Bone cement composition
By adjusting the ratio of methyl methacrylate-styrene copolymer and polymethyl methacrylate in the bone cement, the problem of insufficient bone cement consolidation time when the operation time is short is solved, and the mesh bag can be used to pressurize the vertebral body. Rapid consolidation and high compressive strength during arthroplasty, suitable for a variety of orthopedic surgeries.
Patent Information
- Application Number
- CN202011062400.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2020-08-18
- Filing Date
- 2020-09-30
- Publication Date
- 2024-10-29
AI Technical Summary
In operations with short operation times, such as mesh bag compression vertebroplasty, the existing bone cement has insufficient consolidation time, resulting in prolonged operation time, waste of resources, and impact on postoperative healing.
Use a combination of methyl methacrylate-styrene copolymer and polymethyl methacrylate, adjust the ratio of solid powder and liquid solution, ensure that the operating time is 5 to 10 minutes, and the solidification time is 10 to 15 minutes, and The compressive strength reaches 90~120MPa.
It realizes the rapid consolidation of bone cement during mesh bag compression vertebroplasty, shortens the operation time, improves the quality of postoperative healing, and is also suitable for other orthopedic surgeries.
Abstract
Description
Technical Field
[0001] The present invention relates to a bone cement composition, in particular to a bone cement composition, wherein the slurry formed after uniform mixing has an operation time of 5 to 10 minutes and a solidification time of 10 to 15 minutes; and the compressive strength of the bone cement after polymerization reaction is 90 to 120 MPa. Background Art
[0002] Bone cement is a commonly used material in orthopedic surgery, most commonly used in hip joint surgery. Its main component is polymethyl methacrylate (PMMA), which is usually made by mixing PMMA powder containing a small amount of initiator and methyl methacrylate (MMA) evenly to produce a polymerization reaction to form a PMMA block. In response to the needs of various orthopedic surgeries, PMMA must have different working times and setting times.
[0003] For example, in U.S. Patent No. 9,821,085, the operation time is mentioned in columns 11, 23 to 44 as 5 to 6 minutes and 8 to 10 minutes, and the solidification time is mentioned in items 12 and 18 of the patent application as being greater than 25 minutes. The solid material is composed of two PMMA powders of different sizes (less than 100 microns and greater than 100 microns, see item 2 of the patent application), a developer, and BPO, and the liquid solution is composed of MMA, N,N-dimethyl para-toluidine (DMPT), and hydroquinone (HQ), see columns 22, 45 to 61 of the patent, wherein the content of DMPT in the liquid solution is 30 to 120 ppm, and the content of BPO in the solid powder is 0.2 to 0.3 wt %, see columns 25, 23 to 42, indicating that the composition is different from that of the present invention, and therefore the solidification time is also different.
[0004] Another example is U.S. Patent No. 9,750,840, in which Items 11 and 14 of the patent application both state that the operation time is at least 10 minutes, and Item 13 of the patent application states that the operation time is at least 20 minutes. Item 1 of the patent application states that its solid material is mainly PMMA and its liquid solution is MMA, while the ratio of BPO to MMA listed in Table 1 in Column 62 is obviously different from the present invention.
[0005] Although U.S. Patent No. 10,029,031 mentions prepolymerized styrene-acrylate, it is different from the methyl methacrylate-styrene copolymer used in the present invention. In addition, the solid material of the invention also contains 1-100 micron ceramic powder, and the surface of the ceramic powder is coated with cross-linked collagen (see Item 1 of the patent application scope of the patent), which is not included in the present invention; furthermore, the solid material also contains BPO, but the liquid solution of the patent contains 0.2-2wt% or 0.3-0.4wt% DMPT (see Column 13, Lines 57-61), while the present invention contains 2.2-2.8wt% DMPT.
[0006] U.S. Patent No. 8,834,772 only adds 5-6 wt% gentamicin and 4%-5 wt% vancomycin to the solid material (acrylic polymer) of general bone cement, see Item 1 of its patent application, which are not included in the present invention.
[0007] In U.S. Patent No. 8,795,382, the first component is a polymerizable resin, and the second component is primary amines, secondary amines, tertiary amines, and / or quaternary amines, see its abstract, wherein the polymerizable resin is epoxy acrylate, modified epoxy acrylate, bisphenol A epoxy methacrylate oligomer, see Item 6 of its patent application, and its composition is completely different from the present invention.
[0008] U.S. Patent No. 8,415,407, the operation time is at least 5 minutes, the monomer (equivalent to the liquid solution of the present invention) is a mixture of lauryl methacrylate (LMA) and / or methyl methacrylate (MMA) in a ratio of 90:10 to 10:90, see columns 20, lines 22 to 26, and tetrahydrofuran (THF), and the amount of BPO used is about 14.4 to 25.8 mg per 10 ml of monomer, see Table 1 in column 60. The present invention does not use THF, and the amount of BPO used relative to 20 monomers (MMA) is about 200 to 400 mg per 10 ml.
[0009] U.S. Patent No. 4,404,327, which is polyacrylate (polyhacrylate), see column 6, lines 5 to 33 (a total of 32 polyacrylates), and polymethacrylate, see column 6, lines 35 to 50 (a total of 16 polymethacrylates), and its composition is also different from the present invention.
[0010] Patent No. I465266 in Taiwan, China, contains cross-linked poly(methyl methacrylate-sodium acrylate-allyl methacrylate), i.e., poly(MMA-AAS-AMA), which has a composition completely different from the present invention (PMMA+S / MM copolymer).
[0011] Patent application No. 201121591 in Taiwan, China, consists of calcium phosphate (powder) and aqueous solution, and its composition is completely different from the present invention (PMMA+S / MM copolymer).
[0012] Chinese patent CN 107213517 B, its solid powder includes PMMA and SIS (small intestinal submucosa, completely decellularized porcine small intestinal submucosa), and the liquid solution contains 0.6-1.5wt% DMPT and 100-350ppm of hydroquinone. See the first item of its patent application scope, it is obvious that its composition is different from the present invention; in addition, its solidification time is 10-20 minutes, which is also different from the present invention.
[0013] China's public application No. CN110025823A, its solid powder includes 30-49% PMMA, 5-20% BaSO4, 5-13% BPO, 5-30% gum arabic, 5-35% nano diatomaceous earth, 1-10% TiO2 and 1-10% ZnO, see item 1 of its patent application scope, which is obviously different from the present invention.
[0014] China's CN109331226A published application, its solid powder includes modified mineralized collagen, prepolymerized polymethyl methacrylate (PMMA) powder, polymerization initiator, and its solid powder and liquid solution ratio is 4.5 ~ 5.0g / mL, which is different from the present invention.
[0015] China's published application No. CN 109316627 A, its solid powder includes modified mineralized collagen, prepolymerized polymethyl methacrylate (PMMA) powder, and polymerization initiator, and the ratio of its solid powder to liquid solution is 1:2.5-4.5 g / mL, see Item 1 of its patent application scope, which is obviously different from the present invention.
[0016] Chinese patent No. CN 103800946 B is similar to CN 109316627A, but its ingredients and ingredient ratios are slightly different. Its solid powder includes modified mineralized collagen, prepolymerized polymethyl methacrylate (PMMA) powder, and a polymerization initiator, and the ratio of its solid powder to liquid solution is 1:1.5-3.0 g / mL. See item 1 of its patent application scope, which is obviously different from the present invention. Summary of the invention
[0017] The invention provides a bone cement composition with a slurry operation time of 5 to 10 minutes.
[0018] The invention provides a bone cement composition with a slurry solidification time of 10 to 15 minutes.
[0019] The invention provides a bone cement composition with a compressive strength of 90 to 120 MPa after consolidation.
[0020] The general design of bone cement is widely used bone cement, and it is expected that most orthopedic surgeries, such as hip surgery, knee surgery, and spinal surgery, can be used; therefore, the setting of the operation time and the consolidation time are relatively loose. For example, the above-mentioned U.S. Patent No. 9,821,085 has a consolidation time of more than 25 minutes (see the 12th item of its patent application scope), so it can be applied to most surgeries. However, for surgeries with shorter operation time, such as mesh bag pressurized vertebroplasty (vesselplasty), the entire operation time does not exceed 20 minutes. Therefore, in order to wait for the bone cement to completely solidify, the operation time is forced to increase. In addition to wasting the time of medical staff and the use time of the operating room, the patient is also caused by the increase in operation time, resulting in poor postoperative healing. The main purpose of the present invention is to design for the above-mentioned mesh bag pressurized vertebroplasty (vesselplasty), so the operation time is set to 10 to 15 minutes, and the working time is set to 5 to 10 minutes, and the compressive strength after consolidation is set to 90 to 120Mpa. Of course, a person skilled in the art can use the bone cement composition of the present invention for other applicable orthopedic surgeries.
[0021] The bone cement composition of the present invention comprises: a solid powder, which comprises: 57-63wt% of methyl methacrylate-styrene copolymer, 9-15wt% of polymethyl methacrylate, 22-34wt% of developer, and about 1.0-2.0wt% of BPO (Benzoyl peroxide); a liquid solution, which comprises: 97.2-97.8wt% of methyl methacrylate (MMA) monomer, 2.2-2.8wt% of N,N-dimethyl-p-toluidine (DMPT), and about 80ppm of hydroquinone; wherein the weight ratio of the solid powder to the liquid solution is between 20:10 and 23:10, so that the slurry formed after uniform mixing has an operation time of 5-10 minutes and a solidification time of 10-15 minutes; and the compressive strength of the bone cement after the polymerization reaction is 90-120MPa.
[0022] The weight ratio of the solid powder to the liquid solution is slightly lower than 20:10 (e.g., 19.8:10), which is not impractical, but will increase the following risks, namely, causing the operation time to be too long, wasting the medical staff's time (waiting), or the bone cement solidifies too late, resulting in a prolonged operation time and slow postoperative healing.
[0023] The weight ratio of the solid powder to the liquid solution is slightly higher than 23:10 (e.g., 23.2:10), which is not impractical, but will increase the following risks, namely, causing the operation time to be too short, the medical staff to be unable to operate in time, or the bone cement to solidify too early, resulting in insufficient bone cement perfusion, and / or difficulty in removing tools.
[0024] The solid powder generally adopts pure polymethylmethacrylate powder (hereinafter referred to as PMMA). However, the working time and setting time of the pure PMMA powder when mixed with methylmethacrylate (hereinafter referred to as MMA) and the strength of the bone cement formed after the mixture are difficult to meet the requirements of 5 to 10 minutes for the working time, 10 to 15 minutes for the setting time and 90 to 120 MPa for the compressive strength of the bone cement after the polymerization reaction (hereinafter referred to as the requirements of the present invention). However, a mixture of methyl methacrylate-styrene copolymer (hereinafter referred to as PMMA-S) and PMMA can meet the requirements of the present invention at the same time.
[0025] In the solid powder, the proportion of PMMA-S is preferably 57-63wt%, preferably 58-62wt%.
[0026] In the solid powder, the proportion of PMMA is preferably 9 to 15 wt %, preferably 10 to 14 wt %.
[0027] The developer in the solid powder can be any known developer, such as barium sulfate, zirconium dioxide, etc. The developer is preferably used in an amount of 22-34wt% of the solid powder, preferably 26-30wt%. If the developer is less than 22wt%, the development effect will be poor, causing the doctor to be unable to clearly grasp the flow direction of the bone cement during the operation, which greatly increases the risk of failure of the operation; when the developer is higher than 34wt%, the compressive strength of the bone cement after solidification is insufficient, making the patient prone to fractures after the operation.
[0028] In the above-mentioned solid powder, the proportion of BPO is preferably 1.0-2.0wt%. The proportion of BPO must be matched with the proportion of PMMA and PMMA-S in the solid powder, the proportion of the liquid solution, and / or the relative matching of the solid powder and the liquid solution to meet the requirements of the present invention; if the proportion of BPO is lower than 1.0wt%, the operation time will be too long, which will waste the time (waiting) of medical staff and relatively prolong the solidification time of bone cement, resulting in too long operation time, indirectly affecting the time of postoperative healing; when the proportion of BPO is higher than 2.0wt%, the operation time and / or solidification time will be too short, which will cause the medical staff to fail to operate in time, or the bone cement will solidify too early, which will greatly increase the risk of operation failure.
[0029] In the above-mentioned liquid solution, the content of N,N-dimethyl para-toluidine (hereinafter referred to as DMPT) is preferably 2.2-2.8wt%, preferably 2.4-2.6wt%. The ratio of DMPT must be the ratio of PMMA, PMMA-S, BPO in the solid powder, and / or the relative coordination of the solid powder and the liquid solution to meet the requirements of the present invention. If the DMPT ratio is lower than 2.2wt%, the operation time will be too long, wasting the time (waiting) of medical staff and relatively prolonging the solidification time of bone cement, resulting in too long operation time, indirectly affecting the time of postoperative healing; when the DMPT ratio is higher than 2.8wt%, the operation time and / or solidification time will be too short, which will cause the medical staff to fail to operate in time, or the bone cement will solidify too early, greatly increasing the risk of surgical failure.
[0030] In the liquid solution, the proportion of methyl methacrylate monomer is 97.2-97.8 wt %, preferably 97.4-97.6 wt %.
[0031] The weight ratio of the solid powder to the liquid solution is about 20:10 to 23:10, preferably 21:10 to 22:10.
[0032] In the liquid solution, the amount of hydroquinone (hereinafter referred to as HQ) is about 80 ppm of the liquid solution, which is feasible within the range of the allowable error (generally 10% of the amount).
[0033] The determination of the operation time and the solidification time of the mixing of the solid powder and the liquid solution, as well as the determination of the compressive strength of the bone cement after the polymerization reaction, are all carried out according to the method described in ISO 5833. DETAILED DESCRIPTION
[0034] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the specific embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0035] To further illustrate the technology of the present invention, the following is described through preferred embodiments:
[0036] Embodiment 1:
[0037] 12 g of methyl methacrylate-styrene copolymer containing 1.2 wt % BPO (purchased from Esschem), 2.4 g of PMMA (purchased from Esschem), and 5.6 g of barium sulfate (purchased from Sigma-Aldrich) were uniformly mixed to form 20 g of solid powder; 9.75 ml of MMA (specific gravity 0.94) containing 80 ppm HQ (purchased from Esschem) and 0.25 ml of DMPT (specific gravity 0.935) were also taken to form a liquid solution; the two were uniformly mixed, and the operation time was measured to be about 7 minutes and 50 seconds, and the solidification time was about 13 minutes and 15 seconds; after the bone cement was solidified, its compressive strength was measured to be 107 MPa (determined by Liangyu Biotechnology Co., Ltd.).
[0038] Embodiment 2:
[0039] The solid powder was changed to 20 g of methyl methacrylate-styrene copolymer containing 1.2 wt% BPO, 11.5 g of PMMA, and 5.7 g of barium sulfate; the liquid solution ratio and dosage were the same as in Example 1. The operation time was measured to be about 8 minutes and 55 seconds, and the solidification time was about 14 minutes and 25 seconds; after the bone cement was solidified, its compressive strength was measured to be 103 MPa.
[0040] Embodiment 3:
[0041] The solid powder was changed to 20 g of methyl methacrylate-styrene copolymer containing 1.2 wt% BPO, 2.6 g of PMMA, and 5.4 g of barium sulfate; the liquid solution ratio and dosage were the same as in Example 1. The operation time was measured to be about 7 minutes and 35 seconds, and the solidification time was about 13 minutes and 5 seconds; after the bone cement was solidified, its compressive strength was measured to be 112 MPa.
[0042] Embodiment 4:
[0043] The solid powder was changed to 20 g of methyl methacrylate-styrene copolymer containing 1.2 wt% BPO, 2.0 g of PMMA, and 6.0 g of barium sulfate; the liquid solution ratio and dosage were the same as in Example 1. The operation time was measured to be about 6 minutes and 30 seconds, and the solidification time was about 12 minutes and 45 seconds; after the bone cement was solidified, its compressive strength was measured to be 98 MPa.
[0044] Embodiment 5:
[0045] The solid powder was changed to 21g of solid powder, which was uniformly mixed with 12.6g of methyl methacrylate-styrene copolymer containing 1.2wt% BPO, 2.5g of PMMA, and 5.9g of barium sulfate; the liquid solution ratio and dosage were the same as those in Example 1. The operation time was measured to be about 6 minutes and 50 seconds, and the solidification time was about 12 minutes and 35 seconds; after the bone cement was solidified, its compressive strength was measured to be 114MPa.
[0046] Embodiment 6:
[0047] The solid powder was changed to 19 g of methyl methacrylate-styrene copolymer containing 1.2 wt% BPO, 2.3 g of PMMA, and 5.3 g of barium sulfate; the liquid solution ratio and dosage were the same as in Example 1. The operation time was measured to be about 8 minutes and 30 seconds, and the solidification time was about 13 minutes and 55 seconds; after the bone cement was solidified, its compressive strength was measured to be 106 MPa.
[0048] Embodiment 7:
[0049] The liquid solution was prepared by 9.72 ml of MMA containing 80 ppm HQ and 0.28 ml of DMPT; the solid powder ratio and dosage were the same as in Example 1. The operation time was measured to be about 8 minutes and 10 seconds, and the solidification time was about 13 minutes and 20 seconds; after the bone cement was solidified, its compressive strength was measured to be 118 MPa.
[0050] Embodiment 8:
[0051] The liquid solution was changed to 9.78 ml of MMA containing 80 ppm HQ and 0.22 ml of DMPT; the solid powder ratio and dosage were the same as in Example 1. The operation time was measured to be about 7 minutes and 40 seconds, and the solidification time was about 12 minutes and 50 seconds; after the bone cement was solidified, its compressive strength was measured to be 101 MPa.
[0052] The above embodiments of the present invention focus on the differences between the various embodiments. As long as the different optimization features between the various embodiments are not contradictory, they can be combined to form a better embodiment. Considering the simplicity of the text, they will not be repeated here.
[0053] The above description is only an embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent substitution, improvement, etc. made within the spirit and principle of the present invention should be included in the scope of the claims of the present invention.
Claims
1. A bone cement composition, It is characterized in that include: A solid powder comprising: 57-63 wt % of methyl methacrylate-styrene copolymer, 9-15 wt % of polymethyl methacrylate, 22-34 wt % of developer, and about 1.0-2.0 wt % of BPO; and A liquid solution comprising: 97.2-97.8 wt % of methyl methacrylate (MMA) monomer, 2.2-2.8 wt % of N,N-dimethyl-p-toluidine (DMPT), and about 80 ppm of hydroquinone; The weight ratio of the solid powder to the liquid solution is approximately between 20:10 and 23:10, so that the slurry formed after uniform mixing has an operation time of 5 to 10 minutes and a solidification time of 10 to 15 minutes; and the compressive strength of the bone cement after the polymerization reaction is 90 to 120 MPa.
2. The bone cement composition according to claim 1, It is characterized in that The proportion of the methyl methacrylate-styrene copolymer in the solid powder is 58-62 wt %.
3. The bone cement composition according to claim 1, It is characterized in that The developer is barium sulfate.
4. The bone cement composition according to claim 3, It is characterized in that The barium sulfate is contained in the solid powder in an amount of 26-30 wt %.
5. The bone cement composition according to claim 1, It is characterized in that The polymethyl methacrylate is contained in the solid powder in a ratio of 10 to 14 wt %.
6. The bone cement composition according to claim 1, It is characterized in that The proportion of methyl methacrylate in the liquid solution is 97.4-97.6 wt %.
7. The bone cement composition according to claim 1, It is characterized in that The weight ratio of the solid powder to the liquid solution is 21:10 to 22:10.