Positive electrode material for solid sulfide battery as well as preparation method and application of positive electrode material

By using a two-step chemical vapor deposition method to prepare the graphene carbon layer structure in the solid-state lithium-ion battery cathode material, the problem of the interface between the cathode material and the sulfide electrolyte is solved, the cycle performance and stability of the battery are improved, and the specific surface area is enhanced. Improves the overall performance of the battery.

CN118841538APending Publication Date: 2024-10-25JINGMEN GEM NEW MATERIAL CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410837502.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

In solid-state lithium-ion batteries, the interface between the cathode material and the sulfide solid inorganic electrolyte is poorly bonded, resulting in poor battery chemical stability and poor cycle performance. In addition, the existing coating layer affects the specific surface area of ​​the material and affects battery safety.

Method used

A two-step chemical vapor deposition method is used to prepare inner and outer graphene carbon layer structures in the cathode material, which work synergistically to reduce interface resistance, improve lithium ion migration efficiency, and increase the specific surface area of ​​the material.

Benefits of technology

Significantly improve the cycle performance, stability and safety of solid-state lithium batteries, enhance the specific surface area of ​​the material, and improve the electrical performance of the battery. The 0.1C discharge capacity reaches 196.4mAh/g, the 1C discharge capacity reaches 174.3mAh/g, and the cycle is 100 The weekly capacity retention rate can reach over 96.3%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004913577600000091
    Figure BDA0004913577600000091
  • Figure BDA0004913577600000111
    Figure BDA0004913577600000111
Patent Text Reader

Abstract

The invention provides a positive electrode material for a solid sulfide battery and a preparation method and application thereof, and the preparation method comprises the following steps: (1) carrying out chemical vapor deposition treatment on a positive electrode precursor in a mixed atmosphere to obtain a modified precursor; (2) mixing the modified precursor with a lithium source, and sintering to obtain a sintered material; and (3) performing chemical vapor deposition treatment on the sintered material in a mixed atmosphere to obtain the positive electrode material for the solid sulfide battery, the mixed atmosphere comprises a gas carbon source and hydrogen. The two-step chemical vapor deposition is adopted to prepare a two-layer graphene carbon layer structure in the positive electrode material, and the synergistic effect of the inner graphene carbon layer and the outer graphene carbon layer not only can solve the problem of poor bonding between the positive electrode material and a sulfide solid inorganic electrolyte interface, but also can reduce the interface impedance and promote the migration efficiency of lithium ions; therefore, the cycle performance, the stability and the safety of the all-solid-state lithium battery material are improved, and the specific surface area of the material can be effectively increased.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of battery materials and relates to a positive electrode material for a solid sulfide battery and a preparation method and application thereof. Background Art

[0002] Traditional lithium-ion batteries will cause safety issues such as rapid temperature rise and even combustion during high-voltage rapid charging and discharging. The main reason for this is that the organic liquid electrolyte makes the battery flammable. From a safety perspective, we have to consider reducing the flammability of the battery's organic liquid electrolyte. The solution to this problem is mostly to improve the physical and chemical properties of the electrolyte.

[0003] Solid-state lithium-ion batteries are lithium-ion batteries that use solid electrolytes. In all-solid-state lithium-ion batteries, the electrolyte is made of non-volatile inorganic solids. In the early days of the development of all-solid-state lithium-ion batteries, people paid great attention to the improvement of lithium ion conductivity in solid electrolyte materials. Through a large number of studies, it was found that inorganic sulfide solid electrolytes can effectively improve the flammability problem of organic liquid electrolytes, but there are still many problems in sulfide solid-state lithium-ion batteries, such as poor chemical stability of the battery, small "solid-solid" contact area of ​​the positive electrode material, and matching between the electrode and the electrolyte. These are the main reasons restricting the commercial development of solid-state lithium-ion batteries.

[0004] CN114267833A discloses a method for coating a ternary positive electrode material with a sulfide solid electrolyte. 2 S and P 2 S 5 Add to the dispersive solvent, ultrasonically stir the solution to obtain a precursor solution, then add a non-protonic polar solvent, a lithium salt containing X and a ternary cathode material and heat and stir, then vacuum evaporate, low-temperature sinter, grind and screen to obtain a ternary cathode material uniformly coated with a sulfide solid electrolyte.

[0005] CN118039833A discloses a modified positive electrode material and a preparation method thereof and an all-solid-state lithium-ion battery. The modified positive electrode material comprises: a positive electrode substrate and a composite coating layer, wherein the composition of the composite coating layer is Li 3k La 2 / 3-k TiO 3 ·M 1-x La x TiO 3 , wherein M is selected from alkaline earth metal elements, k is selected from 0.1-0.3, and x is selected from 0.1-0.2.

[0006] Improving the interface problem between the positive electrode material and the sulfide solid electrolyte is of great significance for improving the stability and safety of all-solid-state lithium batteries. However, the coating layer of the positive electrode material described in the above scheme will affect the specific surface area of ​​the material, and the stability of the coating layer is poor, which affects the cycle performance of the material. Summary of the invention

[0007] The purpose of the present invention is to provide a positive electrode material for a solid sulfide battery, and a preparation method and application thereof. The present invention adopts two-step chemical vapor deposition to prepare a two-layer graphene carbon layer structure in the positive electrode material. The synergistic effect of the inner and outer graphene carbon layers can not only solve the problem of poor bonding between the positive electrode material and the sulfide solid inorganic electrolyte interface, but also reduce the interface impedance, promote the migration efficiency of lithium ions, thereby improving the cycle performance and stability safety of the all-solid-state lithium battery material, and can also effectively increase the specific surface area of ​​the material.

[0008] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0009] In a first aspect, the present invention provides a method for preparing a positive electrode material for a solid sulfide battery, the preparation method comprising the following steps:

[0010] (1) subjecting the cathode precursor to a one-step chemical vapor deposition treatment under a first mixed atmosphere to obtain a modified precursor;

[0011] (2) mixing the modified precursor with a lithium source and subjecting the mixture to sintering treatment to obtain a sintered material;

[0012] (3) performing a two-step chemical vapor deposition treatment on the sintered material under a second mixed atmosphere to obtain the positive electrode material for the solid sulfide battery;

[0013] The first mixed atmosphere and the second mixed atmosphere independently include a gaseous carbon source and hydrogen.

[0014] The present invention uses a method of chemical vapor deposition to prepare a layer of graphene carbon layer structure in situ on the surface of the positive electrode precursor in advance. The structure of the graphene carbon layer is stable and the thickness is controllable. The graphene carbon layer of suitable thickness will not affect the combination of lithium ions and precursors to generate positive electrode materials in the subsequent process of mixed sintering with a lithium source. After the lithium-containing sintering material is obtained, a layer of graphene carbon layer is prepared by chemical vapor deposition. The outer graphene carbon layer and the inner graphene carbon layer play a certain synergistic role, which solves the problem of poor combination between the positive electrode material and the sulfide solid inorganic electrolyte interface, reduces the interface impedance, promotes the lithium ion transmission efficiency, and improves the cycle stability and safety performance of the battery. At the same time, because graphene is a two-dimensional structure with a very high specific surface area, the inner and outer layers contain graphene structures, which can greatly increase the specific surface area of ​​the material, thereby improving the electrical properties of the material.

[0015] Preferably, the gaseous carbon source in the first mixed atmosphere in step (1) includes any one of methane, ethylene or acetylene, or a combination of at least two of them. Typical but non-limiting combinations include a combination of methane and ethylene, a combination of methane and acetylene, or a combination of ethylene and acetylene, etc.

[0016] Preferably, taking the total volume of the gas in the first mixed atmosphere in step (1) as 100%, the volume proportion of the gaseous carbon source is 60-80%, for example: 60%, 65%, 70%, 75% or 80%, etc., not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0017] Preferably, taking the total volume of the gas in the first mixed atmosphere in step (1) as 100%, the volume proportion of the hydrogen is 20-40%, for example: 20%, 25%, 30%, 35% or 40%, etc., not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0018] Preferably, the positive electrode precursor in step (1) comprises a ternary nickel-cobalt-manganese precursor.

[0019] Preferably, the pressure of the chemical vapor deposition process in step (1) is 0.5×10 -3 ~1.5×10 -3 Pa, for example: 0.5×10 -3 Pa, 0.8×10 -3 Pa, 1×10 -3 Pa, 1.2×10 -3 Pa or 1.5×10 -3 Pa, etc. are not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0020] Preferably, the temperature of the one-step chemical vapor deposition treatment in step (1) is 400-800°C, for example, 400°C, 500°C, 600°C, 700°C or 800°C, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0021] Preferably, the mixed gas flow rate of the one-step chemical vapor deposition treatment in step (1) is 0.1 to 1 L / min, for example: 0.1 L / min, 0.2 L / min, 0.5 L / min, 0.8 L / min or 1 L / min, etc., not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0022] Preferably, the time for the one-step chemical vapor deposition treatment in step (1) is 0.2 to 1 h, for example, 0.2 h, 0.4 h, 0.6 h, 0.8 h or 1 h, etc., and is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0023] Preferably, the lithium source in step (2) comprises lithium hydroxide and / or lithium carbonate.

[0024] Preferably, the molar ratio of the total molar amount of metal elements in the modified precursor in step (2) to the lithium element in the lithium source is 1:(1.01-1.05), for example: 1:1.01, 1:1.02, 1:1.03, 1:1.04 or 1:1.05, etc., not limited to the listed values, other unlisted values ​​within the numerical range are also applicable.

[0025] Preferably, the sintering temperature in step (2) is 700-1000°C, for example, 700°C, 750°C, 800°C, 900°C or 1000°C, etc., but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0026] Preferably, the sintering time in step (2) is 8 to 20 hours, for example, 8 hours, 10 hours, 15 hours, 18 hours or 20 hours, etc., not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0027] Preferably, the atmosphere of the sintering treatment in step (2) includes an oxygen-containing atmosphere.

[0028] Preferably, the gaseous carbon source in the second mixed atmosphere in step (3) includes any one of methane, ethylene or acetylene, or a combination of at least two of them.

[0029] Preferably, taking the total volume of the gas in the second mixed atmosphere in step (3) as 100%, the volume proportion of the gas carbon source is 80% to 96%, for example: 80%, 85%, 88%, 90% or 96%, etc., not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0030] Preferably, taking the total volume of the gas in the first mixed atmosphere in step (3) as 100%, the volume proportion of the hydrogen is 4% to 20%, for example: 4%, 10%, 12%, 15% or 80%, etc., and is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0031] Preferably, the pressure of the two-step chemical vapor deposition process in step (3) is 0.5×10 -3 ~1.5×10 -3 Pa, for example: 0.5×10-3 Pa, 0.8×10 -3 Pa, 1×10 -3 Pa, 1.2×10 -3 Pa or 1.5×10 -3 Pa, etc. are not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0032] Preferably, the temperature of the one-step chemical vapor deposition treatment in step (3) is 400-800°C, for example, 400°C, 500°C, 600°C, 700°C or 800°C, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0033] Preferably, the mixed gas flow rate of the one-step chemical vapor deposition treatment in step (3) is 0.1 to 1 L / min, for example: 0.1 L / min, 0.2 L / min, 0.5 L / min, 0.8 L / min or 1 L / min, etc., not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0034] Preferably, the time for the one-step chemical vapor deposition treatment in step (3) is 2 to 4 hours, for example: 2 hours, 2.5 hours, 3 hours, 3.5 hours or 4 hours, etc., not limited to the listed values, other values ​​not listed within the numerical range are also applicable.

[0035] In a second aspect, the present invention provides a positive electrode material for a solid sulfide battery, wherein the positive electrode material for a solid sulfide battery is prepared by the preparation method described in the first aspect.

[0036] In a third aspect, the present invention provides a positive electrode plate, wherein the positive electrode plate comprises the positive electrode material for a solid sulfide battery as described in the second aspect.

[0037] In a fourth aspect, the present invention provides a solid-state sulfide battery, wherein the solid-state sulfide battery comprises the positive electrode sheet as described in the third aspect.

[0038] Compared with the prior art, the present invention has the following beneficial effects:

[0039] (1) The present invention adopts two-step chemical vapor deposition to prepare a two-layer graphene carbon layer structure in the positive electrode material. The synergistic effect of the inner and outer graphene carbon layers can not only solve the problem of poor bonding between the positive electrode material and the sulfide solid inorganic electrolyte interface, reduce the interface impedance, and promote the migration efficiency of lithium ions, thereby improving the cycle performance and stability and safety of the all-solid-state lithium battery material, but also effectively increase the specific surface area of ​​the material.

[0040] (2) The specific surface area of ​​the positive electrode material for solid sulfide batteries prepared by the present invention can reach 16.2 m2 / g or more, the 0.1C discharge capacity of the battery can reach more than 196.4mAh / g, the 1C discharge capacity can reach more than 174.3mAh / g, and the capacity retention rate after 100 cycles can reach more than 96.3%. DETAILED DESCRIPTION

[0041] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0042] Example 1

[0043] This embodiment provides a positive electrode material for a solid sulfide battery, and the positive electrode material for a solid sulfide battery is prepared by the following method:

[0044] (1) Weigh 20 g of dry Ni 0.8 Co 0.1 Mn 0.1 (OH) 2 The cathode precursor was evenly coated on a quartz plate and placed in a chemical vapor deposition (CVD) furnace. The CVD furnace was evacuated and heated to 600 °C and maintained at 1 × 10 -3 A mixed gas of methane and hydrogen with a volume ratio of 7:3 was introduced at a speed of 0.5 L / min under a pressure of 1.3 Pa for 0.5 h to obtain a modified precursor;

[0045] (2) mixing the modified precursor with lithium carbonate in a ratio of Li / M=1.02:1, and sintering at 800° C. for 12 h to obtain a sintered material;

[0046] (3) The sintered material is evenly coated on a quartz plate and placed in a CVD furnace. The CVD furnace is evacuated and heated to 600°C and maintained at 1×10 -3 A mixed gas of methane and hydrogen with a volume ratio of 9:1 was introduced at a speed of 0.5 L / min under a pressure of 1.5 Pa for 3 hours to obtain the positive electrode material for the solid sulfide battery.

[0047] Example 2

[0048] This embodiment provides a positive electrode material for a solid sulfide battery, and the positive electrode material for a solid sulfide battery is prepared by the following method:

[0049] (1) Weigh 20 g of dry Ni 0.8 Co 0.1 Mn 0.1 (OH) 2The cathode precursor was evenly coated on a quartz plate and placed in a chemical vapor deposition (CVD) furnace. The CVD furnace was evacuated and heated to 400 °C and maintained at 1.5 × 10 -3 A one-step chemical vapor deposition treatment was performed for 0.2 h by introducing a mixed gas of ethylene and hydrogen with a volume ratio of 6:4 at a speed of 0.1 L / min under a pressure of 1.3 Pa to obtain a modified precursor;

[0050] (2) mixing the modified precursor with lithium carbonate in a ratio of Li / M=1.02:1, and sintering at 700° C. for 20 h to obtain a sintered material;

[0051] (3) The sintered material is evenly coated on a quartz plate and placed in a CVD furnace. The CVD furnace is evacuated and heated to 400°C and maintained at 1.2×10 -3 A mixed gas of ethylene and hydrogen with a volume ratio of 9.6:0.4 was introduced at a speed of 0.6 L / min under a pressure of 1.3 Pa to carry out a two-step chemical vapor deposition treatment for 4 hours to obtain the positive electrode material for the solid sulfide battery.

[0052] Example 3

[0053] This embodiment provides a positive electrode material for a solid sulfide battery, and the positive electrode material for a solid sulfide battery is prepared by the following method:

[0054] (1) Weigh 20 g of dry Ni 0.8 Co 0.1 Mn 0.1 (OH) 2 The cathode precursor was evenly coated on a quartz plate and placed in a chemical vapor deposition (CVD) furnace. The CVD furnace was evacuated and heated to 400 °C and maintained at 0.5 × 10 -3 A one-step chemical vapor deposition treatment was performed for 1 h by introducing a mixed gas of acetylene and hydrogen with a volume ratio of 7:3 at a speed of 1 L / min under a pressure of 1.3 Pa to obtain a modified precursor;

[0055] (2) mixing the modified precursor with lithium carbonate in a ratio of Li / M=1.02:1, and sintering at 1000° C. for 20 h to obtain a sintered material;

[0056] (3) The sintered material is evenly coated on a quartz plate and placed in a CVD furnace. The CVD furnace is evacuated and heated to 400°C and maintained at 0.8×10 -3 A mixed gas of acetylene and hydrogen with a volume ratio of 8:2 was introduced at a speed of 0.2 L / min under a pressure of 1.3 Pa for 2 hours to obtain the positive electrode material for the solid sulfide battery.

[0057] Example 4

[0058] The only difference between this embodiment and embodiment 1 is that the volume ratio of methane to hydrogen in the atmosphere of one-step chemical vapor deposition is 8.5:1.5, and other conditions and parameters are exactly the same as those in embodiment 1.

[0059] Example 5

[0060] The only difference between this embodiment and embodiment 1 is that the volume ratio of methane to hydrogen in the atmosphere of one-step chemical vapor deposition is 5:5, and other conditions and parameters are exactly the same as those in embodiment 1.

[0061] Example 6

[0062] The only difference between this embodiment and embodiment 1 is that the volume ratio of methane to hydrogen in the atmosphere of the two-step chemical vapor deposition is 7.5:2.5, and the other conditions and parameters are exactly the same as those in embodiment 1.

[0063] Example 7

[0064] The only difference between this embodiment and embodiment 1 is that the volume ratio of methane to hydrogen in the atmosphere of the two-step chemical vapor deposition is 9.8:0.2, and the other conditions and parameters are exactly the same as those in embodiment 1.

[0065] Comparative Example 1

[0066] The only difference between this comparative example and Example 1 is that no chemical vapor deposition process is performed, and other conditions and parameters are exactly the same as those in Example 1.

[0067] Comparative Example 2

[0068] The only difference between this comparative example and Example 1 is that the two-step chemical vapor deposition process is not performed, and the other conditions and parameters are exactly the same as those in Example 1.

[0069] Comparative Example 3

[0070] The only difference between this comparative example and Example 1 is that the precursor is directly mixed with the lithium source and sintered to form the positive electrode material.

[0071] Performance Testing:

[0072] The positive electrode materials prepared in the embodiment and the comparative example were tested for their specific surface areas and then made into solid sulfide batteries. The charge and discharge cycle test was carried out using the Blue Electric electrical measurement system CT2001A. The voltage range was 2.5-4.3V. The charge and discharge cycle test was carried out at 0.1C and 1C rates, respectively. The test results are shown in Table 1:

[0073] Table 1

[0074]

[0075] As can be seen from Table 1, from Examples 1-3, the specific surface area of ​​the positive electrode material for solid sulfide batteries prepared by the present invention can reach 16.2 m 2 / g or more, the 0.1C discharge capacity of the battery can reach more than 196.4mAh / g, the 1C discharge capacity can reach more than 174.3mAh / g, and the capacity retention rate after 100 cycles can reach more than 96.3%.

[0076] By comparing Example 1 with Examples 4-5, it can be seen that in the preparation process of the positive electrode material for the solid sulfide battery according to the present invention, the volume proportion of the gaseous carbon source in the atmosphere of the one-step chemical vapor deposition treatment will affect its performance. The volume proportion of the gaseous carbon source in the atmosphere of the one-step chemical vapor deposition treatment is controlled at 60-80%, and the performance of the positive electrode material for the solid sulfide battery obtained is better. If the carbon source proportion is too high, the formed graphene carbon layer is too dense and thick, which hinders the reaction between lithium and the precursor during the sintering process and affects the performance of the material. If the carbon source proportion is too low, a stable graphene carbon layer cannot be formed, affecting the structural stability of the material.

[0077] By comparing Example 1 with Examples 6-7, it can be seen that in the preparation process of the positive electrode material for the solid sulfide battery according to the present invention, the volume proportion of the gaseous carbon source in the atmosphere of the two-step chemical vapor deposition treatment will affect its performance. The volume proportion of the gaseous carbon source in the atmosphere of the two-step chemical vapor deposition treatment is controlled at 80-96%, and the performance of the positive electrode material for the solid sulfide battery obtained is better. If the proportion of the carbon source is too high, the graphene carbon layer formed is too thick, which affects the performance of the material. If the proportion of the carbon source is too low, the structural stability of the formed graphene carbon layer is poor, and the cycle performance of the material is reduced.

[0078] By comparing Example 1 and Comparative Examples 1-3, it can be seen that the present invention adopts two-step chemical vapor deposition to prepare a two-layer graphene carbon layer structure in the positive electrode material, and the synergistic effect of the inner and outer graphene carbon layers can not only solve the problem of poor bonding between the positive electrode material and the sulfide solid inorganic electrolyte interface, but also reduce the interfacial impedance, promote the migration efficiency of lithium ions, thereby improving the cycle performance and stability and safety of the all-solid-state lithium battery material, and can also effectively increase the specific surface area of ​​the material.

[0079] Application Example 1

[0080] This application example uses the positive electrode material for solid sulfide batteries prepared in Example 1 to make a Li 7 La 3 Zr 2 O 12 , that is, a solid-state battery with LLZO as the electrolyte.

[0081] Comparative application example 1

[0082] The only difference between this comparative application example and application example 1 is that the conventional ternary positive electrode material is prepared using comparative example 3, and the other conditions and parameters are exactly the same as those of application example 1.

[0083] The solid-state batteries prepared in Example 1 and Comparative Application Example 1 were tested for performance. The test results are as follows:

[0084] Table 2

[0085]

[0086] It can be seen from Application Example 1 and Comparative Application Example 1 that the positive electrode material for a solid sulfide battery according to the present invention can only improve the problem of poor bonding between the positive electrode material and the sulfide solid inorganic electrolyte interface, reduce the interface impedance, promote the lithium ion transmission efficiency, and improve the battery's cycle stability and safety performance, but it is not targeted at other solid electrolytes (such as LLZO). This also reflects that the positive electrode material for a solid sulfide battery according to the present invention has strong selectivity.

[0087] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing a positive electrode material for a solid sulfide battery, characterized in that: The preparation method comprises the following steps: (1) subjecting the cathode precursor to a one-step chemical vapor deposition treatment under a first mixed atmosphere to obtain a modified precursor; (2) mixing the modified precursor with a lithium source and subjecting the mixture to sintering treatment to obtain a sintered material; (3) performing a two-step chemical vapor deposition treatment on the sintered material under a second mixed atmosphere to obtain the positive electrode material for the solid sulfide battery; The first mixed atmosphere and the second mixed atmosphere independently include a gaseous carbon source and hydrogen.

2. The preparation method according to claim 1, characterized in that Step (1) The gaseous carbon source in the first mixed atmosphere includes any one of methane, ethylene or acetylene, or a combination of at least two thereof; Preferably, based on the total volume of the gas in the first mixed atmosphere in step (1) being 100%, the volume of the gaseous carbon source accounts for 60 to 80%; Preferably, based on the total volume of the gas in the first mixed atmosphere in step (1) being 100%, the volume proportion of the hydrogen gas is 20-40%; Preferably, the positive electrode precursor in step (1) comprises a ternary nickel-cobalt-manganese precursor.

3. The preparation method according to claim 1 or 2, characterized in that: The pressure of the chemical vapor deposition process in step (1) is 0.5×10 -3 ~1.5×10 -3 Pa; Preferably, the temperature of the one-step chemical vapor deposition process in step (1) is 400-800° C.; Preferably, the mixed gas flow rate of the one-step chemical vapor deposition process in step (1) is 0.1 to 1 L / min; Preferably, the one-step chemical vapor deposition treatment in step (1) takes 0.2 to 1 h.

4. The preparation method according to any one of claims 1 to 3, characterized in that: The lithium source in step (2) includes lithium hydroxide and / or lithium carbonate; Preferably, the molar ratio of the total molar amount of metal elements in the modified precursor in step (2) to the molar ratio of lithium elements in the lithium source is 1:(1.01-1.05).

5. The preparation method according to any one of claims 1 to 4, characterized in that: The sintering temperature in step (2) is 700-1000° C. Preferably, the sintering time in step (2) is 8 to 20 hours; Preferably, the atmosphere of the sintering treatment in step (2) includes an oxygen-containing atmosphere.

6. The preparation method according to any one of claims 1 to 5, characterized in that: Step (3) the gaseous carbon source in the second mixed atmosphere includes any one of methane, ethylene or acetylene, or a combination of at least two thereof; Preferably, based on the total volume of the gas in the second mixed atmosphere in step (3) being 100%, the volume proportion of the gaseous carbon source is 80-96%; Preferably, based on the total volume of the gas in the first mixed atmosphere in step (3) being 100%, the volume proportion of the hydrogen gas is 4-20%.

7. The preparation method according to any one of claims 1 to 6, characterized in that: The pressure of the two-step chemical vapor deposition process in step (3) is 0.5×10 -3 ~1.5×10 -3 Pa; Preferably, the temperature of the one-step chemical vapor deposition process in step (3) is 400-800° C.; Preferably, the mixed gas flow rate of the one-step chemical vapor deposition process in step (3) is 0.1 to 1 L / min; Preferably, the one-step chemical vapor deposition treatment in step (3) takes 2 to 4 hours.

8. A positive electrode material for a solid sulfide battery, characterized in that: The positive electrode material for solid-state sulfide battery is prepared by the preparation method according to any one of claims 1 to 7.

9. A positive electrode sheet, characterized in that: The positive electrode sheet comprises the positive electrode material for a solid sulfide battery as claimed in claim 8.

10. A solid-state sulfide battery, characterized in that: The solid-state sulfide battery comprises the positive electrode sheet as claimed in claim 9.