-hydrophilic ultra-thin vapor chamber proposed by the present invention;

[0026] Figure 4 Schematic diagram of the synthesis of modified polyacrylic acid fullerene proposed in the present invention.

[0027] In the accompanying drawings, the components represented by the reference numerals are listed as follows:

[0028] 1. Sealing frame; 2. Reflux column; 3. Evaporation plate; 4. Reflux block; 5. Condensation plate. DETAILED DESCRIPTION

[0029] The principles and features of the present invention are described below in conjunction with the accompanying drawings. The examples given are only used to explain the present invention and are not used to limit the scope of the present invention. The present invention is described in more detail by way of example with reference to the accompanying drawings in the following paragraphs. It should be noted that the accompanying drawings are all in a very simplified form and are not in precise proportions, and are only used to facilitate and clearly assist in explaining the purpose of the embodiments of the present invention.

[0030] It should be noted that when a component is referred to as being "fixed to" another component, it may be directly on the other component or there may also be a component centered. When a component is considered to be "connected to" another component, it may be directly connected to the other component or there may also be a component centered. When a component is considered to be "set on" another component, it may be directly set on the other component or there may also be a component centered. The terms "vertical", "horizontal", "left", "right" and similar expressions used herein are for illustrative purposes only.

[0031] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0032] See also Figures 1 to 4 In an embodiment of the present invention, a super-hydrophilic ultra-thin heat spreader includes an evaporation plate 3, a sealing frame 1, and a condensation plate 5. The condensation plate 5 and the evaporation plate 3 are fixedly connected to the upper and lower sides of the sealing frame 1, respectively. The evaporation plate 3, the sealing frame 1, and the condensation plate 5 form a closed cavity, and the cavity is filled with a liquid working medium. A plurality of densely arranged reflux blocks 4 are fixedly connected to the bottom side wall of the condensation plate 5, and each reflux block 4 is arranged in an inverted quadrangular shape. The inverted quadrangular shape can make the water on the reflux block 4 quickly and concentratedly flow to the reflux column 2, thereby improving the reflux effect of the working medium. The bottom end of each reflux block 4 is fixedly connected to the reflux column 2, and the bottom end of the reflux column 2 is fixedly connected to the upper side of the evaporation plate 3. The side walls of the reflux block 4 and the reflux column 2 are coated with a super-hydrophilic coating, and the super-hydrophilic coating includes a bottom layer and a surface layer.

[0033] The bottom layer is composed of the following ingredients: 10-15 parts of cationic monomer, 5-10 parts of photoinitiator, 1-2 parts of crosslinking agent, and 80-100 parts of solvent;

[0034] The surface layer is composed of the following ingredients: 8-15 parts of modified polyacrylic acid fullerene, 10-12 parts of photosensitive semiconductor, 6-9 parts of surfactant and 80-100 parts of ethanol.

[0035] Specifically, the cationic monomer is a combination of one or more of dimethyldiallylammonium chloride, acryloyloxyethyldimethylbenzylammonium chloride, methacryloyloxyethyltrimethylammonium chloride, and acryloyloxyethyltrimethylammonium chloride.

[0036] Specifically, the photoinitiator is a combination of one or more of benzophenone, 2,4-dihydroxybenzophenone, α-aminoalkylphenone, and benzoin dimethyl ether.

[0037] Specifically, the surfactant is a combination of one or more of sodium dodecyl sulfate, octadecyltrimethylammonium bromide, and hexadecyltrimethylammonium bromide.

[0038] Specifically, the reflux block 4 and the reflux column 2 are both made of copper.

[0039] Specifically, the preparation steps of the modified polyacrylic acid fullerene include: dissolving fullerene, diisobutylonitrile and acrylic acid in toluene, reacting for 24 hours under light-proof conditions, evaporating the solution under reduced pressure and dissolving the product in anhydrous N,N-dimethylformamide, filtering to remove insoluble matter, dialyzing in anhydrous ethanol, using a semipermeable membrane to remove small molecular compounds with a molecular weight of less than 1000, and obtaining the modified polyacrylic acid fullerene after removing the anhydrous ethanol.

[0040] The method of coating the super hydrophilic coating on the surface of the reflux block 4 and the reflux column 2 comprises the following steps:

[0041] 1) adding the cationic monomer and the crosslinking agent into a solvent and stirring them uniformly at room temperature to obtain a solution A;

[0042] 2) preparing a dispersion of modified polyacrylic acid fullerene and ethanol, adding a surfactant and stirring after ultrasonic stirring, then adding a photosensitive semiconductor, and continuing stirring at 50-80° C. for 2-10 hours to obtain a solution B;

[0043] 3) Add photoinitiator to solution A, mix well and apply to the surface of reflux block 4 and reflux column 2, irradiate with ultraviolet light for 1-3 seconds for pre-curing, then apply solution B, irradiate with ultraviolet light for 1-3 seconds after coating to complete curing.

[0044] Because the super-hydrophilic coating uses modified polyacrylic acid fullerene as a carrier of photosensitive semiconductors, it is used in the super-hydrophilic coating. Due to the huge specific surface area of ​​modified polyacrylic acid fullerene, a higher photosensitive semiconductor material load can be achieved, and it can be slowly released through sustained release, thereby extending the service life of the coating. At the same time, modified polyacrylic acid fullerene itself is a hydrophilic polymer, which further improves the hydrophilic effect of the super-hydrophilic coating.

[0045] The working principle of the present invention is:

[0046] When heat is conducted from the heat source to the evaporation plate 3, the liquid working medium in the cavity begins to vaporize after being heated in a low vacuum environment. When the gas phase working medium contacts the relatively cold condensation plate 5, it liquefies. The liquefied working medium can flow back to the evaporation plate 3 under the action of the reflux block 4 and the reflux column 2. This operation will be repeated in the cavity to continuously dissipate heat. Among them, the super-hydrophilic coating on the surface of the reflux block 4 and the reflux column 2 can increase the liquid reflux speed, increase the heat transfer efficiency, and accelerate the heat exchange.

[0047] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Any ordinary technician in the industry can smoothly implement the present invention as shown in the drawings and described above. However, any equivalent changes, modifications and evolutions made by technicians familiar with the profession without departing from the scope of the technical solution of the present invention using the technical content disclosed above are all equivalent embodiments of the present invention. At the same time, any equivalent changes, modifications and evolutions made to the above embodiments based on the essential technology of the present invention are still within the protection scope of the technical solution of the present invention.

Claims

1. A super-hydrophilic ultra-thin heat spreader, comprising an evaporation plate (3), a sealing frame (1), and a condensation plate (5), characterized in that: The condensation plate (5) and the evaporation plate (3) are respectively fixedly connected to the upper and lower sides of the sealing frame (1); the evaporation plate (3), the sealing frame (1) and the condensation plate (5) form a closed cavity inside; the cavity is filled with a liquid working medium; a plurality of densely arranged reflux blocks (4) are fixedly connected to the bottom side wall of the condensation plate (5); each of the reflux blocks (4) is arranged in an inverted quadrangular shape; a reflux column (2) is fixedly connected to the bottom end of each reflux block (4); the bottom end of the reflux column (2) is fixedly connected to the upper side of the evaporation plate (3); the side walls of the reflux blocks (4) and the reflux columns (2) are coated with a super-hydrophilic coating; the super-hydrophilic coating comprises a bottom layer and a surface layer.

2. The ultra-hydrophilic ultra-thin vapor chamber according to claim 1, characterized in that: The bottom layer is composed of the following ingredients: 10-15 parts of cationic monomer, 5-10 parts of photoinitiator, 1-2 parts of crosslinking agent and 80-100 parts of solvent.

3. The ultra-hydrophilic ultra-thin vapor chamber according to claim 1, characterized in that: The surface layer is composed of the following ingredients: 8-15 parts of modified polyacrylic acid fullerene, 10-12 parts of photosensitive semiconductor, 6-9 parts of surfactant and 80-100 parts of ethanol.

4. The ultra-hydrophilic ultra-thin vapor chamber according to claim 1, characterized in that: The preparation steps of the modified polyacrylic acid fullerene include: dissolving fullerene, diisobutylonitrile and acrylic acid in toluene, reacting for 24 hours under light-proof conditions, evaporating the solution under reduced pressure and dissolving the product in anhydrous N,N-dimethylformamide, filtering to remove insoluble matter, dialyzing in anhydrous ethanol, using a semipermeable membrane to remove small molecular compounds with a molecular weight of less than 1000, and obtaining the modified polyacrylic acid fullerene after removing the anhydrous ethanol.

5. The ultra-hydrophilic ultra-thin vapor chamber according to claim 1, characterized in that: The method for coating the super-hydrophilic coating on the surface of the reflux block (4) and the reflux column (2) comprises the following steps: 1) adding the cationic monomer and the crosslinking agent into a solvent and stirring them uniformly at room temperature to obtain a solution A; 2) preparing a dispersion of modified polyacrylic acid fullerene and ethanol, adding a surfactant and stirring after ultrasonic stirring, then adding a photosensitive semiconductor, and continuing stirring at 50-80° C. for 2-10 hours to obtain a solution B; 3) Adding a photoinitiator to solution A, mixing well, coating the solution on the surface of the reflux block (4) and the reflux column (2), irradiating the solution with ultraviolet light for 1-3 seconds for pre-curing, and then coating solution B, irradiating the solution with ultraviolet light for 1-3 seconds after coating, and completing curing.

6. The ultra-hydrophilic ultra-thin vapor chamber according to claim 1, characterized in that: The cationic monomer is a combination of one or more of dimethyldiallylammonium chloride, acryloyloxyethyldimethylbenzylammonium chloride, methacryloyloxyethyltrimethylammonium chloride and acryloyloxyethyltrimethylammonium chloride.

7. The ultra-hydrophilic ultra-thin vapor chamber according to claim 1, characterized in that: The photoinitiator is a combination of one or more of benzophenone, 2,4-dihydroxybenzophenone, α-aminoalkylphenone, and benzoin dimethyl ether.

8. The ultra-hydrophilic ultra-thin vapor chamber according to claim 1, characterized in that: The surfactant is a combination of one or more of sodium dodecyl sulfate, octadecyl trimethyl ammonium bromide, and hexadecyl trimethyl ammonium bromide.

9. The ultra-hydrophilic ultra-thin vapor chamber according to claim 1, characterized in that: The reflux block (4) and the reflux column (2) are both made of copper.