Doped ferric sodium pyrophosphate positive electrode material, preparation method and application thereof
By doping carbon and boron or nitrogen and boron in the coating layer of the sodium iron pyrophosphate cathode material, an electron transmission network is constructed, which solves the problem of poor conductivity of the cathode material in sodium ion batteries and improves the electrochemical performance and capacity. Higher compaction density and stability are achieved.
Patent Information
- Application Number
- CN202410804341.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-20
- Publication Date
- 2024-10-25
AI Technical Summary
Existing sodium iron phosphate pyrophosphate cathode materials used in sodium-ion batteries have poor electron transmission, resulting in poor electrical conductivity, prominent electrochemical performance problems, low capacity, poor rate performance, high cost, and easy generation of electrolyte during the synthesis process. The electrochemically active sodium iron phosphate impurity phase affects performance.
By doping carbon atoms and boron atoms or the synergistic effect of carbon, nitrogen, and boron in the coating layer of sodium iron pyrophosphate cathode material, an electron transmission network between different particles is constructed, the electronic conductivity is improved, and during the spray drying process It can shape the spherical morphology, avoid wall sticking phenomenon, and improve the compaction density and electrochemical performance of the material.
Significantly improve the electronic conductivity and electrochemical capacity of the cathode material, maintain the stability and consistency of the product, improve the long-term cycle stability and electrochemical performance, solve the stability problem of the internal crystal structure of the material, and avoid unnecessary Capacity generation of NaFePO4 olivine heterogeneous phase.
Smart Images

Figure HDA0004904645680000011 
Figure HDA0004904645680000021 
Figure HDA0004904645680000031
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of positive electrode materials, and in particular to a doped sodium iron phosphate pyrophosphate positive electrode material, a preparation method and use thereof. Background Art
[0002] In recent years, storing energy from sustainable but intermittent resources (such as solar and wind energy) in large-scale energy storage systems has become a key issue. Although lithium-ion batteries have achieved great success in the application of small portable electronic products and medium-sized products (such as hybrid electric vehicles, electric vehicles, etc.), the shortage and uneven distribution of lithium mineral resources on the earth, as well as the sharp increase in demand for lithium batteries, have caused the price of scarce lithium mineral resources to continue to rise. At the same time, the rate charge and discharge capacity of lithium-ion batteries is reduced under low temperature conditions. All these problems limit the application of lithium-ion batteries in large-scale energy storage systems.
[0003] Since sodium and lithium belong to the same main group, have similar electrochemical properties, and are abundant in the earth's crust, sodium-ion batteries are expected to become a new generation of energy storage technology with performance and cost advantages after lithium batteries. Currently, sodium iron pyrophosphate-type sodium positive electrode materials have a relatively stable structure, excellent long-cycle stability and low-temperature rate performance, and low raw material costs and production processes, making them one of the ideal choices to replace lithium-ion batteries in the field of energy storage.
[0004] The existing sodium iron phosphate pyrophosphate type positive electrode materials for sodium ion batteries generally have poor electron transmission, resulting in poor conductivity of the material, and the electrochemical performance of the material is more prominent, resulting in low capacity of sodium ion batteries, poor rate performance of the material, low battery energy density, and high battery cost. At the same time, as a mixed phase of sodium iron phosphate and sodium iron pyrophosphate, sodium iron phosphate pyrophosphate is easily generated during the synthesis process, which greatly affects the electrochemical performance of the material. Summary of the invention
[0005] In response to the technical problems existing in the prior art, the present application provides a doped sodium iron phosphate pyrophosphate positive electrode material, a preparation method and its use. The positive electrode material can effectively construct an electron transport network between different particles through the synergistic effect of carbon atoms and boron atoms or carbon atoms and nitrogen atoms or carbon atoms, nitrogen atoms and boron atoms, thereby improving the electronic conductivity of the material.
[0006] The specific technical solutions of this application are as follows:
[0007] 1. A doped sodium iron phosphate pyrophosphate positive electrode material, wherein the structural formula of the positive electrode material is:
[0008] Na4Fe x M 3-x(PO4)2P2O7@C&A, where Na4Fe x M 3-x (PO4)2P2O7 is a core layer, C&A is a coating layer, A contains boron or nitrogen or contains nitrogen and boron; x is greater than 2.5 and less than or equal to 3;
[0009] M is selected from one or more of Mg, Co, Ni, Cu, Zn, Mn, Ti and V.
[0010] 2. The sodium iron phosphate pyrophosphate positive electrode material according to item 1, wherein A comprises nitrogen and boron.
[0011] 3. The sodium iron phosphate pyrophosphate positive electrode material according to item 1 or 2, wherein the compaction density of the sodium iron phosphate pyrophosphate positive electrode material is 2.3-3 g / cm 3 , and / or
[0012] The spraying balling rate of the sodium iron phosphate pyrophosphate positive electrode material is above 90%, preferably 92-100%.
[0013] 4. A method for preparing a doped sodium iron phosphate pyrophosphate positive electrode material, comprising:
[0014] Adding a sodium source, an iron source, a phosphorus source, a carbon source, an optional M source, and an A source into water and mixing to obtain a slurry;
[0015] The slurry is spray-dried to obtain a spherical precursor;
[0016] The spherical precursor is sintered and sieved to obtain a sodium iron pyrophosphate positive electrode material;
[0017] The A source comprises a boron source or a nitrogen source or a nitrogen source and a boron source.
[0018] 5. The method according to item 4, wherein the molar ratio of sodium source: iron source: phosphorus source is 3.90-4.10:2.70-3.00:3.90-4.10, preferably 4.0-4.1:2.7-2.9:4.0-4.1 or the molar ratio of sodium source: iron source: phosphorus source: M source is: 3.90-4.10:2.70-3.00:3.90-4.10:0-0.5.
[0019] 6. The method according to item 4 or 5, wherein the amount of the carbon source added is 1-12 wt %, preferably 5-10 wt % of the spherical precursor.
[0020] 7. The method according to any one of items 4 to 6, wherein when source A comprises a boron source, the amount of the boron source added is 1-3 wt % of the spherical precursor;
[0021] When source A includes a nitrogen source, the nitrogen source is added in an amount of 1-3 wt % of the spherical precursor;
[0022] When the source A comprises a nitrogen source and a boron source, the amount of the nitrogen source added is 1-3 wt % of the spherical precursor; the amount of the boron source added is 1-3 wt % of the spherical precursor.
[0023] 8. The method according to any one of items 4 to 7, wherein the boron source comprises boron chloride, boric acid, boron trioxide, sodium tetraborate or boron nitride or a combination thereof; and / or
[0024] The nitrogen source comprises urea, thiourea, melamine, polypyrrole or polyvinylpyrrolidone or a combination thereof;
[0025] The carbon source comprises a mixture of an organic carbon source and an inorganic carbon source.
[0026] 9. The method according to item 8, wherein the organic carbon source comprises citric acid, glucose, sucrose, maltose, lactose, cyclodextrin or water-soluble starch or a combination thereof;
[0027] The inorganic carbon source comprises super P, acetylene black, natural graphite, artificial graphite, hard carbon, carbon nanotubes, flake graphite, graphene or mesophase carbon microspheres or a combination thereof.
[0028] 10. A battery comprising the positive electrode material described in any one of items 1 to 3 or the positive electrode material prepared by the method described in any one of items 4 to 9.
[0029] Effects of the Invention
[0030] The positive electrode material described in the present application can effectively construct an electron transport network between different particles through the synergistic effect of carbon-boron elements or carbon and nitrogen elements or carbon, nitrogen and boron elements, thereby improving the electronic conductivity of the material; on the other hand, through element doping, the internal crystal structure of the material can be stabilized, the appearance of NaFePO4 olivine impurity phase with no capacity can be avoided, and the electrochemical capacity of the material can be improved.
[0031] The positive electrode material described in the present application has a voltage window of 2-3.6V, a charge capacity of 123mAh / g at 0.1C, and a discharge capacity of 113mAh / g, and has excellent long-cycle stability and electrochemical performance.
[0032] By adding carbon and boron or carbon and nitrogen or carbon, nitrogen and boron into the coating layer, the present application can better shape the spherical morphology of the particles during the spraying stage, thereby maintaining the stability and consistency of the product, solving the inherent wall sticking phenomenon during the spraying process, and improving the compaction density of the product. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1It is an electron microscope image of the positive electrode materials obtained in Examples 1-5 and the comparative example.
[0034] Figure 2 It is a schematic diagram of the charging and discharging results of the positive electrode materials obtained in the embodiment and the comparative example.
[0035] Figure 3 This is the crystal phase diagram of the positive electrode material obtained in Example 1. DETAILED DESCRIPTION
[0036] The present application is described in detail below in conjunction with the described embodiments. Although specific embodiments of the present application are shown, it should be understood that the present application can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided to enable a more thorough understanding of the present application and to enable the scope of the present application to be fully communicated to those skilled in the art.
[0037] It should be noted that certain words are used in the specification and claims to refer to specific components. Those skilled in the art should understand that technicians may use different nouns to refer to the same component. This specification and claims do not use the difference in nouns as a way to distinguish components, but use the functional differences of components as the criterion for distinction. As mentioned throughout the specification and claims, "including" or "comprising" are open-ended terms and should be interpreted as "including but not limited to". The subsequent description of the specification is a preferred embodiment of the present application, but the description is based on the general principles of the specification and is not intended to limit the scope of the present application. The scope of protection of the present application shall be determined by the attached claims.
[0038] The present application provides a doped sodium iron phosphate pyrophosphate positive electrode material, wherein the structural formula of the positive electrode material is:
[0039] Na4Fe x M 3-x (PO4)2P2O7@C&A, where Na4Fe x M 3-x (PO4)2P2O7 is a core layer, C&A are coating layers, A contains boron or nitrogen or contains nitrogen and boron; x is greater than 2.5 and less than or equal to 3. In some embodiments, A contains nitrogen and boron.
[0040] The present application can effectively construct an electron transport network between different particles by doping carbon and boron, or carbon and nitrogen, or carbon, nitrogen and boron in the coating layer, thereby improving the electronic conductivity of the material.
[0041] The positive electrode material described in the present application has a high compaction density of 2.3-3 g / cm 3The positive electrode material has a good spherical morphology and a high spray ball forming rate, which is above 90%, preferably 92-100%.
[0042] In the present application, there is no limitation on the method for measuring compaction density, which can be measured by conventional methods in the art, for example, the positive electrode material can be placed in a four-probe mold and measured for compaction density at a pressure of 350 MPa.
[0043] In the present application, there is no limitation on the method for determining the spray balling rate, which can be determined by conventional methods in the art, such as the counting method.
[0044] For example, x can be 2.5, 2.6, 2.7, 2.8, 2.9, 3.0, etc.
[0045] The compacted density can be 2.3g / cm 3 , 2.4g / cm 3 , 2.5g / cm 3 , 2.6g / cm 3 , 2.7g / cm 3 , 2.8g / cm 3 , 2.9g / cm 3 、3.0g / cm 3 wait.
[0046] The spray ball forming rate can be 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98%, 99%, 100%, etc.
[0047] The present application provides a method for preparing a doped sodium iron phosphate pyrophosphate positive electrode material, which comprises:
[0048] Adding a sodium source, an iron source, a phosphorus source, a carbon source, an optional M source, and an A source into water and mixing to obtain a slurry;
[0049] The slurry is spray-dried to obtain a spherical precursor;
[0050] The spherical precursor is sintered and sieved to obtain a sodium iron pyrophosphate positive electrode material;
[0051] The A source comprises a boron source or a nitrogen source or a nitrogen source and a boron source.
[0052] The present application uses the above-described method to better shape the spherical morphology of the particles during the spraying stage, thereby maintaining the stability and uniformity of the product and preventing the particles from sticking to the wall during the spraying process.
[0053] In some embodiments, the molar ratio of sodium source: iron source: phosphorus source is 3.90-4.10:2.70-3.00:3.90-4.10, preferably 4.0-4.1:2.7-2.9:4.0-4.1 or the molar ratio of sodium source: iron source: phosphorus source: M source is: 3.90-4.10:2.70-3.00:3.90-4.10:0-0.5.
[0054] When the core layer does not contain the doping element M, the molar ratio of sodium source: iron source: phosphorus source (n 钠源 :n 铁源 :n 磷源 ) can be 3.90:2.70:3.90, 4.10:2.80:4.00, 3.90:2.70:4.10, 3.90:2.80:4.10, 3.90:2.90:4.10, 3.90:3.00:4.10, 3.90:3.10:4.10, etc.;
[0055] When the core layer contains doping elements, the molar ratio of sodium source: iron source: phosphorus source: M source (n 钠源 :n 铁源 :m 磷源 :n M源 ) can be 3.90:2.70:3.90:0.1, 4.10:2.80:4.00:0.5, 3.90:2.70:4.10:0.4, 3.90:2.80:4.10:0.5, 3.90:2.90:4.10:0.3, 3.90:3.00:4.10:0.2, 3.90:3.10:4.10:0.1, etc.
[0056] In some embodiments, the amount of the carbon source added is 1-12 wt %, preferably 5-10 wt % of the spherical precursor.
[0057] For example, the added amount of the carbon source can account for 1wt%, 2wt%, 3wt%, 4wt%, 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 10wt%, 11wt%, 12wt% and the like of the spherical precursor.
[0058] In some embodiments, when the source A comprises a boron source, the boron source is added in an amount of 1-3 wt % of the spherical precursor;
[0059] When source A includes a nitrogen source, the nitrogen source is added in an amount of 1-3 wt % of the spherical precursor;
[0060] When the source A comprises a nitrogen source and a boron source, the amount of the nitrogen source added is 1-3 wt % of the spherical precursor; the amount of the boron source added is 1-3 wt % of the spherical precursor.
[0061] For example, when the source A includes a boron source, the amount of the boron source added may account for 1 wt%, 1.5 wt%, 2 wt%, 2.5 wt%, 3 wt%, etc. of the spherical precursor;
[0062] When source A includes a nitrogen source, the amount of the nitrogen source added may account for 1 wt%, 1.5 wt%, 2 wt%, 2.5 wt%, 3 wt%, etc. of the spherical precursor;
[0063] When source A includes a nitrogen source and a boron source, the amount of the nitrogen source added can account for 1wt%, 1.5wt%, 2wt%, 2.5wt%, 3wt% etc. of the spherical precursor; the amount of the boron source added can account for 1wt%, 1.5wt%, 2wt%, 2.5wt%, 3wt% etc. of the spherical precursor.
[0064] In some embodiments, the boron source comprises boron chloride, boric acid, boron trioxide, sodium tetraborate or boron nitride or a combination thereof; and / or
[0065] The nitrogen source comprises urea, thiourea, melamine, polypyrrole or polyvinylpyrrolidone or a combination thereof;
[0066] The carbon source comprises a mixture of an organic carbon source and an inorganic carbon source.
[0067] In some embodiments, the organic carbon source comprises citric acid, glucose, sucrose, maltose, lactose, cyclodextrin or water-soluble starch or a combination thereof;
[0068] The inorganic carbon source comprises super P, acetylene black, natural graphite, artificial graphite, hard carbon, carbon nanotubes, flake graphite, graphene or mesophase carbon microspheres or a combination thereof.
[0069] The present application provides a battery, which comprises the positive electrode material described above or the positive electrode material prepared by the method described above.
[0070] Example
[0071] The present application provides a general and / or specific description of the materials and test methods used in the experiments. In the following examples, unless otherwise specified, % means wt%, i.e., weight percentage. The reagents or instruments used without indicating the manufacturer are all conventional reagent products that can be obtained commercially.
[0072] Example 1
[0073] (1) 21.24 g (0.2 mol) of sodium carbonate, 41.05 g (0.27 mol) of iron phosphate, 1.2 g (0.15 mol) of titanium dioxide, 15.08 g (0.13 mol) of diammonium hydrogen phosphate, 9.01 g of citric acid, 1.00 g of polypyrrole, 1.25 g of boric acid and an appropriate amount of deionized water were mixed to control the solid content of the slurry to be 20%. The mixed slurry was added into a sand mill until the particle size was less than 100 nanometers to obtain a slurry.
[0074] (2) placing the slurry into a spray dryer for spray drying to obtain a spherical precursor, wherein the parameters of the spray dryer are: feed rate of 100 ml / min, air inlet temperature of 200° C., and air outlet temperature of 100° C. During the spray drying process, the slurry does not stick to the wall.
[0075] (3) The spherical precursor was placed in a tube furnace for sintering, and nitrogen was introduced as a protective gas. The sintering temperature was 600°C, the heating rate was 5°C / min, and the holding time was 15h. Then, the doped sodium iron phosphate pyrophosphate positive electrode material was obtained by screening. Its XRD pattern is shown in Figure 3 shown.
[0076] from Figure 3 It can be seen that the standard spectrum of Na4Fe3P4O 15 By comparison, the obtained positive electrode material does not contain impurities and is a pure phase, indicating that a doped sodium iron phosphate pyrophosphate positive electrode material has been prepared.
[0077] In addition, the obtained positive electrode material was photographed using an electron microscope, and the results are as follows Figure 1 shown.
[0078] from Figure 1 It can be seen that the obtained positive electrode material has good morphology and relatively uniform particles.
[0079] (4) Assembling the doped sodium ferric phosphate pyrophosphate positive electrode material into a button cell: The doped sodium ferric phosphate pyrophosphate positive electrode material, the conductive agent carbon black, the binder PVDF and the solvent N-methylpyrrolidone were mixed uniformly in a mass ratio of 8:1:1 to prepare a slurry. The slurry was coated on a carbon-coated aluminum foil, and after vacuum drying, it was punched into a positive electrode sheet. The metal sodium sheet was used as the negative electrode, the glass fiber paper was used as the separator, and the electrolyte ratio was 1 mol / L NaClO4. The button cell was assembled in EC:DEC (1:1 vol%) in an argon atmosphere and a glove box with a moisture content of ≤50 ppm.
[0080] Example 2
[0081] (1) 21.24 g (0.2 mol) of sodium carbonate, 41.05 g (0.27 mol) of iron phosphate, 1.2 g (0.015 mol) of titanium dioxide, 15.08 g (0.13 mol) of diammonium hydrogen phosphate, 9.01 g of citric acid, 1.00 g of polypyrrole and an appropriate amount of deionized water were mixed to control the solid content of the slurry to be 20%. The mixed slurry was added to a high-grit mill until the particle size was less than 100 nanometers to obtain a slurry;
[0082] (2) The same as step (2) of Example 1, during the spray drying process, the slurry slightly adhered to the wall.
[0083] (3) The same as step (3) of Example 1, and the obtained positive electrode material was photographed using an electron microscope, and the result is as follows Figure 1 shown.
[0084] from Figure 1 It can be seen that the obtained positive electrode material has good morphology and uniform particles.
[0085] (4) Same as step (4) of Example 1.
[0086] Example 3
[0087] (1) 21.24 g (0.2 mol) of sodium carbonate, 41.05 g (0.27 mol) of iron phosphate, 1.2 g (0.015 mol) of titanium dioxide, 15.08 g (0.13 mol) of diammonium hydrogen phosphate, 9.01 g of citric acid, 1.25 g of boric acid and an appropriate amount of deionized water were mixed to control the solid content of the slurry to be 20%. The mixed slurry was added to a sand mill until the particle size was less than 100 nanometers to obtain a slurry.
[0088] (2) The same as step (2) of Example 1, during the spray drying process, the slurry slightly adhered to the wall.
[0089] (3) The same as step (3) of Example 1, and the obtained positive electrode material was photographed using an electron microscope, and the result is as follows Figure 1 shown.
[0090] from Figure 1 It can be seen that the obtained positive electrode material has good morphology and uniform particles.
[0091] (4) Same as step (4) of Example 1.
[0092] Example 4
[0093] (1) 21.24 g (0.2 mol) of sodium carbonate, 41.05 g (0.27 mol) of iron phosphate, 1.2 g (0.015 mol) of titanium dioxide, 15.08 g (0.13 mol) of diammonium hydrogen phosphate, 9.01 g of citric acid, 2.00 g of polypyrrole, 2.50 g of boric acid and an appropriate amount of deionized water were mixed to control the solid content of the slurry to be 20%. The mixed slurry was added into a sand mill until the particle size was less than 100 nanometers to obtain a slurry.
[0094] (2) The same as step (2) of Example 1, during the spray drying process, the slurry does not stick to the wall.
[0095] (3) The same as step (3) of Example 1, and the obtained positive electrode material was photographed using an electron microscope, and the result is as follows Figure 1 shown.
[0096] from Figure 1 It can be seen that the obtained positive electrode material has good morphology and relatively uniform particles.
[0097] (4) Same as step (4) of Example 1.
[0098] Example 5
[0099] (1) 21.24 g (0.2 mol) of sodium carbonate, 41.05 g (0.27 mol) of iron phosphate, 1.2 g (0.015 mol) of titanium dioxide, 15.08 g (0.13 mol) of diammonium hydrogen phosphate, 9.01 g of citric acid, 0.5 g of polypyrrole, 0.63 g of boric acid and an appropriate amount of deionized water were mixed to control the solid content of the slurry to be 20%. The mixed slurry was added to a sand mill until the particle size was less than 100 nanometers to obtain a slurry.
[0100] (2) As in step (2) of Example 1, during the spray drying process, some of the slurry adhered to the wall.
[0101] (3) The same as step (3) of Example 1, and the obtained positive electrode material was photographed using an electron microscope, and the result is as follows Figure 1 shown.
[0102] from Figure 1 It can be seen that the obtained positive electrode material has average morphology and average particle uniformity.
[0103] (4) Same as step (4) of Example 1.
[0104] Example 6
[0105] (1) 21.24 g (0.2 mol) of sodium carbonate, 41.05 g (0.27 mol) of iron phosphate, 1.2 g (0.015 mol) of titanium dioxide, 15.08 g (0.13 mol) of diammonium hydrogen phosphate, 9.01 g of citric acid, 2.70 g of polypyrrole and an appropriate amount of deionized water were mixed to control the solid content of the slurry to be 20%. The mixed slurry was added to a high-grit mill until the particle size was less than 100 nanometers to obtain a slurry;
[0106] (2) The same as step (2) of Example 1, during the spray drying process, the slurry slightly adhered to the wall.
[0107] (3) The same as step (3) of Example 1, and the obtained positive electrode material is photographed using an electron microscope. The obtained positive electrode material has good morphology and uniform particles.
[0108] (4) Same as step (4) of Example 1.
[0109] Example 7
[0110] (1) 21.24 g (0.2 mol) of sodium carbonate, 41.05 g (0.27 mol) of iron phosphate, 1.2 g (0.015 mol) of titanium dioxide, 15.08 g (0.13 mol) of diammonium hydrogen phosphate, 9.01 g of citric acid, 3.25 g of polypyrrole and an appropriate amount of deionized water were mixed to control the solid content of the slurry to be 20%. The mixed slurry was added to a high-grit mill until the particle size was less than 100 nanometers to obtain a slurry;
[0111] (2) As in step (2) of Example 1, during the spray drying process, some of the slurry adhered to the wall.
[0112] (3) The same as step (3) of Example 1, and the obtained positive electrode material was photographed using an electron microscope. The morphology of the obtained positive electrode material was average and the particle uniformity was average.
[0113] (4) Same as step (4) of Example 1.
[0114] Example 8
[0115] (1) 21.24 g (0.2 mol) of sodium carbonate, 41.05 g (0.27 mol) of iron phosphate, 1.2 g (0.015 mol) of titanium dioxide, 15.08 g (0.13 mol) of diammonium hydrogen phosphate, 9.01 g of citric acid, 0.50 g of polypyrrole and an appropriate amount of deionized water were mixed to control the solid content of the slurry to be 20%. The mixed slurry was added to a high-grit mill until the particle size was less than 100 nanometers to obtain a slurry;
[0116] (2) As in step (2) of Example 1, during the spray drying process, some of the slurry adhered to the wall.
[0117] (3) The same as step (3) of Example 1, and the obtained positive electrode material was photographed using an electron microscope. The morphology of the obtained positive electrode material was average and the particle uniformity was average.
[0118] (4) Same as step (4) of Example 1.
[0119] Example 9
[0120] (1) 21.24 g (0.2 mol) of sodium carbonate, 41.05 g (0.27 mol) of iron phosphate, 1.2 g (0.015 mol) of titanium dioxide, 15.08 g (0.13 mol) of diammonium hydrogen phosphate, 9.01 g of citric acid, 2.71 g of boric acid and an appropriate amount of deionized water were mixed to control the solid content of the slurry to be 20%. The mixed slurry was added to a sand mill until the particle size was less than 100 nanometers to obtain a slurry.
[0121] (2) The same as step (2) of Example 1, during the spray drying process, the slurry slightly adhered to the wall.
[0122] (3) The same as step (3) of Example 1, and the obtained positive electrode material is photographed using an electron microscope. The obtained positive electrode material has good morphology and uniform particles.
[0123] (4) Same as step (4) of Example 1.
[0124] Example 10
[0125] (1) 21.24 g (0.2 mol) of sodium carbonate, 41.05 g (0.27 mol) of iron phosphate, 1.2 g (0.015 mol) of titanium dioxide, 15.08 g (0.13 mol) of diammonium hydrogen phosphate, 9.01 g of citric acid, 3.65 g of boric acid and an appropriate amount of deionized water were mixed to control the solid content of the slurry to be 20%. The mixed slurry was added to a sand mill until the particle size was less than 100 nanometers to obtain a slurry.
[0126] (2) As in step (2) of Example 1, during the spray drying process, some of the slurry adhered to the wall.
[0127] (3) The same as step (3) of Example 1, and the obtained positive electrode material was photographed using an electron microscope. The morphology of the obtained positive electrode material was average and the particle uniformity was average.
[0128] Embodiment 11
[0129] (1) 21.24 g (0.2 mol) of sodium carbonate, 41.05 g (0.27 mol) of iron phosphate, 1.2 g (0.015 mol) of titanium dioxide, 15.08 g (0.13 mol) of diammonium hydrogen phosphate, 9.01 g of citric acid, 0.44 g of boric acid and an appropriate amount of deionized water were mixed to control the solid content of the slurry to be 20%. The mixed slurry was added to a sand mill until the particle size was less than 100 nanometers to obtain a slurry.
[0130] (2) As in step (2) of Example 1, during the spray drying process, some of the slurry adhered to the wall.
[0131] (3) The same as step (3) of Example 1, and the obtained positive electrode material was photographed using an electron microscope. The morphology of the obtained positive electrode material was average and the particle uniformity was average.
[0132] Example 12
[0133] (1) 21.24 g (0.2 mol) of sodium carbonate, 41.05 g (0.27 mol) of iron phosphate, 1.2 g (0.015 mol) of titanium dioxide, 15.08 g (0.13 mol) of diammonium hydrogen phosphate, 9.01 g of citric acid, 2.70 g of polypyrrole, 1.25 g of boric acid and an appropriate amount of deionized water were mixed to control the solid content of the slurry to be 20%. The mixed slurry was added into a sand mill until the particle size was less than 100 nanometers to obtain a slurry.
[0134] (2) The same as step (2) of Example 1, during the spray drying process, the slurry does not stick to the wall.
[0135] (3) The same as step (3) of Example 1, and the obtained positive electrode material is photographed using an electron microscope. The obtained positive electrode material has a good morphology and relatively uniform particles.
[0136] (4) Same as step (4) of Example 1.
[0137] Embodiment 13
[0138] (1) 21.24 g (0.2 mol) of sodium carbonate, 41.05 g (0.27 mol) of iron phosphate, 1.2 g (0.015 mol) of titanium dioxide, 15.08 g (0.13 mol) of diammonium hydrogen phosphate, 9.01 g of citric acid, 3.71 g of polypyrrole, 1.25 g of boric acid and an appropriate amount of deionized water were mixed to control the solid content of the slurry to be 20%. The mixed slurry was added into a sand mill until the particle size was less than 100 nanometers to obtain a slurry.
[0139] (2) As in step (2) of Example 1, during the spray drying process, some of the slurry adhered to the wall.
[0140] (3) The same as step (3) of Example 1, and the obtained positive electrode material was photographed using an electron microscope. The morphology of the obtained positive electrode material was average and the particle uniformity was average.
[0141] (4) Same as step (4) of Example 1.
[0142] Embodiment 14
[0143] (1) 21.24 g (0.2 mol) of sodium carbonate, 41.05 g (0.27 mol) of iron phosphate, 1.2 g (0.015 mol) of titanium dioxide, 15.08 g (0.13 mol) of diammonium hydrogen phosphate, 9.01 g of citric acid, 0.50 g of polypyrrole, 1.25 g of boric acid and an appropriate amount of deionized water were mixed to control the solid content of the slurry to be 20%. The mixed slurry was added into a sand mill until the particle size was less than 100 nanometers to obtain a slurry.
[0144] (2) As in step (2) of Example 1, during the spray drying process, some of the slurry adhered to the wall.
[0145] (3) The same as step (3) of Example 1, and the obtained positive electrode material was photographed using an electron microscope. The morphology of the obtained positive electrode material was average and the particle uniformity was average.
[0146] (4) Same as step (4) of Example 1.
[0147] Embodiment 15
[0148] (1) 21.24 g (0.2 mol) of sodium carbonate, 41.05 g (0.27 mol) of iron phosphate, 1.2 g (0.015 mol) of titanium dioxide, 15.08 g (0.13 mol) of diammonium hydrogen phosphate, 9.01 g of citric acid, 1.00 g of polypyrrole, 2.74 g of boric acid and an appropriate amount of deionized water were mixed to control the solid content of the slurry to be 20%. The mixed slurry was added to a sand mill until the particle size was less than 100 nanometers to obtain a slurry.
[0149] (2) The same as step (2) of Example 1, during the spray drying process, the slurry does not stick to the wall.
[0150] (3) The same as step (3) of Example 1, and the obtained positive electrode material is photographed using an electron microscope. The obtained positive electrode material has a good morphology and relatively uniform particles.
[0151] (4) Same as step (4) of Example 1.
[0152] Example 16
[0153] (1) 21.24 g (0.2 mol) of sodium carbonate, 41.05 g (0.27 mol) of iron phosphate, 1.2 g (0.015 mol) of titanium dioxide, 15.08 g (0.13 mol) of diammonium hydrogen phosphate, 9.01 g of citric acid, 1.00 g of polypyrrole, 3.22 g of boric acid and an appropriate amount of deionized water were mixed to control the solid content of the slurry to be 20%. The mixed slurry was added into a sand mill until the particle size was less than 100 nanometers to obtain a slurry.
[0154] (2) As in step (2) of Example 1, during the spray drying process, some of the slurry adhered to the wall.
[0155] (3) The same as step (3) of Example 1, and the obtained positive electrode material was photographed using an electron microscope. The morphology of the obtained positive electrode material was average and the particle uniformity was average.
[0156] (4) Same as step (4) of Example 1.
[0157] Embodiment 17
[0158] (1) 21.24 g (0.2 mol) of sodium carbonate, 41.05 g (0.27 mol) of iron phosphate, 1.2 g (0.015 mol) of titanium dioxide, 15.08 g (0.13 mol) of diammonium hydrogen phosphate, 9.01 g of citric acid, 1.00 g of polypyrrole, 0.45 g of boric acid and an appropriate amount of deionized water were mixed to control the solid content of the slurry to be 20%. The mixed slurry was added to a sand mill until the particle size was less than 100 nanometers to obtain a slurry.
[0159] (2) As in step (2) of Example 1, during the spray drying process, some of the slurry adhered to the wall.
[0160] (3) The same as step (3) of Example 1, and the obtained positive electrode material was photographed using an electron microscope. The morphology of the obtained positive electrode material was average and the particle uniformity was average.
[0161] (4) Same as step (4) of Example 1.
[0162] Comparative Example 1
[0163] (1) 21.24 g (0.2 mol) of sodium carbonate, 41.05 g (0.27 mol) of iron phosphate, 1.2 g (0.015 mol) of titanium dioxide, 15.08 g (0.13 mol) of diammonium hydrogen phosphate, 9.01 g of citric acid and an appropriate amount of deionized water were mixed to control the solid content of the slurry to be 20%. The mixed slurry was added to a sand mill until the particle size was less than 100 nanometers to obtain a slurry.
[0164] (2) As in step (2) of Example 1, a large amount of slurry adhered to the wall during the spray drying process.
[0165] (3) The same as step (3) of Example 1, and the obtained positive electrode material was photographed using an electron microscope, and the result is as follows Figure 1 shown.
[0166] from Figure 1 It can be seen that the morphology of the obtained positive electrode material is not good and the particles are uneven.
[0167] (4) Same as step (4) of Example 1.
[0168] Experimental Example 1 Determination of compaction density and spray balling rate
[0169] The positive electrode materials obtained in Examples 1-17 and Comparative Example 1 were placed in a four-probe mold, and the test was performed after the pressure curve was set. Finally, the compaction density under a pressure of 350 MPa was read. The results are shown in Table 1.
[0170] The spray balling rate is the ratio of the number of broken balls to the total number of balls in the field of view, which is obtained by counting the pictures scanned by an electron microscope using image J software or by counting with the naked eye. The results are shown in Table 1.
[0171] Table 1
[0172] project <![CDATA[Compaction density g / cm 3 > Spray balling rate % Example 1 2.60 99.5 Example 2 2.43 85.0 Example 3 2.40 83.0 Example 4 2.59 95.0 Example 5 2.48 92.0 Example 6 2.44 84.0 Example 7 2.41 78.0 Example 8 2.41 75.0 Example 9 2.45 82.0 Example 10 2.39 75.0 Embodiment 11 2.38 73.0 Example 12 2.55 94.0 Embodiment 13 2.51 92.0 Embodiment 14 2.49 90.0 Embodiment 15 2.56 95.0 Example 16 2.52 93.0 Embodiment 17 2.50 91.0 Comparative Example 1 2.20 60.0
[0173] As can be seen from the above table, the embodiment simultaneously doped nitrogen / boron elements, nano-sized the particles during the sand milling process, and obtained a regular spherical morphology during the spray drying process, and the process did not produce the inherent wall sticking phenomenon in the spraying process. Compared with the comparative example 1 without doping, the compaction density of the product can be greatly improved, and the energy density of the product can be greatly improved at the downstream battery cell end;
[0174] In addition, from the comparison between Example 1 and Examples 2-3, it can be seen that when nitrogen and boron are added simultaneously for doping, the compaction density of the product can be greatly improved, indicating that doping nitrogen and boron can synergistically enhance the effect.
[0175] The obtained positive electrode material has good spherical morphology and the spraying ball forming rate is above 90%.
[0176] Experimental Example 2: Button Battery Performance Test
[0177] The button cells assembled in Examples 1-17 and Comparative Example 1 were subjected to electrochemical performance tests using the Xinwei battery system. That is, after the battery was connected to the channel, the corresponding active material was input, and it was first left to stand for 6 hours to ensure that the electrolyte was fully infiltrated, and then charged to 3.6V at 0.1C constant current and constant voltage. After standing for 10 minutes, it was discharged to 2.0V at 0.1C constant current. The charging and discharging results of Examples 1-5 and Comparative Example 1 are as follows: Figure 2 As shown in Table 2, the curve with an upward trend is the charging curve, and the curve with a downward trend is the discharging curve. The charge and discharge capacities of Examples 1-17 and Comparative Example 1 are shown in Table 2.
[0178] Table 2
[0179] Charging capacity mAh / g Discharge capacity mAh / g Example 1 123.47 113.46 Example 2 113.72 104.50 Example 3 111.67 102.61 Example 4 121.05 110.88 Example 5 116.88 107.06 Example 6 114.55 105.32 Example 7 111.34 103.45 Example 8 112.56 103.32 Example 9 114.98 104.32 Example 10 111.33 101.05 Embodiment 11 110.37 100.06 Example 12 120.23 109.89 Embodiment 13 118.34 106.59 Embodiment 14 117.45 107.43 Embodiment 15 121.45 110.43 Example 16 118.58 107.82 Embodiment 17 118.73 105.34 Comparative Example 1 107.69 93.58
[0180] from Figure 2 As can be seen from Table 2, the embodiments are doped with nitrogen, boron or nitrogen / boron elements at the same time, the particles are nanosized during the sand milling process, and a regular spherical morphology is obtained during the spray drying process, and the process does not produce the wall sticking phenomenon inherent in the spraying process, or only has a slight wall sticking phenomenon. Compared with the control example without doping (charging capacity of 107.69 mAh / g, discharge capacity of 93.58 mAh / g), the charge and discharge capacity is significantly improved, and the energy density of the product can be greatly improved at the battery cell end.
[0181] The above is only the preferred embodiment of the present application, and does not limit the present application in other forms. Any technician familiar with the profession may use the above disclosed technical content to change or modify it into an equivalent embodiment with equivalent changes. However, any simple modification, equivalent change and modification made to the above embodiment based on the technical essence of the present application without departing from the technical solution of the present application still falls within the protection scope of the technical solution of the present application.
Claims
1. A doped sodium iron phosphate pyrophosphate positive electrode material, wherein the structural formula of the positive electrode material is: Na 4 Fe x M 3-x (PO 4 ) 2 P 2 O 7 @C&A, where Na 4 Fe x M 3-x (PO 4 ) 2 P 2 O 7 is a core layer, C&A are coating layers, A contains boron or nitrogen or contains nitrogen and boron; x is greater than 2.5 and less than or equal to 3; M is one or more selected from the group consisting of Mg, Co, Ni, Cu, Zn, Mn, Ti and V.
2. The sodium iron phosphate pyrophosphate positive electrode material according to claim 1, in, A contains nitrogen and boron.
3. The sodium iron phosphate pyrophosphate positive electrode material according to claim 1 or 2, wherein the compaction density of the sodium iron phosphate pyrophosphate positive electrode material is 2.3-3 g / cm 3 , and / or The spraying balling rate of the sodium iron phosphate pyrophosphate positive electrode material is above 90%, preferably 92-100%.
4. A method for preparing a doped sodium iron phosphate pyrophosphate positive electrode material, wherein include: Adding a sodium source, an iron source, a phosphorus source, a carbon source, an optional M source, and an A source into water and mixing to obtain a slurry; The slurry is spray-dried to obtain a spherical precursor; The spherical precursor is sintered and sieved to obtain a sodium iron pyrophosphate positive electrode material; The A source comprises a boron source or a nitrogen source or a nitrogen source and a boron source.
5. The method according to claim 4, wherein the molar ratio of sodium source: iron source: phosphorus source is 3.90-4.10:2.70-3.00:3.90-4.10, preferably 4.0-4.1:2.7-2.9:4.0-4.1 or the molar ratio of sodium source: iron source: phosphorus source: M source is: 3.90-4.10:2.70-3.00:3.90-4.10:0-0.
5.
6. The method according to claim 4 or 5, in, The amount of the carbon source added is 1-12 wt % of the spherical precursor, preferably 5-10 wt %.
7. The method according to any one of claims 4 to 6, in, When the source A includes a boron source, the amount of the boron source added is 1-3 wt % of the spherical precursor; When source A includes a nitrogen source, the nitrogen source is added in an amount of 1-3 wt % of the spherical precursor; When the source A comprises a nitrogen source and a boron source, the amount of the nitrogen source added is 1-3 wt % of the spherical precursor; the amount of the boron source added is 1-3 wt % of the spherical precursor.
8. The method according to any one of claims 4 to 7, in, The boron source comprises boron chloride, boric acid, boron trioxide, sodium tetraborate or boron nitride or a combination thereof; and / or The nitrogen source comprises urea, thiourea, melamine, polypyrrole or polyvinylpyrrolidone or a combination thereof; The carbon source comprises a mixture of an organic carbon source and an inorganic carbon source.
9. The method according to claim 8, in, The organic carbon source comprises citric acid, glucose, sucrose, maltose, lactose, cyclodextrin or water-soluble starch or a combination thereof; The inorganic carbon source comprises super P, acetylene black, natural graphite, artificial graphite, hard carbon, carbon nanotubes, flake graphite, graphene or mesophase carbon microspheres or a combination thereof.
10. A battery comprising the positive electrode material according to any one of claims 1 to 3 or the positive electrode material prepared by the method according to any one of claims 4 to 9.
Citation Information
Cited By
Low-resistivity carbon composite phosphoric acid and sodium ferric pyrophosphate positive electrode material, preparation method thereof and application of positive electrode material in sodium-ion battery
CN119637836A
High-covalent-component sodium ferric pyrophosphate positive electrode material as well as preparation method and application of high-covalent-component sodium ferric pyrophosphate positive electrode material
CN119965262A
Nitrogen-doped carbon-coated mixed sodium ferric pyrophosphate polyanion positive electrode material and preparation method thereof
CN121149203A