Copper inner electrode nonlinear multilayer ceramic capacitor and sintering method thereof

By debonding and sintering copper internal electrode nonlinear multilayer ceramic capacitors under an inert or reducing atmosphere, combined with specific sintering aids, the problem of co-firing of copper internal electrodes and antiferroelectric materials is solved, achieving high energy storage and insulation characteristics, simplifying the process and reducing costs.

CN118841260APending Publication Date: 2024-10-25SUZHOU SICUI ELECTRONIC FUNCTIONAL MATERIALS TECH RES INST CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411015256.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

The existing technology cannot effectively prepare the co-firing method of copper internal electrodes and antiferroelectric materials, resulting in an unknown sintering method for nonlinear multilayer ceramic capacitors with copper internal electrodes, and the Pb2+ in the dielectric material may be reduced, resulting in internal electrode materials and Media materials interpenetrate each other.

Method used

To debond and sinter copper internal electrode nonlinear multilayer ceramic capacitors under an inert or reducing atmosphere, use a mixed gas of nitrogen and hydrogen or carbon monoxide to control the sintering temperature and time, and add lead oxide, aluminum oxide, zinc oxide, boron oxide, Sintering aids such as potassium oxide ensure that the copper internal electrode is not oxidized and Pb2+ is not reduced.

Benefits of technology

The co-firing of the copper internal electrode and the PLZST nonlinear dielectric material is realized, which avoids the oxidation of the internal electrode and the reduction of the dielectric material, improves the energy storage characteristics and insulation characteristics, simplifies the process, reduces the cost, and provides help for industrialization.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004965507180000111
    Figure BDA0004965507180000111
  • Figure HDA0004965507190000011
    Figure HDA0004965507190000011
  • Figure HDA0004965507190000012
    Figure HDA0004965507190000012
Patent Text Reader

Abstract

The invention discloses a copper inner electrode non-linear multilayer ceramic capacitor and a sintering method thereof, and the method comprises the steps: carrying out the bonding of the copper inner electrode non-linear multilayer ceramic capacitor in an inert atmosphere or a reducing atmosphere, and obtaining a copper inner electrode non-linear multilayer ceramic capacitor green body; placing the obtained copper inner electrode nonlinear multilayer ceramic capacitor green body in a corundum crucible and covering the corundum crucible with ceramic powder; the ceramic capacitor green body covered with the ceramic powder is sintered in inert gas or reducing gas, the copper inner electrode nonlinear multilayer ceramic capacitor is obtained, and by means of the sintering method, the purposes that the copper inner electrode is not oxidized and lead ions are not reduced are achieved; the inner electrode is continuous and the dielectric layer is compact; the insulation resistance is kept at the order of magnitude of 1012 ohms; the dielectric loss is within 0.1; the breakdown electric field reaches 260 kV / cm, and the maximum polarization intensity reaches 34 [mu] C / cm < 2 >. According to the invention, the production cost is greatly reduced, and the industrial development of the copper inner electrode multilayer ceramic capacitor is promoted.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of ceramic capacitor preparation, and relates to a copper inner electrode nonlinear multilayer ceramic capacitor and a sintering method thereof. Background Art

[0002] As a key passive electronic component, multilayer ceramic capacitors are widely used in 5G communications, automotive electronics, smart wearables, aerospace and other scenarios, and are known as the "rice of the electronics industry". Antiferroelectric materials, as a nonlinear dielectric material, will undergo an "antiferroelectric-ferroelectric phase transition" under the action of an external electric field. Their dielectric constant increases with the increase of the external electric field, has a positive voltage coefficient, and has high energy storage density and efficiency. The current internal electrode materials used in multilayer ceramic capacitors are Ag / Pd or Ni. In contrast, copper, as a base metal material, has the lowest manufacturing cost, low resistivity, and good high-frequency characteristics. Therefore, copper internal electrode nonlinear multilayer ceramic capacitors have broad application prospects.

[0003] Currently, Japan's TDK company has sold copper inner electrode antiferroelectric multilayer ceramic capacitors as high-end products. However, domestic manufacturers have not yet sold any products, mainly because they have not found a method for co-firing antiferroelectric materials and copper inner electrodes. CN115947598A and CN116813337A introduced the sintering method of antiferroelectric ceramic materials in a reducing atmosphere, but they were not prepared into multilayer ceramic capacitors, so it is still unknown whether their sintering methods are suitable for copper inner electrode nonlinear multilayer ceramic capacitors. CN 117038334 A introduced a copper inner electrode MLCC and its sintering method, but the dielectric material used in the patent is a linear dielectric material (strontium calcium zirconate), and the dielectric material does not contain elements that can be reduced in a reducing atmosphere, so its co-firing method is not suitable for the lead-based antiferroelectric material of this patent.

[0004] Based on the above background, in order to prepare copper inner electrode nonlinear multilayer ceramic capacitors, it is necessary to independently overcome the co-firing problem and master the core technology. Summary of the invention

[0005] In order to overcome the defects of the prior art, the present invention provides a copper inner electrode nonlinear multilayer ceramic capacitor and a sintering method thereof, and provides a sintering method for a copper inner electrode nonlinear multilayer ceramic capacitor whose dielectric material is PLZST, so that the copper inner electrode material is not oxidized, and the Pb in the dielectric material is 2+ It is not reduced and has high energy storage and insulation properties.

[0006] In order to achieve the above object, the present invention adopts the following technical scheme: a sintering method of a copper inner electrode nonlinear multilayer ceramic capacitor, comprising the following steps:

[0007] Debonding the copper inner electrode nonlinear multilayer ceramic capacitor under an inert atmosphere or a reducing atmosphere to obtain a copper inner electrode nonlinear multilayer ceramic capacitor green body;

[0008] The obtained copper inner electrode nonlinear multilayer ceramic capacitor green body is placed in a corundum crucible and covered with ceramic powder;

[0009] The ceramic capacitor green body covered with ceramic powder is sintered in an inert gas or a reducing gas to obtain a copper inner electrode nonlinear multilayer ceramic capacitor.

[0010] Furthermore, the nonlinear ceramic material used in the copper inner electrode nonlinear multilayer ceramic capacitor is an antiferroelectric ceramic material, and the main crystal phase is lead lanthanum zirconium tin titanium.

[0011] Furthermore, the inert gas is nitrogen, and the reducing gas is hydrogen or carbon monoxide.

[0012] Furthermore, the volume ratio of reducing gas during debonding is nitrogen:hydrogen=1000:1, and the volume ratio of reducing gas during sintering is nitrogen:carbon monoxide=500:1-1000:1.

[0013] Furthermore, the temperature during the debonding is 300-400°C, the heat preservation time is 24-72h, the heating rate is 1°C / min, and the temperature is reduced to room temperature at a rate of 3°C / min.

[0014] Furthermore, the sintering temperature is 920-1050° C., the holding time is 2-4 h, the heating rate is 3° C. / min, and the temperature is lowered to room temperature at a rate of 3° C. / min.

[0015] Furthermore, the ceramic powder is the same as the dielectric material of the copper inner electrode nonlinear multilayer ceramic capacitor.

[0016] Furthermore, the nonlinear multilayer ceramic capacitor contains 2.6%wt-3.0%wt of a sintering aid, and the sintering aid is lead oxide, aluminum oxide, zinc oxide, boron oxide, potassium oxide or a plurality of others.

[0017] The present invention can also provide a copper inner electrode nonlinear multilayer ceramic capacitor, which is obtained by the above sintering method, wherein the copper inner electrode material of the copper inner electrode nonlinear multilayer ceramic capacitor is not oxidized, and the Pb in the dielectric material is not oxidized. 2+ It is not reduced, and there is no mutual penetration between the inner electrode material and the dielectric material.

[0018] Compared with the prior art, the present invention has the following beneficial effects: the sintering method adopted by the present invention successfully realizes the co-firing of the copper inner electrode material and the PLZST nonlinear dielectric material; the copper inner electrode material of the obtained copper inner electrode nonlinear multilayer ceramic capacitor is not oxidized, and the Pb in the dielectric material is 2+It has not been reduced, there is no mutual penetration between the inner electrode material and the dielectric material, and it has high energy storage characteristics and insulation characteristics; the sintering method is simple and easy to operate, and provides effective assistance to the industrialization of copper inner electrode nonlinear multilayer ceramic capacitors; it is unique, innovative and practical, which helps to significantly reduce the cost of multilayer ceramic capacitors and contribute to the development of the industry. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] The following figures / tables illustrate only certain embodiments of the present invention and therefore should not be considered limiting of the scope.

[0020] Figure 1 These are optical microscope images of Example 9 and Example 11.

[0021] Figure 2 The scanning electron microscope images and energy spectrum analysis images of Example 9 and Example 11 are shown.

[0022] Figure 3 2 are hysteresis loop diagrams of Example 9 and Example 11.

[0023] Figure 4 Graphs showing leakage currents of Examples 9 and 11. DETAILED DESCRIPTION

[0024] The present invention is described in further detail below:

[0025] A copper inner electrode nonlinear multilayer ceramic capacitor and a sintering method thereof, wherein the specific steps are as follows:

[0026] Step 1: lay a copper inner electrode nonlinear multilayer ceramic capacitor flat on an alumina plate, wherein the nonlinear ceramic material of the multilayer ceramic capacitor includes a main crystal phase of lead lanthanum zirconium tin titanium (PLZST) and a sintering aid, and the sintering aid is a variety of compositions of lead oxide, aluminum oxide, zinc oxide, boron oxide, and potassium oxide.

[0027] Step 2, debonding the sample obtained in step 1 in an atmosphere furnace to obtain a multilayer ceramic capacitor green body; wherein, the debonding temperature is 300-400°C, the holding time is 20-72h, the heating rate is 1°C / min, and the temperature is cooled to room temperature at a rate of 3°C / min. The debonding atmosphere is a mixed gas formed by an inert gas (nitrogen) and a reducing gas (hydrogen), and the gas volume ratio is nitrogen: hydrogen = 1000:1.

[0028] Step 3: placing the multilayer ceramic capacitor green body obtained in step 2 in a corundum crucible and covering it with ceramic powder of the same nonlinear ceramic material.

[0029] Step 4, sintering the sample obtained in step 3 in an atmosphere furnace to obtain a finished multilayer ceramic capacitor; wherein the sintering temperature is 920-1050°C, the holding time is 2-4h, the heating rate is 3°C / min, and the temperature is cooled to room temperature at a rate of 3°C / min. The atmosphere used is a mixed gas formed by an inert gas (nitrogen) and a reducing gas (carbon monoxide), and the gas volume ratio is nitrogen: carbon monoxide = 500:1-1000:1

[0030] The present invention is described in detail below in conjunction with the embodiments and drawings to facilitate a more comprehensive understanding of the present invention by those skilled in the art, but the present invention is not limited to the scope of all embodiments. All other embodiments obtained without creative work are within the scope of protection of the present invention.

[0031] Example 1

[0032] The nonlinear ceramic material used in the copper inner electrode nonlinear multilayer ceramic capacitor in this embodiment is a main crystal phase material PLZST and a sintering aid, and the amount of the sintering aid added is 0.5%wt lead oxide, 0.5%wt aluminum oxide, 1.0%wt boron oxide, and 0.8%wt potassium oxide. The copper inner electrode nonlinear multilayer ceramic capacitor prepared by the dielectric material is debonded in a mixed gas atmosphere formed by nitrogen and hydrogen. The specific preparation method is as follows:

[0033] Step 1: Lay a copper inner electrode nonlinear multilayer ceramic capacitor flat on an alumina plate, wherein the nonlinear ceramic material of the multilayer ceramic capacitor includes PLZST and lead oxide, aluminum oxide, boron oxide, and potassium oxide.

[0034] Step 2, debonding the sample obtained in step 1 in an atmosphere furnace to obtain a multilayer ceramic capacitor green body; wherein, the debonding temperature is 300°C, the holding time is 72h, the heating rate is 1°C / min, and the temperature is cooled to room temperature at a rate of 3°C / min. The debonding atmosphere is a mixed gas formed by an inert gas (nitrogen) and a reducing gas (hydrogen), and the gas volume ratio is nitrogen: hydrogen = 1000:1.

[0035] Example 2

[0036] The nonlinear ceramic material used in the copper inner electrode nonlinear multilayer ceramic capacitor in this embodiment is a main crystal phase material PLZST and a sintering aid, and the amount of the sintering aid added is 0.5%wt lead oxide, 0.5%wt aluminum oxide, 1.2%wt boron oxide, and 0.8%wt potassium oxide. The copper inner electrode nonlinear multilayer ceramic capacitor prepared by the dielectric material is debonded in a mixed gas atmosphere formed by nitrogen and hydrogen. The specific preparation method is as follows:

[0037] Step 1: Lay a copper inner electrode nonlinear multilayer ceramic capacitor flat on an alumina plate, wherein the nonlinear ceramic material of the multilayer ceramic capacitor includes PLZST and lead oxide, aluminum oxide, boron oxide, and potassium oxide.

[0038] Step 2, debonding the sample obtained in step 1 in an atmosphere furnace to obtain a multilayer ceramic capacitor green body; wherein, the debonding temperature is 350°C, the holding time is 48h, the heating rate is 1°C / min, and the temperature is cooled to room temperature at a rate of 3°C / min. The debonding atmosphere is a mixed gas formed by an inert gas (nitrogen) and a reducing gas (hydrogen), and the gas volume ratio is nitrogen:hydrogen = 1000:1.

[0039] Example 3

[0040] The nonlinear ceramic material used in the copper inner electrode nonlinear multilayer ceramic capacitor in this embodiment is a main crystal phase material PLZST and a sintering aid, and the amount of the sintering aid added is 0.5%wt lead oxide, 0.5%wt aluminum oxide, 1.2%wt boron oxide, and 0.8%wt potassium oxide. The copper inner electrode nonlinear multilayer ceramic capacitor prepared by the dielectric material is debonded in a mixed gas atmosphere formed by nitrogen and hydrogen. The specific preparation method is as follows:

[0041] Step 1: Lay a copper inner electrode nonlinear multilayer ceramic capacitor flat on an alumina plate, wherein the nonlinear ceramic material of the multilayer ceramic capacitor is composed of PLZST and sintering aids such as lead oxide, aluminum oxide, boron oxide, and potassium oxide.

[0042] Step 2, debonding the sample obtained in step 1 in an atmosphere furnace to obtain a multilayer ceramic capacitor green body; wherein, the debonding temperature is 400°C, the holding time is 24h, the heating rate is 1°C / min, and the temperature is cooled to room temperature at a rate of 3°C / min. The debonding atmosphere is a mixed gas formed by an inert gas (nitrogen) and a reducing gas (hydrogen), and the gas volume ratio is nitrogen:hydrogen = 1000:1.

[0043] Example 4

[0044] The nonlinear ceramic material used in the copper inner electrode nonlinear multilayer ceramic capacitor in this embodiment is a main crystal phase material PLZST and a sintering aid, and the amount of the sintering aid added is 0.6%wt lead oxide, 0.2%wt zinc oxide, 1.2%wt boron oxide, and 0.6%wt potassium oxide. The copper inner electrode nonlinear multilayer ceramic capacitor prepared by the dielectric material is debonded in a mixed gas atmosphere formed by nitrogen and hydrogen. The specific preparation method is as follows:

[0045] Step 1: Lay a copper inner electrode nonlinear multilayer ceramic capacitor flat on an alumina plate, wherein the nonlinear ceramic material of the multilayer ceramic capacitor is composed of PLZST and sintering aids such as lead oxide, zinc oxide, boron oxide, and potassium oxide.

[0046] Step 2, debonding the sample obtained in step 1 in an atmosphere furnace to obtain a multilayer ceramic capacitor green body; wherein, the debonding temperature is 300°C, the holding time is 72h, the heating rate is 1°C / min, and the temperature is cooled to room temperature at a rate of 3°C / min. The debonding atmosphere is a mixed gas formed by an inert gas (nitrogen) and a reducing gas (hydrogen), and the gas volume ratio is nitrogen: hydrogen = 1000:1.

[0047] Example 5

[0048] The nonlinear ceramic material used in the copper inner electrode nonlinear multilayer ceramic capacitor in this embodiment is a main crystal phase material PLZST and a sintering aid, and the amount of the sintering aid added is 0.6%wt lead oxide, 0.2%wt zinc oxide, 1.2%wt boron oxide, and 0.6%wt potassium oxide. The copper inner electrode nonlinear multilayer ceramic capacitor prepared by the dielectric material is debonded in a mixed gas atmosphere formed by nitrogen and hydrogen. The specific preparation method is as follows:

[0049] Step 1: Lay a copper inner electrode nonlinear multilayer ceramic capacitor flat on an alumina plate, wherein the nonlinear ceramic material of the multilayer ceramic capacitor is composed of PLZST and sintering aids such as lead oxide, zinc oxide, boron oxide, and potassium oxide.

[0050] Step 2, debonding the sample obtained in step 1 in an atmosphere furnace to obtain a multilayer ceramic capacitor green body; wherein, the debonding temperature is 350°C, the holding time is 48h, the heating rate is 1°C / min, and the temperature is cooled to room temperature at a rate of 3°C / min. The debonding atmosphere is a mixed gas formed by an inert gas (nitrogen) and a reducing gas (hydrogen), and the gas volume ratio is nitrogen:hydrogen = 1000:1.

[0051] Example 6

[0052] The nonlinear ceramic material used in the copper inner electrode nonlinear multilayer ceramic capacitor in this embodiment is a main crystal phase material PLZST and a sintering aid, and the amount of the sintering aid added is 0.6%wt lead oxide, 0.2%wt zinc oxide, 1.2%wt boron oxide, and 0.6%wt potassium oxide. The copper inner electrode nonlinear multilayer ceramic capacitor prepared by the dielectric material is debonded in a mixed gas atmosphere formed by nitrogen and hydrogen. The specific preparation method is as follows:

[0053] Step 1: Lay a copper inner electrode nonlinear multilayer ceramic capacitor flat on an alumina plate, wherein the nonlinear ceramic material of the multilayer ceramic capacitor is composed of PLZST and sintering aids such as lead oxide, zinc oxide, boron oxide, and potassium oxide.

[0054] Step 2, debonding the sample obtained in step 1 in an atmosphere furnace to obtain a multilayer ceramic capacitor green body; wherein, the debonding temperature is 400°C, the holding time is 24h, the heating rate is 1°C / min, and the temperature is cooled to room temperature at a rate of 3°C / min. The debonding atmosphere is a mixed gas formed by an inert gas (nitrogen) and a reducing gas (hydrogen), and the gas volume ratio is nitrogen:hydrogen = 1000:1.

[0055] Example 7

[0056] The copper inner electrode nonlinear multilayer ceramic capacitor green body used in this embodiment is obtained from Example 3 and then placed in an atmosphere furnace for sintering. The specific preparation method is as follows:

[0057] Step 11, placing the multilayer ceramic capacitor green body obtained in Example 3 in a corundum crucible, and covering it with ceramic powder of the same nonlinear ceramic material.

[0058] Step 12, sintering the sample obtained in step 11 in an atmosphere furnace to obtain a finished multilayer ceramic capacitor; wherein the sintering temperature is 920°C, the holding time is 4h, the heating rate is 3°C / min, and the temperature is cooled to room temperature at a rate of 3°C / min. The atmosphere used is a mixed gas formed by an inert gas (nitrogen) and a reducing gas (carbon monoxide), and the gas volume ratio is nitrogen: carbon monoxide = 500:1.

[0059] Example 8

[0060] The copper inner electrode nonlinear multilayer ceramic capacitor green body used in this embodiment is obtained from Example 3 and then placed in an atmosphere furnace for sintering. The specific preparation method is as follows:

[0061] Step 11, placing the multilayer ceramic capacitor green body obtained in Example 3 in a corundum crucible, and covering it with ceramic powder of the same nonlinear ceramic material.

[0062] Step 12, sintering the sample obtained in step 11 in an atmosphere furnace to obtain a finished multilayer ceramic capacitor; wherein the sintering temperature is 1000°C, the holding time is 3h, the heating rate is 3°C / min, and the temperature is cooled to room temperature at a rate of 3°C / min. The atmosphere used is a mixed gas formed by an inert gas (nitrogen) and a reducing gas (carbon monoxide), and the gas volume ratio is nitrogen: carbon monoxide = 800:1.

[0063] Example 9

[0064] The copper inner electrode nonlinear multilayer ceramic capacitor green body used in this embodiment is obtained from Example 3 and then placed in an atmosphere furnace for sintering. The specific preparation method is as follows:

[0065] Step 11, placing the multilayer ceramic capacitor green body obtained in Example 3 in a corundum crucible, and covering it with ceramic powder of the same nonlinear ceramic material.

[0066] Step 12, sintering the sample obtained in step 11 in an atmosphere furnace to obtain a finished multilayer ceramic capacitor; wherein the sintering temperature is 1050°C, the holding time is 2h, the heating rate is 3°C / min, and the temperature is cooled to room temperature at a rate of 3°C / min. The atmosphere used is a mixed gas formed by an inert gas (nitrogen) and a reducing gas (carbon monoxide), and the gas volume ratio is nitrogen: carbon monoxide = 1000:1.

[0067] Example 10

[0068] The copper inner electrode nonlinear multilayer ceramic capacitor green body used in this embodiment is obtained from Example 6 and then sintered in an atmosphere furnace. The specific preparation method is as follows:

[0069] Step 11, placing the multilayer ceramic capacitor green body obtained in Example 6 in a corundum crucible, and covering it with ceramic powder of the same nonlinear ceramic material.

[0070] Step 12, sintering the sample obtained in step 11 in an atmosphere furnace to obtain a finished multilayer ceramic capacitor; wherein the sintering temperature is 920°C, the holding time is 4h, the heating rate is 3°C / min, and the temperature is cooled to room temperature at a rate of 3°C / min. The atmosphere used is a mixed gas formed by an inert gas (nitrogen) and a reducing gas (carbon monoxide), and the gas volume ratio is nitrogen: carbon monoxide = 500:1.

[0071] Embodiment 11

[0072] The copper inner electrode nonlinear multilayer ceramic capacitor green body used in this embodiment is obtained from Example 6 and then sintered in an atmosphere furnace. The specific preparation method is as follows:

[0073] Step 11, placing the multilayer ceramic capacitor green body obtained in Example 6 in a corundum crucible, and covering it with ceramic powder of the same nonlinear ceramic material.

[0074] Step 12, sintering the sample obtained in step 11 in an atmosphere furnace to obtain a finished multilayer ceramic capacitor; wherein the sintering temperature is 1000°C, the holding time is 3h, the heating rate is 3°C / min, and the temperature is cooled to room temperature at a rate of 3°C / min. The atmosphere used is a mixed gas formed by an inert gas (nitrogen) and a reducing gas (carbon monoxide), and the gas volume ratio is nitrogen: carbon monoxide = 800:1.

[0075] Example 12

[0076] The copper inner electrode nonlinear multilayer ceramic capacitor green body used in this embodiment is obtained from Example 6 and then sintered in an atmosphere furnace. The specific preparation method is as follows:

[0077] Step 11, placing the multilayer ceramic capacitor green body obtained in Example 6 in a corundum crucible, and covering it with ceramic powder of the same nonlinear ceramic material.

[0078] Step 12, sintering the sample obtained in step 11 in an atmosphere furnace to obtain a finished multilayer ceramic capacitor; wherein the sintering temperature is 1050°C, the holding time is 2h, the heating rate is 3°C / min, and the temperature is cooled to room temperature at a rate of 3°C / min. The atmosphere used is a mixed gas formed by an inert gas (nitrogen) and a reducing gas (carbon monoxide), and the gas volume ratio is nitrogen: carbon monoxide = 1000:1.

[0079] Table 1 shows the test results of the copper inner electrode nonlinear multilayer ceramic capacitors of Examples 1 to 6 after debonding. The multilayer ceramic capacitor contains a large amount of organic matter inside. The organic matter will decompose into carbon dioxide gas and be discharged when it contacts oxygen at high temperature, but the copper inner electrode is easily oxidized in an oxygen environment. In addition, if the organic matter is not completely decomposed and the residual amount is too much, the porcelain body will crack during the sintering process. Therefore, Examples 1 to 6 use a weak oxygen atmosphere formed by nitrogen and hydrogen, so that the organic matter is decomposed and discharged from the inside of the porcelain body on the basis of ensuring that the copper is not oxidized. To measure whether the organic matter is completely or fully decomposed, the two parameters of weight loss rate and residual carbon rate are usually used for evaluation, as shown in Table 1. The sintering aids used in Examples 1 to 3 are lead oxide, aluminum oxide, boron oxide, and potassium oxide, and the sintering aids used in Examples 4-6 are lead oxide, zinc oxide, boron oxide, and potassium oxide. It can be seen from the table that the weight loss rate of Examples 1 to 3 and Examples 4-6 increases with the increase of the debonding temperature, and the residual carbon rate decreases with the increase of the debonding temperature, indicating that the increase in temperature promotes the decomposition of organic matter, and also indicates that the mixed gas environment is suitable. Comparing Example 1, Example 2 and Example 3, the weight loss rate of Example 3 is increased by 0.06% compared with that of Example 2, and the residual carbon rate is decreased by 0.04%; the weight loss rate of Example 2 is increased by 0.31% compared with that of Example 1, and the residual carbon rate is decreased by 0.79%. It can be seen that the multilayer ceramic capacitor of Example 3 has been fully debonded, and similarly, the multilayer ceramic capacitor of Example 6 has also been fully debonded.

[0080] Table 1

[0081] Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Weight loss rate (%) 7.55 7.86 7.92 7.58 7.82 7.93 Carbon residue rate (%) 1.35 0.56 0.52 1.40 0.54 0.52

[0082] Table 2 shows the test results of the copper inner electrode nonlinear multilayer ceramic capacitors after sintering of Examples 7 to 12. Examples 7 to 9 and Examples 10 to 12 used the samples after debonding of Example 3 and Example 6, respectively. The insulation resistance of Examples 7 to 12 was kept at 10 12 Ω order of magnitude, Example 9 and Example 11 have the largest insulation resistance of 4.05×10 12 Ω and 5.98×10 12Ω. In addition, the capacitance values ​​of Example 9 and Example 11 also have larger values ​​of 8.1nF and 8.5nF, and the losses are 0.008 and 0.005, respectively. The above results show that the copper inner electrode nonlinear multilayer ceramic capacitors with different sintering aids have different optimal sintering temperatures and sintering atmospheres. Example 9 has the best performance at 1050°C and nitrogen: carbon monoxide = 1000:1, while Example 11 has the best performance at 1000°C and nitrogen: carbon monoxide = 800:1.

[0083] Table 2

[0084]

[0085] Based on the above factors, this patent further analyzes Example 9 and Example 11.

[0086] After polishing the ends of the multilayer ceramic capacitors of Example 9 and Example 11, the internal structures were observed under an optical microscope. Figure 1 As shown. Example 9 and Example 11 show a good multilayer structure, the inner electrode continuously presents a metallic luster, and the ceramic dielectric is dense and has no holes. The distribution of Pb and Cu in the ceramic dielectric layer and the inner electrode layer is further observed under a scanning electron microscope, as shown Figure 2 As shown. In Example 9 and Example 11, the distribution of Pb in the inner electrode Cu and the porcelain dielectric layer is obvious, and there is no mutual penetration. The above results show that in Example 9 and Example 11, the goal of not oxidizing the copper inner electrode and not reducing the lead ions is achieved under this sintering method.

[0087] In order to evaluate the energy storage characteristics of the sintered multilayer ceramic capacitor, the hysteresis loops of Example 9 and Example 11 were tested. Figure 3 As shown in the figure, the hysteresis loops of Example 9 and Example 11 show thin features. The breakdown electric field of Example 9 is 260 kV / cm, and the maximum polarization intensity is 34 μC / cm 2 The breakdown electric field of Example 11 is 265 kV / cm, and the maximum polarization intensity is 29 μC / cm 2 It shows that the two sintering methods have different effects on the energy storage characteristics of multilayer ceramic capacitors. Based on this, the leakage current of the two is further tested. Figure 4 The leakage current density of Example 9 and Example 11 varies with the applied electric field. It can be seen that the leakage current density of both examples is maintained at 0.05 μC / cm 2 Hereinafter, Example 11 has a smaller leakage current density.

[0088] The present invention can also provide a copper inner electrode nonlinear multilayer ceramic capacitor, which is obtained by the above sintering method, wherein the copper inner electrode material of the copper inner electrode nonlinear multilayer ceramic capacitor is not oxidized, and the Pb in the dielectric material is not oxidized. 2+ It is not reduced, and there is no mutual penetration between the inner electrode material and the dielectric material.

[0089] In summary, the present invention successfully prepared a copper inner electrode nonlinear multilayer ceramic capacitor by optimizing the sintering method and the sintering aid of the nonlinear ceramic material. In order to prevent the multilayer ceramic capacitor from cracking during the sintering process, the internal organic matter needs to be discharged. By comparing the weight loss rate and the residual carbon rate after debonding, the debonding environment with a debonding temperature of 400°C and a gas volume ratio of nitrogen:hydrogen=500:1 was determined. According to the test results of insulation resistance, capacitance and loss of multilayer ceramic capacitors under different sintering temperatures and sintering atmospheres, the best sintering conditions are determined, that is, for the copper inner electrode multilayer ceramic capacitor whose dielectric material is mainly crystalline phase material PLZST and sintering aids are lead oxide, aluminum oxide, boron oxide and potassium oxide (Example 9), the sintering temperature is 1050°C, and the gas volume ratio is nitrogen: carbon monoxide = 1000:1; for the copper inner electrode multilayer ceramic capacitor whose dielectric material is mainly crystalline phase material PLZST and sintering aids are lead oxide, zinc oxide, boron oxide and potassium oxide (Example 11), the sintering temperature is 1000°C, and the gas volume ratio is nitrogen: carbon monoxide = 800:1. In addition, the Pb distribution of the inner electrode Cu and the ceramic dielectric layer of Examples 9 and 11 is obvious, and there is no mutual penetration phenomenon. It has a thin double hysteresis loop and a small leakage current, and the insulation resistance is maintained at 10 12 Ω order of magnitude; dielectric loss within 0.1; breakdown electric field reaches 260kV / cm, maximum polarization intensity reaches 34μC / cm 2 , indicating that its energy storage characteristics are good. The above results show that the patent of this invention successfully achieved the goal of not oxidizing the copper inner electrode and not reducing the lead ions, and successfully prepared the copper inner electrode nonlinear multilayer ceramic capacitor, which is of great significance for promoting the industrial mass production of copper inner electrode multilayer ceramic capacitors.

Claims

1. A sintering method for a copper inner electrode nonlinear multilayer ceramic capacitor, characterized in that: The following steps are involved: Debonding the copper inner electrode nonlinear multilayer ceramic capacitor under an inert atmosphere or a reducing atmosphere to obtain a copper inner electrode nonlinear multilayer ceramic capacitor green body; The obtained copper inner electrode nonlinear multilayer ceramic capacitor green body is placed in a corundum crucible and covered with ceramic powder; The ceramic capacitor green body covered with ceramic powder is sintered in an inert gas or a reducing gas to obtain a copper inner electrode nonlinear multilayer ceramic capacitor.

2. The sintering method of a copper inner electrode nonlinear multilayer ceramic capacitor according to claim 1, characterized in that: The nonlinear ceramic material used in the copper inner electrode nonlinear multilayer ceramic capacitor is an antiferroelectric ceramic material, and the main crystal phase is lead lanthanum zirconium tin titanium.

3. The sintering method of a copper inner electrode nonlinear multilayer ceramic capacitor according to claim 1, characterized in that: The inert gas is nitrogen, and the reducing gas is hydrogen or carbon monoxide.

4. The sintering method of a copper inner electrode nonlinear multilayer ceramic capacitor according to claim 3, characterized in that: The volume ratio of reducing gas during debonding is nitrogen: hydrogen = 1000:1, and the volume ratio of reducing gas during sintering is nitrogen: carbon monoxide = 500:1~1000:

1.

5. The sintering method of a copper inner electrode nonlinear multilayer ceramic capacitor according to claim 1, characterized in that: The temperature during the debonding is 300-400° C., the heat preservation time is 24-72 hours, the heating rate is 1° C. / minute, and the temperature is reduced to room temperature at a rate of 3° C. / minute.

6. The sintering method of a copper inner electrode nonlinear multilayer ceramic capacitor according to claim 1, characterized in that: The sintering temperature is 920-1050°C, the holding time is 2-4h, the heating rate is 3°C / min, and the temperature is reduced to room temperature at a rate of 3°C / min.

7. The sintering method of a copper inner electrode nonlinear multilayer ceramic capacitor according to claim 1, characterized in that: The ceramic powder is the same as the dielectric material of the copper inner electrode nonlinear multilayer ceramic capacitor.

8. The sintering method of a copper inner electrode nonlinear multilayer ceramic capacitor according to claim 2, characterized in that: The nonlinear multilayer ceramic capacitor contains 2.6%wt-3.0%wt of a sintering aid, wherein the sintering aid is lead oxide, aluminum oxide, zinc oxide, boron oxide, potassium oxide or a plurality of other agents.

9. A copper inner electrode nonlinear multilayer ceramic capacitor, characterized in that: The copper inner electrode material of the copper inner electrode nonlinear multilayer ceramic capacitor is not oxidized by the sintering method according to any one of claims 1 to 8, and the Pb in the dielectric material is 2+ It is not reduced, and there is no mutual penetration between the inner electrode material and the dielectric material.

Citation Information

Cited By

  • Copper inner electrode multi-layer co-fired piezoelectric actuator based on low-temperature reduction and preparation method thereof