Flotation reagent and method for flotation separation of micro-fine particle cassiterite and magnesium-containing gangue minerals

Through the combined use of phosphonic acid nano-colloidal collector and hydroxyl polysaccharide compounds, the problem of recovering fine-grained cassiterite and magnesium-containing gangue minerals in the flotation process is solved, and efficient collection of cassiterite and magnesium gangue is achieved. Mineral suppression improves the recovery efficiency and concentrate grade of tin resources.

CN118847375AActive Publication Date: 2024-10-29CENT SOUTH UNIV
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411242947.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-10-29
Estimated Expiration
2044-09-05

AI Technical Summary

Technical Problem

Existing technology is difficult to effectively recover fine-grained cassiterite and magnesium-containing gangue minerals, resulting in loss of tin resources and low recovery efficiency. Especially during the flotation process, the collection and selectivity of fine-grained cassiterite are insufficient, and common inhibitors are not effective. Prevent suspended magnesium-containing gangue minerals from entering the concentrate product.

Method used

Using a combination of phosphonic acid nano-colloidal collectors formed by coordination and assembly of phosphonic acid compounds and metal ions of more than two valences and hydroxyl polysaccharide compounds as inhibitors, the phosphonic acid nano-colloidal collectors achieve the targeting of fine-grained cassiterite Aggregation and efficient collection, hydroxyl polysaccharide compounds inhibit the floatability of magnesium-containing gangue minerals through hydroxyl activation and flocculation activation.

Benefits of technology

It achieves efficient collection of fine-grained cassiterite and selective suppression of magnesium-containing gangue minerals, improving the recovery rate of tin resources and concentrate grade. The tin grade is 5.55% to 10.24%, and the tin recovery rate is 31.65% to 45.37%. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118847375A_ABST
    Figure CN118847375A_ABST
Patent Text Reader

Abstract

The invention discloses a flotation reagent and a method for flotation separation of micro-fine particle cassiterite and magnesium-containing gangue minerals, and belongs to the technical field of mineral separation. The flotation reagent comprises a collecting agent and an inhibitor; the collecting agent is a phosphonic acid nano colloid collecting agent, and the phosphonic acid nano colloid collecting agent is formed by coordinating and assembling a phosphonic acid compound and metal ions with the valence higher than bivalent; the inhibitor is a hydroxyl polysaccharide compound; the collecting agent can promote targeted aggregation of micro-fine particle cassiterite, effective collection of the micro-fine particle cassiterite is achieved, the inhibitor can selectively generate a hydroxyl activation effect and an ex-site adsorption effect on magnesium sites on the surface of magnesium-containing gangue, hydrophilic activation and flocculation activation of magnesium-containing gangue minerals are achieved, and the purpose of collecting the micro-fine particle cassiterite is achieved. And selective inhibition of the magnesium-containing gangue minerals is achieved, and therefore efficient flotation separation of the micro-fine particle cassiterite and the magnesium-containing gangue minerals is enhanced under the combined action of the micro-fine particle cassiterite and the magnesium-containing gangue minerals.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a flotation agent, in particular to a flotation agent for separating fine cassiterite from magnesium-containing gangue minerals, and also to an agent and method for flotation separation of fine cassiterite and magnesium-containing gangue minerals, belonging to the technical field of mineral flotation. Background Art

[0002] Cassiterite (SnO2) is the main raw material for extracting tin metal in industry. The tin metal extracted from cassiterite is widely used in solder, optoelectronics, catalysis, tin chemical products and tinplate, and is one of the important resources for scientific and technological development. However, most tin resources exist in primary deposits. This type of tin resource is mainly formed during the evolution of magmatic hydrothermal fluids. When tin-containing hydrothermal fluids encounter magnesium-iron minerals such as biotite, they can be replaced to form minerals such as magnesium-rich chlorite, or contact carbonate-type surrounding rocks to form gangue minerals such as magnesium-rich tourmaline in the contact zone between hydrothermal fluids and surrounding rocks. The tin resources thus formed have the disadvantages of fine embedded particle size and complex associated components. Crushing and grinding operations must be carried out before mineral selection. Cassiterite is brittle and easy to mud. Crushing and grinding operations will inevitably lead to the fine mudification of part of the cassiterite, resulting in difficulty in flotation recovery and loss of tin resources. In addition, magnesium-containing clay gangue minerals such as magnesium-rich tourmaline and magnesium-rich chlorite are also easy to mud, which further hinders the recovery of fine-grained cassiterite.

[0003] At present, with the aggravation of the shortage of tin resources, attempts to recover fine-grained tin resources have been carried out in industry. Common cassiterite collectors at present are hydroxamic acid collectors. Such agents show good capture and selectivity in capturing conventional particle-grade cassiterite, but in the flotation process of fine-grained cassiterite, their capture and selectivity are obviously insufficient. Therefore, developing collectors suitable for fine-grained cassiterite is one of the key points of fine-grained tin resource recovery. In addition, the flotation separation of magnesium-containing gangue minerals and fine-grained cassiterite is also one of the research focuses. At present, common inhibitors such as water glass, sodium fluorosilicate and nano alkaline earth metal fluoride colloidal particles (CN109985731B) etc. have achieved the inhibition of magnesium-containing gangue minerals to a certain extent by enhancing the hydrophilicity of magnesium-containing gangue minerals. However, such inhibitors cannot effectively prevent the fine-grained magnesium-containing gangue minerals suspended in the ore pulp from entering the process of concentrate products with the fluid and foam layer, and it is difficult to achieve the effective enrichment and recovery of fine-grained cassiterite. Therefore, further research and development of agents and methods for flotation separation of fine-grained cassiterite and magnesium-containing gangue minerals to achieve efficient flotation enrichment of fine-grained cassiterite and efficient suppression of magnesium-containing gangue minerals is of great significance to the development and utilization of fine-grained tin resources. Summary of the invention

[0004] In view of the technical difficulties existing in the existing fine-grained cassiterite and magnesium-containing gangue minerals and flotation separation processes, the first object of the present invention is to provide a flotation agent for separating fine-grained cassiterite from magnesium-containing gangue minerals, wherein the collector in the flotation agent can achieve targeted aggregation of fine-grained cassiterite, increase the size of fine-grained cassiterite, and has the advantages of strong collecting ability, while the inhibitor used in combination can selectively activate the hydroxyl group and adsorb at the same site on the magnesium site on the surface of the magnesium-containing gangue, thereby achieving hydrophilic activation and flocculation activation of the magnesium-containing gangue minerals, so that the cooperation of the two can achieve selective inhibition of the magnesium-containing gangue minerals.

[0005] In order to achieve the above technical purpose, the present invention provides a flotation reagent for separating fine-grained cassiterite from magnesium-containing gangue minerals, wherein the flotation reagent comprises a collector and an inhibitor; the collector is a phosphonic acid nanocolloid collector; the phosphonic acid nanocolloid collector is assembled by coordination of a phosphonic acid compound and a divalent or higher metal ion; the phosphonic acid compound comprises at least one C6-C 18 and at least one phosphonic acid group; the inhibitor is a hydroxy polysaccharide compound.

[0006] The flotation reagent provided by the present invention comprises a phosphonic acid nano-colloidal collector and a hydroxy polysaccharide compound inhibitor. The phosphonic acid nano-colloidal collector has a targeted aggregation effect on fine-grained cassiterite, while the hydroxy polysaccharide compound has a hydrophilic activation and flocculation activation effect on magnesium-containing gangue minerals. The combination of the two enhances the flotation separation of fine-grained cassiterite and magnesium-containing gangue minerals, achieving a better separation effect. The phosphonic acid nano-colloid collector is formed by assembling phosphonic acid nano-colloids through chelating reactions between phosphonic acid compounds and high-valent metal ions. The obtained phosphonic acid nano-colloids have multiple active points that can achieve targeted attraction between the phosphonic acid nano-colloids themselves and between the phosphonic acid nano-colloids and fine-grained cassiterite, thereby promoting targeted aggregation of fine-grained cassiterite and achieving efficient capture and recovery of fine-grained cassiterite. The hydroxyl and carboxyl groups contained in the hydroxyl polysaccharide compounds can undergo hydroxyl activation and same-site adsorption with the abundant magnesium sites on the surface of magnesium-containing gangue minerals, thereby achieving hydrophilic activation and flocculation activation of the magnesium-containing gangue minerals, increasing the particle size and hydrophilic activity of the magnesium-containing gangue minerals, and reducing the floatability of the magnesium-containing gangue minerals, thereby achieving inhibition of the magnesium-containing gangue minerals.

[0007] The phosphonic acid compound of the present invention has C6~C 18 The long-chain alkyl group may be a straight-chain alkyl group or a branched-chain alkyl group.

[0008] As a preferred embodiment, the phosphonic acid compound includes at least one of hexylphosphonic acid, heptylphosphonic acid, octylphosphonic acid, dodecylaminobis(methylenephosphonic acid), dioctylphosphonic acid, 2-butyloctylphosphonic acid, and α-hydroxyhexylphosphonic acid.

[0009] The phosphonic acid nanocolloid collector of the present invention is formed by the coordination assembly of a phosphonic acid compound and a divalent or higher metal ion. There are multiple coordination assembly modes between the phosphonic acid compound and the divalent or higher metal ion. The phosphonic acid nanocolloid collector can be a mixture of multiple coordination assemblies or a single coordination assembly. The coordination assembly of a divalent metal ion and a long-chain alkylphosphonic acid is used as an example for explanation. The typical coordination assembly structure is as follows: etc.; where M is a divalent or higher metal ion; R is C6~C 18 Alkyl chain.

[0010] As a preferred solution, the divalent or higher metal ion is Pb 2+ 、Zn 2+ , Cu 2+ , Fe 3+ At least one of the following. Different central metal ions have different abilities to act on cassiterite by forming phosphonic acid nanocolloid collectors by coordination.

[0011] As a preferred solution, the coordination mass ratio of the phosphonic acid compound to the divalent or higher metal ion is 0.5:1 to 2:1.

[0012] The phosphonic acid nano-colloid collector of the present invention is a complex having a certain three-dimensional structure assembled by phosphonic acid compounds and divalent or higher metal ions through coordination and chelation. These complexes have nano-colloid properties, a large specific surface area, and a large number of active points on the surface, which can achieve targeted attraction between the phosphonic acid nano-colloids themselves and between the phosphonic acid nano-colloids and fine cassiterite particles, promote targeted aggregation of fine cassiterite particles, and thus achieve efficient collection of fine cassiterite particles.

[0013] As a preferred solution, the hydroxy polysaccharide compound is at least one of carboxymethyl cellulose, sodium carboxymethyl cellulose and guar gum. The preferred hydroxy polysaccharide compound undergoes hydroxyl activation and same-site adsorption with magnesium sites on the surfaces of minerals such as tourmaline and chlorite, which can achieve hydrophilic activation and flocculation activation of the surfaces of these minerals, increase the particle size and hydrophilic activity of these minerals, and thus inhibit their floatability.

[0014] The present invention also provides a method for flotation separation of fine-grained cassiterite and magnesia-containing gangue minerals, which comprises subjecting low-grade fine-grained tin ore containing magnesia gangue minerals to magnetic separation for iron removal and flotation desulfurization in sequence, and then using the flotation agent to perform flotation separation to obtain fine-grained cassiterite concentrate.

[0015] As a preferred solution, the magnesium-containing gangue mineral is at least one of tourmaline and chlorite.

[0016] As a preferred solution, the flotation separation includes one roughing process and 3 to 5 cleaning processes.

[0017] As a preferred solution, the flotation reagent system in the roughing process is: collector 500-1000 g / t; depressant 40-200 g / t. The collector is added in the form of a solution with a mass concentration of 2.5-5%. The depressant is added in the form of a solution with a mass concentration of 0.2-0.5%. Sodium carbonate is also used as a pH adjuster in the roughing process, and the amount of sodium carbonate used ranges from 500 to 1000 g / t.

[0018] As a preferred solution, the flotation reagent system in the concentration process is: 0.1-50g / t of depressant. The flotation reagent follows the principle of halving during the concentration process.

[0019] Under the optimal flotation process and reagent system, the final flotation froth concentrate product is cassiterite concentrate with a tin grade ranging from 5.55% to 10.24%, and a tin recovery rate of 31.65% to 45.37%.

[0020] The method for flotation separation of fine cassiterite and magnesium-containing gangue minerals of the present invention comprises the following specific steps:

[0021] (1) Iron removal: Low-grade fine-grained tin-containing ore is first subjected to magnetic separation to remove iron. The magnetic field strength is 1 to 1.2 T. The non-magnetic product obtained is concentrated. The concentrated slurry concentration is 40 to 50% to obtain the flotation ore.

[0022] (2) Desulfurization: The raw ore entering the flotation in step (1) is subjected to reverse flotation desulfurization treatment to remove the sulfide ore in the raw ore entering the flotation to obtain foam tailings and desulfurized concentrate in the tank. The desulfurization process is a conventional operation in the prior art.

[0023] (3) Floating tin: adding sodium carbonate as a pH adjuster to the desulfurized concentrate of step (2) and slurrying for 3-4 minutes, adding hydroxy polysaccharide compounds as an inhibitor and slurrying for 3-4 minutes, adding phosphonic acid nanocolloid collector and slurrying for 4-6 minutes, adding frother and slurrying for 0.5-1 minute, the flotation time is 4-6 minutes, and obtaining a flotation foam concentrate, the sodium carbonate as a pH adjuster is added in the form of a sodium carbonate solution with a mass percentage concentration of 1-10%, and the pure dry weight amount is 500-1000 g / (t·input ore); the hydroxy polysaccharide compounds as an inhibitor are added in the form of a mass percentage concentration of The inhibitor is added in the form of a 0.2-0.5% hydroxy polysaccharide solution, and the pure dry weight amount of the inhibitor hydroxy polysaccharide compound is 40-200 g / (t·the original ore to be floated); the phosphonic acid nano-colloid collector is added in the form of a nano-colloid solution with a mass concentration of 2.5-5%, and the pure dry weight amount of the phosphonic acid nano-colloid collector is 500-1000 g / (t·the original ore to be floated); the pH adjuster is sodium carbonate with a mass concentration of 5-10%, and the ratio of the amount of sodium carbonate to the amount of the collector is in the range of 0.8:1-1.2:1; the speed of the flotation machine is 1900-2100 r / min.

[0024] (4) Concentration: The flotation froth concentrate obtained in step (3) is used as the selected raw ore and subjected to 3 to 5 concentrating operations. In each concentrating operation, an inhibitor hydroxy polysaccharide compound is added and the slurry is adjusted for 3 minutes. The flotation time is 1 to 4 minutes to obtain the final flotation froth concentrate. The hydroxy polysaccharide compound is added in the form of a hydroxy polysaccharide solution with a mass percentage concentration of 0.2 to 0.5%, and the pure dry weight amount of the hydroxy polysaccharide compound is 0.1 to 50 g / (t·the raw ore to be floated).

[0025] (5) Flotation product processing: The final flotation foam concentrate product is filtered and dried to obtain a cassiterite concentrate with a tin grade of 5.55-10.24% and a tin recovery rate of 31.65%-45.37%.

[0026] Compared with the prior art, the beneficial technical effects brought by the technical solution of the present invention are:

[0027] The flotation reagent for separating fine-grained cassiterite from magnesium-containing gangue minerals provided by the present invention comprises a novel phosphonic acid nano-colloidal collector formed by coordination assembly of a phosphonic acid compound and a divalent or higher metal ion, which can achieve targeted aggregation of fine-grained cassiterite and increase the size of the fine-grained cassiterite, and has the advantage of strong capture performance, and can achieve efficient capture of fine-grained cassiterite. The flotation reagent also comprises a hydroxyl polysaccharide compound inhibitor, which can selectively cause hydroxyl activation and same-site adsorption at the magnesium site on the surface of the magnesium-containing gangue, and achieve hydrophilic activation and flocculation activation of the magnesium-containing gangue mineral, and achieve selective inhibition of the magnesium-containing gangue mineral. The combined use of the phosphonic acid nano-colloidal collector and the hydroxyl polysaccharide compound inhibitor can enhance the flotation separation effect between fine-grained cassiterite and magnesium-containing gangue, and finally can obtain a cassiterite concentrate with a tin grade of 5.55-10.24%, and a tin recovery rate of 31.65-45.37%. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is a flotation process flow chart for Example 2 and Example 3.

[0029] Figure 2 This is the monomer dissociation diagram of cassiterite in the fine-grained tin-containing ore from a certain place in Example 2.

[0030] Figure 3 The infrared spectrum of the phosphonic acid nanocolloid collector prepared in Example 1 (taking dodecylaminobis(methylenephosphonic acid) and lead ions as coordination examples); Figure 3 Middle 3199.91cm -1 Produced by asymmetric stretching vibration of OH or NH vibration; 2956.88cm -1 、2922.16cm -1 、2852.72cm-1 The absorption peaks near are generated by -CH3 and -CH2- components; 1454.33 cm -1 、1384cm -1 and 866.04cm -1 The nearby peak is caused by CH vibration; 1120.64cm -1 Produced by P=O bond vibration and 1045.42cm -1 It is generated by the vibration of PO bond, 690.52cm -1 and 470.63cm -1 Produced by O-Pb vibration. DETAILED DESCRIPTION

[0031] The content of the present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments of the specification. The protection scope of the claims of the present invention is not limited to the described content.

[0032] Example 1

[0033] The synthesis method of phosphonic acid nano-colloid collector is as follows:

[0034] Take the synthesis of phosphonic acid nanocolloid collector from dodecylaminobis(methylenephosphonic acid) and lead ions as an example: dodecylaminobis(methylenephosphonic acid) is placed in a sodium hydroxide solution with a mass fraction of 5% to prepare a dodecylaminobis(methylenephosphonic acid) solution with a mass fraction of 1%, and ultrapure water is used to prepare a lead nitrate solution with a concentration of 0.07 mol / L. 20g of dodecylaminobis(methylenephosphonic acid) solution is placed in a beaker, and the beaker is placed in a constant temperature water bath pot with an ultrasonic generator, the magnetic stirring system and the ultrasonic generator are turned on and heated to 80°C, the lead ion solution is slowly added to the bisphosphonic acid solution under magnetic stirring at a rate of 0.01mL / s, and the mass ratio of lead nitrate and diphosphoric acid is 1:1. After the addition is completed, the constant temperature is maintained for 1h to obtain a phosphonic acid nanocolloid collector solution. Finally, the collector solution is placed in a vacuum oven at 45°C and dried for about 48h to obtain a solid phosphonic acid nanocolloid collector.

[0035] Example 2

[0036] The example uses a low-grade fine-grained tin-containing tailings from a certain place with a tin grade of about 0.16%, and the main gangue minerals are magnesium tourmaline, etc. Figure 2 As shown, the content of magnesia tourmaline is about 50%. The phosphonic acid nano-colloid collector synthesized in Example 1 is a collector for cassiterite, and sodium carboxymethyl cellulose is an inhibitor for magnesia gangue mineral magnesia tourmaline. Among them, sodium carboxymethyl cellulose and sodium carbonate are analytically pure, and the phosphonic acid nano-colloid collector is industrially pure, and the application is carried out according to the following steps:

[0037] (1) Iron removal: A vertical ring high gradient magnetic separator is used to remove iron from fine tin-containing tailings to remove magnetic iron impurities mainly composed of siderite. The magnetic field strength is selected to be 1.2T to obtain non-magnetic products and concentrate the slurry to a concentration of 45% as the raw ore for flotation;

[0038] (2) Desulfurization: The raw ore for floating in step (1) is added to a hanging tank flotation machine. The desulfurization operation includes a roughing selection, a fine selection and a scavenging selection. The sulfide ore activator is copper sulfate, and the sulfide ore collector is xanthate. The amount of copper sulfate used in the roughing selection is 100 g / (t·raw ore for floating), the amount of xanthate used in the roughing selection is 200 g / (t·raw ore for floating), no agent is added in the fine selection, and the amount of xanthate used in the scavenging selection is 100 g / (t·raw ore for floating), to obtain foam tailings and desulfurized concentrate in the tank.

[0039] (3) Floating tin: 1000 g / (t·floating ore) of 5% sodium carbonate solution is added to the desulfurized concentrate slurry in the tank obtained in step (2) and the slurry is adjusted for 3 minutes, 50 g / (t·floating ore) of 0.5% sodium carboxymethyl cellulose is added and the slurry is adjusted for 3 minutes, 1000 g / (t·floating ore) of phosphonic acid nanocolloid collector is added and the slurry is adjusted for 5 minutes, a frother is added and the slurry is adjusted for 1 minute, and positive flotation is performed to obtain a foam concentrate product and a tailings product in the tank;

[0040] (4) Concentration: The foam concentrate product of step (3) is subjected to five concentration operations, in each of which sodium carboxymethyl cellulose (added in the form of a solution with a mass percentage concentration of 0.5%) is used as an inhibitor and the slurry is adjusted for 3 minutes. The amounts of sodium carboxymethyl cellulose used in the first to fifth passes are 10 g / (t·the original ore to be floated), 2 g / (t·the original ore to be floated), 1 g / (t·the original ore to be floated), 0.5 g / (t·the original ore to be floated), and 0.1 g / (t·the original ore to be floated), respectively, to obtain a final foam product;

[0041] (5) Flotation product processing: The tailings product obtained in step (3) and the final foam product of step (4) are filtered, dried, weighed, and the grade is tested and the product indicators are calculated. The tin grade in the final tin concentrate is flotation. The final flotation foam concentrate product is filtered and dried to obtain a cassiterite concentrate with a tin grade of 10.24%, and the tin recovery rate is 34.05%.

[0042] Example 3

[0043] The tin grade of the fine-grained tin resource in a certain place used in the example is about 0.23%, and the main gangue minerals are chlorite, etc., among which the chlorite content is about 40%, which has the characteristics of high mudification and great difficulty in inhibition. The process of Example 1 is used to synthesize the tin-containing resource based on heptylphosphonic acid + Pb 2+ / Cu 2+ , dioctylphosphonic acid + Pb 2+ / Zn 2+ , α-Hydroxyhexylphosphonic acid + Pb 2+ / Fe 3+ Phosphonic acid nanocolloid collector is used as an example of flotation collector, and hydroxy polysaccharide compound guar gum is used as a chlorite inhibitor. Guar gum and pH adjuster sodium carbonate are analytically pure, and cassiterite collector is industrially pure. The application is carried out according to the following steps:

[0044] (1) Iron removal: A vertical ring high gradient magnetic separator is used to remove iron from fine tin-containing tailings to remove magnetic iron impurities. The magnetic field strength is selected to be 1.2T to obtain non-magnetic products and concentrate the slurry to a concentration of 45% as the raw ore for flotation;

[0045] (2) Desulfurization: The raw ore for floating in step (1) is added to a hanging tank flotation machine. The desulfurization operation includes a roughing selection, a fine selection and a scavenging selection. The sulfide ore activator is copper sulfate, and the sulfide ore collector is xanthate. The amount of copper sulfate used in the roughing selection is 200 g / (t·raw ore for floating), the amount of xanthate used in the roughing selection is 200 g / (t·raw ore for floating), no agent is added in the fine selection, and the amount of xanthate used in the scavenging selection is 100 g / (t·raw ore for floating), to obtain foam tailings and desulfurized concentrate in the tank.

[0046] (3) Floating tin: 750 g / (t·floating ore) of 5% sodium carbonate solution is added to the desulfurized concentrate slurry in the tank obtained in step (2) and the slurry is adjusted for 3 minutes, 150 g / (t·floating ore) of 0.5% guar gum is added and the slurry is adjusted for 3 minutes, 1000 g / (t·floating ore) of different phosphonic acid nanocolloid collectors are added and the slurry is adjusted for 5 minutes, a frother is added and the slurry is adjusted for 1 minute, and positive flotation is performed to obtain a foam concentrate product and a tailings product in the tank;

[0047] (4) Concentration: The foam concentrate product of step (3) is subjected to four concentrating operations, and guar gum (added in the form of a solution with a mass percentage concentration of 0.5%) is used as an inhibitor in each concentrating operation and the slurry is adjusted for 3 minutes. The amounts of guar gum used in the first to fourth concentrating operations are 40 g / (t·the raw ore to be floated), 30 g / (t·the raw ore to be floated), 15 g / (t·the raw ore to be floated), and 10 g / (t·the raw ore to be floated), respectively, to obtain the final foam product;

[0048] (5) Flotation product processing: The tailings product obtained in step (3) and the final foam product in step (4) are filtered, dried, weighed, and graded, and the product indexes are calculated. The flotation indexes of the final flotation tin concentrate are shown in Table 1.

[0049] Table 1 Phosphonic acid nano-colloid collector flotation concentrate index

[0050]

[0051] Comparative Example 1

[0052] The raw ore used in this example is the non-magnetic product after iron removal in Example 2, with a tin grade of about 0.21%. The difference in the effect of other conventional inhibitors on inhibiting magnesium tourmaline and hydroxy polysaccharide compound carboxymethyl cellulose is listed. Sodium fluorosilicate, carboxymethyl cellulose, and pH adjuster sodium carbonate are analytically pure, and the phosphonic acid nanocolloid collector (synthesized in Example 1) and water glass are industrially pure. The application is carried out according to the following steps:

[0053] (1) Desulfurization: The raw ore to be floated is added to the hanging tank flotation machine, followed by a desulfurization roughing operation. Copper sulfate and xanthate are used as activators and collectors for the sulfide ore, respectively. The amount of copper sulfate is 100g / (t·raw ore to be floated), and the amount of xanthate is 200g / (t·raw ore to be floated), to obtain foam tailings and desulfurized concentrate in the tank.

[0054] (2) Floating tin: adding 1000 g / (t·floating ore) of 5% sodium carbonate solution to the desulfurized concentrate slurry in the tank obtained in step (1) and mixing the slurry for 3 min, adding inhibitors of different types and amounts and mixing the slurry for 3 min, adding 1000 g / (t·floating ore) of phosphonic acid nanocolloid collector and mixing the slurry for 5 min, adding a frother and mixing the slurry for 1 min, performing positive flotation and scraping to obtain a foam concentrate product and a tailings product in the tank;

[0055] (3) Concentration: The foam concentrate product of step (2) is subjected to a blank concentration operation to obtain a refined concentrate product.

[0056] (4) Flotation product processing: The tailings product obtained in step (2) and the final froth product in step (3) are filtered, dried, weighed, and graded, and product indicators are calculated to obtain concentrate products using different types and amounts of inhibitors.

[0057] Among them, the inhibitors of different types and amounts in step (2) include 50, 100, 200 g / (t·raw ore to be floated) sodium fluorosilicate (pure dry weight), 200, 400, 600, 1000 g / (t·raw ore to be floated) water glass (stock solution), 50, 100 g / (t·raw ore to be floated) hydroxyl polysaccharide compound carboxymethyl cellulose, and the final flotation index is shown in Table 2.

[0058] It is difficult to achieve efficient inhibition of magnesia tourmaline with other conventional inhibitors such as sodium fluorosilicate and water glass. However, the hydroxy polysaccharide compound carboxymethyl cellulose can effectively inhibit magnesia tourmaline at a lower dosage and under the condition of blank selection. The tin grade is increased from 0.2% to 1.15-1.39%, and the recovery rate of tin in the concentrate is maintained at a high level, reaching 41.42-53.56%.

[0059] Table 2 Flotation results of concentrate under different depressant conditions

[0060]

[0061] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

[0062] Comparative Example 2

[0063] The raw ore used in this example is the same as that used in comparative example 1, and the tin grade is about 0.21%. The difference in flotation of cassiterite between the phosphonic acid nanocolloid collector synthesized in comparative example 1 and the dodecylaminobis(methylenephosphonic acid) collector is shown in the following steps:

[0064] (1) Desulfurization: The raw ore to be floated is added to the hanging tank flotation machine, followed by a desulfurization roughing operation. Copper sulfate and xanthate are used as activators and collectors for the sulfide ore, respectively. The amount of copper sulfate is 100g / (t·raw ore to be floated), and the amount of xanthate is 200g / (t·raw ore to be floated), to obtain foam tailings and desulfurized concentrate in the tank.

[0065] (2) Floating tin: adding 1000 g / (t·floating ore) of 5% sodium carbonate solution to the desulfurized concentrate slurry in the tank obtained in step (1) and mixing the slurry for 3 min, adding 50 g / (t·floating ore) of sodium carboxymethyl cellulose as an inhibitor and mixing the slurry for 3 min, adding 1000 g / (t·floating ore) of different collectors and mixing the slurry for 5 min, adding a frother and mixing the slurry for 1 min, performing positive flotation and scraping to obtain a foam concentrate product and a tailings product in the tank;

[0066] (3) Concentration: The foam concentrate product of step (2) is subjected to a blank concentration operation to obtain a refined concentrate product.

[0067] (4) Flotation product processing: The tailings product obtained in step (2) and the final foam product in step (3) are filtered, dried, weighed, and graded, and the product indicators are calculated to obtain the first concentrate product using different types and amounts of inhibitors. The final flotation indicators are shown in Table 3.

[0068] Compared with single dodecylaminobis(methylenephosphonic acid) as cassiterite flotation collector, the phosphonic acid nanocolloid collector synthesized in Example 1 exhibits better collection ability and selectivity for cassiterite, and is more likely to achieve effective enrichment of low-grade fine-particle tin-containing minerals.

[0069] Table 3 Comparison of concentrate indexes of single phosphonic acid collector and phosphonic acid nanocolloid collector

[0070]

Claims

1. A flotation agent for separating fine cassiterite from magnesium-containing gangue minerals, characterized in that: The flotation reagents include collectors and depressants; The collector is a phosphonic acid nano-colloid collector; The phosphonic acid nanocolloid collector is assembled by coordination of a phosphonic acid compound and a divalent or higher metal ion; The phosphonic acid compound contains at least one C6-C 18 A long-chain alkyl group and at least one phosphonic acid group; The inhibitor is a hydroxy polysaccharide compound.

2. A flotation agent for separating fine-grained cassiterite from magnesium-containing gangue minerals according to claim 1, characterized in that: The divalent or higher metal ion is Pb 2+ 、Zn 2+ , Cu 2+ , Fe 3+ At least one of them.

3. A flotation agent for separation of fine cassiterite and magnesium-containing gangue minerals according to claim 1, characterized in that: The phosphonic acid compound includes at least one of hexylphosphonic acid, heptylphosphonic acid, octylphosphonic acid, dodecylaminobis(methylenephosphonic acid), dioctylphosphonic acid, 2-butyloctylphosphonic acid, and α-hydroxyhexylphosphonic acid.

4. A flotation agent for separating fine cassiterite from magnesium-containing gangue minerals according to any one of claims 1 to 3, characterized in that: The coordination mass ratio of the phosphonic acid compound to the divalent or higher metal ions is 0.5:1 to 2:

1.

5. A flotation agent for separation of fine cassiterite and magnesium-containing gangue minerals according to claim 1, characterized in that: The hydroxy polysaccharide compound is at least one of carboxymethyl cellulose, sodium carboxymethyl cellulose and guar gum.

6. A method for flotation separation of fine cassiterite and magnesium-containing gangue minerals, characterized in that: After magnetic separation for iron removal and flotation desulfurization of low-grade fine-grained tin ore containing magnesia gangue minerals, flotation separation is performed using the flotation agent described in any one of claims 1 to 5 to obtain fine-grained cassiterite concentrate.

7. The method for flotation separation of fine-grained cassiterite and magnesium-containing gangue minerals according to claim 6, characterized in that: The magnesium-containing gangue mineral is at least one of tourmaline and chlorite.

8. A method for flotation separation of fine cassiterite and magnesium-containing gangue minerals according to claim 6 or 7, characterized in that: The flotation separation includes one roughing process and 3 to 5 cleaning processes.

9. The method for flotation separation of fine-grained cassiterite and magnesium-containing gangue minerals according to claim 6, characterized in that: The flotation reagent system in the roughing process is: collector 500-1000g / t; depressant 40-200g / t.

10. The method for flotation separation of fine-grained cassiterite and magnesium-containing gangue minerals according to claim 6, characterized in that: The flotation reagent system in the concentration process is: depressant 0.1 ~ 50g / t.

Citation Information

Patent Citations

  • A high-magnesium sulfide mineral flotation inhibitor with slow-release conversion function and its application

    CN109985731B

  • Hydroximic acid-organic phosphoric acid multi-ligand metal complex collecting agent, and preparation method and application thereof

    CN110721816A

  • Combined flotation agent for inhibiting magnesium-containing silicate gangue minerals

    CN111359782A

  • Tin mineral collecting agent, preparation method and application

    CN113976327A

  • Preparation method and application of nanoparticle collecting agent

    CN117551130A