A method for preparing TC4 titanium alloy seamless tube

By improving the extrusion-rolling process, the problems of high production difficulty and mass production challenges of TC4 titanium alloy seamless tubes have been solved, realizing efficient mass production of TC4 titanium alloy seamless tubes and optimizing tube performance and yield.

CN118847747BActive Publication Date: 2026-11-17CHENGDU ADVANCED METAL MATERIALS IND TECH RES INST CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410818228.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-24
Publication Date
2026-11-17
Estimated Expiration
2044-06-24

AI Technical Summary

Technical Problem

TC4 titanium alloy seamless tubes are difficult to produce, difficult to mass-produce, have a low yield, require high-end equipment, and are prone to cracking.

Method used

An improved extrusion-rolling process is adopted, including high-vacuum non-consumable electric arc furnace melting, double-layer cladding extrusion, and alternating hot and cold rolling. The melting method, extrusion and rolling process parameters are controlled, and the annealing treatment is optimized.

Benefits of technology

This technology enables the mass production of seamless TC4 titanium alloy tubes, reducing equipment requirements and wear, increasing yield, and optimizing tube microstructure and properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118847747B_ABST
    Figure CN118847747B_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing TC4 titanium alloy seamless tubes, belonging to the technical field of titanium alloy seamless tubes and their preparation methods. The method includes: preparing raw materials; placing the raw materials into a high-vacuum non-consumable arc furnace and evacuating it; first filling the high-vacuum non-consumable arc furnace with hydrogen and argon before starting melting; forging the obtained TC4 titanium alloy ingot to obtain an extrusion billet; after double-layering the billet surface with copper and iron, extruding it, and then annealing the billet; hot rolling; cold rolling; repeating hot rolling and cold rolling until a TC4 titanium alloy seamless tube meeting dimensional requirements is obtained. The method for preparing TC4 titanium alloy seamless tubes of this invention achieves mass production of TC4 titanium alloy seamless tubes by controlling the melting method, extrusion, and rolling, solving the problems of high production difficulty and easy cracking caused by the large deformation resistance and strong work hardening of this tube.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the technical field of seamless titanium alloy tubes and their preparation methods, specifically relating to a preparation method of TC4 titanium alloy seamless tubes. Background Technology

[0002] TC4 (Ti-6Al-4V) is a typical α-type two-phase titanium alloy with advantages such as high specific strength, low density, good thermal stability and corrosion resistance. It is used to manufacture seamless titanium alloy tubes, which have broad application prospects in many fields such as marine engineering, shipbuilding, aerospace, chemical industry, automobile and power.

[0003] There are various methods for manufacturing titanium and titanium alloy tubes, mainly including hot extrusion, hot rolling, cold deformation, and welding, or a combination of these methods.

[0004] TC4 titanium alloy exhibits high deformation resistance, strong work hardening, and a tendency to crack, making its seamless tube production challenging. Furthermore, mass production of TC4 titanium alloy seamless tubes is difficult, requiring sophisticated equipment, resulting in high wear and tear and a low yield.

[0005] Based on the above, it is necessary to develop a method for producing TC4 titanium alloy seamless tubes that is simple, can be mass-produced, and has good performance. Summary of the Invention

[0006] Based on this, and to address the shortcomings of the prior art, a method for preparing TC4 titanium alloy seamless tubes is provided. This method improves the extrusion-rolling process of TC4 alloy tubes, aiming to provide a feasible preparation process for the industrial production of TC4 titanium alloy seamless tubes.

[0007] To achieve the above objectives, the following technical solution is adopted: This invention provides a method for preparing a seamless TC4 titanium alloy tube, comprising the following steps: S101. Prepare the raw materials for TC4 titanium alloy: 0A grade small-particle sponge titanium, AlV55 alloy and aluminum granules; S102. Place the raw materials, grade 0A small-particle sponge titanium, AlV55 alloy and aluminum granules, into a high-vacuum non-consumable arc furnace and evacuate the vacuum. S103. First, hydrogen gas is introduced into the high vacuum non-consumable arc furnace, followed by argon gas, and smelting begins to obtain TC4 titanium alloy ingots. S104. The TC4 titanium alloy ingot is forged to obtain the extrusion billet raw material; the surface of the extrusion billet raw material is coated with a double layer of copper and iron, and then extruded. After extrusion, the billet is air-cooled to room temperature; then the billet is annealed. S105. Hot rolling of the tube blank; S106. Cold rolling of the tube blank; S107. Repeat S105 to S106 until a TC4 titanium alloy seamless tube that meets the dimensional requirements is obtained, and then perform annealing treatment to obtain the finished TC4 titanium alloy seamless tube.

[0008] In some embodiments, the annealing process in S104 is as follows: annealing in a horizontal vacuum annealing furnace at a temperature of 10°C / min to 850-900°C for 2-3 hours, followed by furnace cooling to 500°C and then air cooling to room temperature.

[0009] In some embodiments, the annealing process in S107 is as follows: the TC4 titanium alloy seamless tube is heated to 550-580°C in a horizontal vacuum annealing furnace at a rate of 7-10°C / min for 1-1.5 hours, and then furnace cooled to room temperature.

[0010] In some embodiments, in S101, 880-920 kg of 0A grade small-particle titanium sponge, 50-70 kg of AlV55 alloy, and 30-50 kg of aluminum granules are fed.

[0011] In some embodiments, the extrusion process in S104 includes: heating the double-coated extrusion billet raw material to 860-920℃ and holding it at that temperature for 1-2 hours before extrusion, with an extrusion ratio of 6-9 and an extrusion speed controlled at 60-80 mm / s.

[0012] In some embodiments, S102, "placing raw material 0A grade small-particle sponge titanium, AlV55 alloy and aluminum granules into a high-vacuum non-consumable arc furnace and drawing a vacuum", includes: Place the raw materials, 0A grade small-particle sponge titanium, AlV55 alloy, and aluminum granules, into the copper crucible of a high-vacuum non-consumable arc furnace. Close the furnace door, start the mechanical pump, turn on the digital vacuum gauge, and open the pre-evacuation valve. Wait until the vacuum level inside the furnace drops to 5 × 10⁻⁶. -3 When Pa, close the main pump valve, close the shut-off valve, close the digital vacuum gauge, and when the molecular pump speed is zero, turn off the molecular pump power supply. In some embodiments, step S103, "first introducing hydrogen gas into a high-vacuum non-consumable arc furnace, then introducing argon gas, and starting the melting process to obtain a TC4 titanium alloy ingot," includes: Open the charging valve and keep the mechanical pump running, ensuring no air gets into the charging pipes, and wait until the vacuum level inside the furnace reaches 5 x 10⁻⁶. -4 Pa, close the charging valve, turn off the mechanical pump, open the hydrogen cylinder and charging valve. When the total gas pressure in the furnace is -0.05MPa, charge in 0.01MPa hydrogen and then open the argon cylinder to charge in 0.04MPa argon.

[0013] In some embodiments, hydrogen accounts for 20% of the total volume of gas in the furnace.

[0014] In some embodiments, in S104, the TC4 titanium alloy ingot is forged 6 times to obtain the extruded billet raw material.

[0015] In some embodiments, the hot rolling parameters of S105 include: hot rolling temperature of 900-950℃, deformation per pass of 30-50%, final rolling temperature of ≥800℃, feed rate of 3-5mm / pass, and rolling speed of 80-100 passes / minute.

[0016] In some embodiments, the cold rolling parameters of S106 include: the deformation amount per cold rolling pass is controlled at 20-30%, the rolling speed is 40-60 times / minute, the intermediate annealing temperature is 800-850℃, and the annealing time is 1.5-2.5h.

[0017] The present invention has the following beneficial technical effects: The method for preparing TC4 titanium alloy seamless tubes disclosed in this invention achieves mass production of TC4 titanium alloy seamless tubes by controlling the melting method, extrusion and rolling process paths, which solves the problems of high production difficulty and easy cracking caused by the large deformation resistance and strong work hardening of this tube.

[0018] The method for preparing TC4 titanium alloy seamless tubes disclosed in this invention uses a high-vacuum non-consumable melting method to obtain more uniform ingots with a short melting time, which is suitable for melting refractory metals such as titanium. The method for preparing TC4 titanium alloy seamless tubes disclosed in this invention reduces the forming temperature of titanium alloys and improves their plasticity through a hot hydrogen treatment process.

[0019] The method for preparing TC4 titanium alloy seamless tubes disclosed in this invention adopts an alternating hot and cold rolling process, which reduces the cost of pure hot rolling process, while optimizing the tube structure and properties during cold rolling annealing.

[0020] The method for preparing TC4 titanium alloy seamless tubes disclosed in this invention involves double-layering a titanium alloy extrusion billet, heating it, and then extruding it to achieve mass production of titanium alloy seamless tubes. Attached Figure Description

[0021] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0022] Figure 1 This is a flowchart of the preparation method of the TC4 titanium alloy seamless tube of the present invention; Figure 2The microstructure of the finished titanium alloy seamless tube of Embodiment 1 of the present invention is shown in the figure; wherein, (a) is a colored microstructure of the finished tube; and (b) is a grayscale microstructure of the finished tube. Figure 3 The microstructure of the finished titanium alloy seamless tube of Embodiment 2 of the present invention is shown in the figure; wherein, (a) is a colored microstructure of the finished tube; and (b) is a grayscale microstructure of the finished tube. Figure 4 The microstructure of the finished titanium alloy seamless tube is shown in the comparative example of the present invention; wherein, (a) is a colored microstructure of the finished tube; and (b) is a grayscale microstructure of the finished tube. Detailed Implementation

[0023] To make the objectives, technical solutions, and advantages of this invention clearer, the embodiments of this invention will be further described in detail below with reference to specific examples and the accompanying drawings. Obviously, the described embodiments are only some, not all, of the embodiments of this invention. All other embodiments obtained by those skilled in the art based on the embodiments of this invention without inventive effort are within the scope of protection of this invention.

[0024] like Figure 1 The method for preparing the TC4 titanium alloy seamless tube shown includes the following steps: S101. Prepare the raw materials for TC4 titanium alloy: 0A grade small-particle sponge titanium, AlV55 alloy and aluminum granules; S102. Place the raw materials 0A grade small-particle sponge titanium, AlV55 alloy and aluminum granules into a high vacuum non-consumable arc furnace and evacuate the vacuum. S103. First, hydrogen gas is introduced into the high vacuum non-consumable arc furnace, followed by argon gas, and smelting begins to obtain TC4 titanium alloy ingots. S104. The TC4 titanium alloy ingot is forged to obtain the extrusion billet raw material; the surface of the extrusion billet raw material is coated with a double layer of copper and iron, and then extruded. After extrusion, the billet is air-cooled to room temperature; then the billet is annealed. S105. Hot rolling of the tube blank; S106. Cold roll the tube blank; S107. Repeat steps S105 to S106 until a TC4 titanium alloy seamless tube that meets the size requirements is obtained. Then, perform annealing treatment to obtain the finished TC4 titanium alloy seamless tube.

[0025] The alternating hot and cold rolling process reduces the cost of pure hot rolling, while the cold rolling annealing process optimizes the microstructure and properties of the tube.

[0026] Further, the annealing process in step S104 is as follows: annealing is carried out in a horizontal vacuum annealing furnace at a temperature of 10℃ / min to 850-900℃ for 2-3 hours, and then the furnace is cooled to 500℃ and then air-cooled to room temperature.

[0027] Further, the annealing process in step S107 is as follows: the TC4 titanium alloy seamless tube is heated to 550-580℃ in a horizontal vacuum annealing furnace at a rate of 7-10℃ / min for 1-1.5h, and then furnace cooled to room temperature.

[0028] Further, in step S104, the TC4 titanium alloy ingot is forged six times to obtain the extrusion billet raw material. The extrusion process in step S104 includes: heating the double-coated extrusion billet raw material to 860-920℃ and holding it for 1-2 hours before extrusion, with an extrusion ratio of 6-9 and an extrusion speed controlled at 60-80 mm / s.

[0029] After double-layer encapsulation of titanium alloy extrusion billets, heating and extrusion are carried out. By controlling process parameters such as heating method, heating temperature, holding time, extrusion ratio, and pressurization speed of the extrusion billets, the batch production of seamless titanium alloy tubes can be achieved. The encapsulation process reduces the extrusion pressure required during extrusion, lowers the requirements for equipment, and results in low loss and high yield.

[0030] Furthermore, step S102, "placing the raw materials 0A-grade small-particle sponge titanium, AlV55 alloy, and aluminum granules into a high-vacuum non-consumable arc furnace and evacuating the furnace," includes: Place the raw materials, 0A grade small-particle sponge titanium, AlV55 alloy, and aluminum granules, into the copper crucible of a high-vacuum non-consumable arc furnace. Close the furnace door, start the mechanical pump, turn on the digital vacuum gauge, and open the pre-evacuation valve. Wait until the vacuum level inside the furnace drops to 5 × 10⁻⁶. -3 When Pa, close the main pump valve, close the shut-off valve, close the digital vacuum gauge, and when the molecular pump speed is zero, turn off the molecular pump power supply. Furthermore, step S103, "first introducing hydrogen into a high-vacuum non-consumable arc furnace, then introducing argon to begin melting, and obtaining TC4 titanium alloy ingots," includes: Open the charging valve and keep the mechanical pump running, ensuring no air gets into the charging pipes, and wait until the vacuum level inside the furnace reaches 5 x 10⁻⁶. -4 At pressure Pa, close the charging valve and mechanical pump, turn on the gas analysis system, and open the hydrogen cylinder and charging valve. When the total gas pressure inside the furnace is -0.05 MPa, charge in 0.01 MPa of hydrogen, then open the argon cylinder and charge in 0.04 MPa of argon. The hydrogen accounts for 20% of the total gas volume inside the furnace. Throughout the process, the ratio of hydrogen to argon is controlled by the gas analysis system.

[0031] Hydrogen has long been considered a harmful element in metallic structural materials because it can cause phenomena such as hydrogen embrittlement. However, hydrogen can also be used as a temporary alloying element to improve the machinability of alloys. Thermal hydrogen treatment can lower the forming temperature of titanium alloys and improve their plasticity.

[0032] Further, in step S104, the TC4 titanium alloy ingot is forged 6 times to obtain the extruded billet raw material.

[0033] Furthermore, the parameters for hot rolling in step S105 include: hot rolling is carried out using a hot rolling mill, the hot rolling temperature is 900-950℃, the deformation per pass is controlled at 30-50%, the final rolling temperature is required to be ≥800℃, the feed amount per pass is 3-5mm / pass, and the rolling speed is 80-100 times / minute.

[0034] Furthermore, the parameters for cold rolling in step S106 include: the deformation amount per cold rolling pass is controlled at 20-30%, the rolling speed is 40-60 times / minute, the intermediate annealing temperature is 800-850℃, and the annealing time is 1.5-2.5h.

[0035] Further, step S102 includes: smelting is carried out using a high-vacuum non-consumable arc furnace. First, the circulating water is started, the equipment power is turned on, the furnace door is opened, and after cleaning the smelting furnace, the raw materials 0A grade small-particle sponge titanium, AlV55 alloy, and aluminum granules are placed in a copper crucible.

[0036] The high-vacuum non-consumable melting method can produce more uniform ingots, with a shorter melting time, making it suitable for melting refractory metals such as titanium.

[0037] The present invention will be further illustrated by the following examples.

[0038] Example 1 A method for preparing a seamless TC4 titanium alloy tube, the specific implementation steps are as follows: (1) The smelting is carried out in a high vacuum non-consumable electric arc furnace. First, start the circulating water, start the power supply of the equipment, open the furnace door, clean the smelting furnace, and then place 910kg of 0A grade small-particle sponge titanium, 50kg of AlV55 alloy and 40kg of aluminum granules in the copper crucible.

[0039] (2) After placing all the raw materials according to step (1), close the furnace door, start the mechanical pump, turn on the digital vacuum gauge, open the pre-evacuation valve, and wait for the vacuum to drop to 5×10 -3 When Pa, close the main pump valve, close the shut-off valve, and close the digital vacuum gauge. When the molecular pump speed reaches zero, turn off the molecular pump power supply.

[0040] (3) Open the charging valve and keep the mechanical pump running to ensure no air enters the charging pipeline. Wait until the vacuum level inside the furnace reaches 5×10⁻⁶.-4 Pa, close the charging valve, turn off the mechanical pump, turn on the gas analysis system, open the hydrogen cylinder and charging valve. When the total gas pressure in the furnace is -0.05MPa, charge in 0.01MPa hydrogen and then open the argon cylinder to charge in 0.04MPa argon. The hydrogen accounts for 20% of the total volume.

[0041] (4) After the ingot is forged 6 times, it is machined to obtain an extruded billet raw material of Ф120×40mm. The billet is clad with copper and iron, heated to 880℃ and held for 1.5h, and then extruded. The extrusion speed is controlled at 70-80mm / s, and the size obtained by extrusion is Ф90×20mm. After extrusion, it is air-cooled to room temperature. After extrusion, the temperature is raised to 900℃ at 10℃ / min and annealed in a horizontal vacuum annealing furnace for 2h. Then it is furnace-cooled to 500℃ and air-cooled to room temperature.

[0042] (5) Hot rolling: Hot rolling is carried out using a hot rolling mill. The hot rolling temperature is 900℃, the deformation per pass is controlled at 30-50%, the final rolling temperature is required to be ≥800℃, the feed amount per pass is 5mm / pass, and the rolling speed is 90 times / minute.

[0043] (6) Cold rolling: The deformation amount of the cold rolling pass is controlled at 20-30%, the rolling speed is 50 times / minute, and the intermediate annealing temperature parameter is 850℃ / 2h.

[0044] (7) Repeat steps (5) to (6) until a TC4 titanium alloy tube with a rolling size of Ф72×8mm is produced; wherein, after step (6), the heating rate is 10℃ / min, and the tube is annealed at 580℃ for 1h, and then furnace cooled to room temperature to obtain a seamless TC4 titanium alloy tube.

[0045] Upon testing, the microstructure of the TC4 titanium alloy seamless tube prepared in this embodiment is as follows: Figure 2 As shown, the microstructure is uniform and no coarse deformed grains are present. Its room temperature mechanical properties meet the following requirements: tensile strength Rm = 952 MPa, Rp0.2 = 878 MPa, and elongation after fracture A = 13.5%, indicating that the TC4 titanium alloy seamless tube prepared by the method of this embodiment has excellent comprehensive mechanical properties.

[0046] Example 2 A method for preparing a seamless TC4 titanium alloy tube, the specific implementation steps are as follows: (1) The smelting is carried out in a high vacuum non-consumable electric arc furnace. First, start the circulating water, start the power supply of the equipment, open the furnace door, clean the smelting furnace, and then place 900kg of 0A grade small-particle sponge titanium, 70kg of AlV55 alloy and 30kg of aluminum granules into the copper crucible.

[0047] (2) After placing all the raw materials according to step (1), close the furnace door, start the mechanical pump, turn on the digital vacuum gauge, open the pre-evacuation valve, and wait for the vacuum to drop to 5×10 -3 When Pa, close the main pump valve, close the shut-off valve, and close the digital vacuum gauge. When the molecular pump speed reaches zero, turn off the molecular pump power supply.

[0048] (3) Open the charging valve and keep the mechanical pump running to ensure no air enters the charging pipeline. Wait until the vacuum level inside the furnace reaches 5×10⁻⁶. -4 At pressure Pa, close the charging valve and mechanical pump, turn on the gas analysis system, and open the hydrogen cylinder and charging valve. When the total gas pressure inside the furnace is -0.05 MPa, charge in 0.01 MPa of hydrogen, then open the argon cylinder and charge in 0.04 MPa of argon. The hydrogen accounts for 20% of the total volume. Throughout the process, the ratio of hydrogen to argon is controlled by the gas analysis system.

[0049] (4) After smelting, TC4 titanium alloy ingots were obtained and then forged in 6 heats before machining to obtain Ф150×40mm extrusion billet raw material. After the billet surface was coated with a double layer of copper and iron, it was heated to 900℃ and held for 1.5h before extrusion. The extrusion speed was controlled at 60-80mm / s to obtain a tube billet with a size of Ф96×12mm, which was then air-cooled to room temperature. After extrusion, the temperature was raised to 900℃ at 10℃ / min and annealed in a horizontal vacuum annealing furnace for 3h, then furnace-cooled to 500℃ and air-cooled to room temperature.

[0050] (5) Hot rolling: The hot rolling is carried out using a hot rolling mill. The hot rolling temperature is 950℃, the deformation per pass is controlled at 30-50%, the final rolling temperature is required to be ≥800℃, the feed amount per pass is 4mm / pass, and the rolling speed is 80 times / minute.

[0051] (6) Cold rolling: The deformation amount of the cold rolling pass is controlled at 20-30%, the rolling speed is 40 times / minute, the intermediate annealing temperature is 850℃, and the annealing time is 2.5h.

[0052] (7) Repeat steps (5) to (6) until a Ф71×9mm TC4 titanium alloy tube is obtained; wherein, after step (6), the heating rate is 10℃ / min, and the tube is held at 550℃ for 1.5h for stress relief annealing, and then furnace cooled to room temperature to obtain a seamless TC4 titanium alloy tube.

[0053] Upon testing, the microstructure of the TC4 titanium alloy seamless tube prepared in this embodiment is as follows: Figure 3 As shown, the microstructure is uniform and no coarse deformed grains are present. Its room temperature mechanical properties meet the following requirements: tensile strength Rm = 964 MPa, Rp0.2 = 882 MPa, and elongation after fracture A = 14.6%, indicating that the TC4 titanium alloy seamless tube prepared by the method of this embodiment has excellent comprehensive mechanical properties.

[0054] Comparative Example A method for preparing a seamless TC4 titanium alloy tube, the specific implementation steps are as follows: (1) The smelting is carried out in a high vacuum non-consumable electric arc furnace. First, start the circulating water, start the power supply of the equipment, open the furnace door, clean the smelting furnace, and then place 900kg of 0A grade small-particle sponge titanium, 70kg of AlV55 alloy and 30kg of aluminum granules into the copper crucible.

[0055] (2) After placing all the raw materials according to step (1), close the furnace door, start the mechanical pump, turn on the digital vacuum gauge, open the pre-evacuation valve, and wait for the vacuum to drop to 5×10 -3 When Pa, close the main pump valve, close the shut-off valve, and close the digital vacuum gauge. When the molecular pump speed reaches zero, turn off the molecular pump power supply.

[0056] (3) Open the gas charging valve and keep the mechanical pump running until the vacuum level inside the furnace reaches 5×10⁻⁶. -4 At pressure 0.05 MPa, close the charging valve and shut off the mechanical pump. Turn on the gas analysis system and open the charging valve. When the total gas pressure inside the furnace is -0.05 MPa, charge with argon gas.

[0057] (4) After smelting, TC4 titanium alloy ingots were obtained and then forged three times before being machined to obtain Ф150×40mm extrusion billet raw materials. The billet surface was coated with a double layer of copper and iron, heated to 900℃ and held for 1.5h before extrusion. The extrusion speed was controlled at 100mm / s to obtain a tube billet with dimensions of Ф96×12mm, which was then air-cooled to room temperature. After extrusion, the temperature was raised to 900℃ at 10℃ / min and annealed in a horizontal vacuum annealing furnace for 3h, then furnace-cooled to 500℃ and air-cooled to room temperature.

[0058] (5) Warm rolling: After heating to 400-500℃ using an induction heating device, rolling is performed with a deformation of 10-20% per pass, a feed rate of 5mm / pass, and a rolling speed of 60 passes / minute. This process continues until a Ф71×9mm TC4 titanium alloy tube is obtained. In step (5), after heating at a rate of 10℃ / min, stress-relief annealing is performed at 550℃ for 2 hours, followed by furnace cooling to room temperature to obtain a seamless TC4 titanium alloy tube.

[0059] Upon testing, the microstructure of the TC4 titanium alloy seamless tube prepared in this embodiment is as follows: Figure 4 As shown, the microstructure is highly uneven in size, with many deformed grains. Its room temperature mechanical properties meet the following requirements: tensile strength Rm = 867 MPa, Rp0.2 = 830 MPa, and elongation after fracture A = 9.7%.

[0060] The above are exemplary embodiments disclosed in this invention. However, it should be noted that various changes and modifications can be made without departing from the scope of the embodiments of this invention as defined by the claims. Although the elements disclosed in the embodiments of this invention may be described or claimed individually, they may be understood as multiple unless explicitly limited to a singular number.

[0061] Those skilled in the art should understand that the discussion of any of the above embodiments is merely exemplary and is not intended to imply that the scope of the invention (including the claims) is limited to these examples. Within the framework of the invention, technical features of the above embodiments or different embodiments can be combined, and many other variations of different aspects of the invention exist, which are not provided in the details for the sake of brevity. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the invention should be included within the protection scope of the invention.

Claims

1. A method for preparing a seamless TC4 titanium alloy tube, characterized in that, Includes the following steps: S101. Prepare the raw materials for TC4 titanium alloy: 0A grade small-particle sponge titanium, AlV55 alloy and aluminum granules; S102. Place the raw materials, grade 0A small-particle sponge titanium, AlV55 alloy and aluminum granules, into a high-vacuum non-consumable arc furnace and evacuate the vacuum. S103. First, hydrogen gas is introduced into the high vacuum non-consumable arc furnace, followed by argon gas, and smelting begins to obtain TC4 titanium alloy ingots. S104. The TC4 titanium alloy ingot is forged to obtain the extrusion billet raw material; the surface of the extrusion billet raw material is coated with a double layer of copper and iron, and then extruded. After extrusion, the billet is air-cooled to room temperature; then the billet is annealed. S105. Hot rolling of the tube blank; S106. Cold rolling of the tube blank; S107. Repeat S105 to S106 until a TC4 titanium alloy seamless tube that meets the dimensional requirements is obtained, and then perform annealing treatment to obtain the finished TC4 titanium alloy seamless tube.

2. The method for preparing TC4 titanium alloy seamless tube according to claim 1, characterized in that, The annealing process in S104 is as follows: annealing in a horizontal vacuum annealing furnace at a temperature of 10℃ / min to 850-900℃ for 2-3 hours, followed by furnace cooling to 500℃ and then air cooling to room temperature. The annealing process in S107 is as follows: the TC4 titanium alloy seamless tube is heated to 550-580℃ in a horizontal vacuum annealing furnace at a rate of 7-10℃ / min for 1-1.5h, and then furnace cooled to room temperature.

3. The method for preparing the TC4 titanium alloy seamless tube according to claim 1, characterized in that, In S101, 880-920 kg of 0A grade small-particle titanium sponge, 50-70 kg of AlV55 alloy, and 30-50 kg of aluminum granules are added.

4. The method for preparing TC4 titanium alloy seamless tube according to claim 1, characterized in that, The extrusion process in S104 includes: heating the double-coated extrusion billet raw material to 860-920℃ and holding it for 1-2 hours before extrusion, with an extrusion ratio of 6-9 and an extrusion speed controlled at 60-80 mm / s.

5. The method for preparing TC4 titanium alloy seamless tube according to claim 1, characterized in that, The step S102, "placing raw materials 0A-grade small-particle sponge titanium, AlV55 alloy, and aluminum granules into a high-vacuum non-consumable arc furnace and then drawing a vacuum," includes: Place the raw materials, 0A grade small-particle sponge titanium, AlV55 alloy, and aluminum granules, into the copper crucible of a high-vacuum non-consumable arc furnace. Close the furnace door, start the mechanical pump, turn on the digital vacuum gauge, and open the pre-evacuation valve. Wait until the vacuum level inside the furnace drops to 5 × 10⁻⁶. -3 When Pa, close the main pump valve, close the shut-off valve, and close the digital vacuum gauge. When the molecular pump speed reaches zero, turn off the molecular pump power supply.

6. The method for preparing TC4 titanium alloy seamless tube according to claim 1, characterized in that, The step S103, "first filling a high-vacuum non-consumable arc furnace with hydrogen, then with argon, to begin melting and obtain a TC4 titanium alloy ingot," includes: Open the charging valve and keep the mechanical pump running, ensuring no air enters the charging pipeline, and wait until the vacuum level inside the furnace is ≤5x10. -4 Pa, close the charging valve, turn off the mechanical pump, open the hydrogen cylinder and charging valve. When the total gas pressure in the furnace is -0.05MPa, charge in 0.01MPa hydrogen and then open the argon cylinder to charge in 0.04MPa argon.

7. The method for preparing TC4 titanium alloy seamless tube according to claim 6, characterized in that, Hydrogen accounts for 20% of the total volume of gas in the furnace.

8. The method for preparing TC4 titanium alloy seamless tube according to claim 1, characterized in that, In step S104, the TC4 titanium alloy ingot is forged six times to obtain the extruded billet raw material.

9. The method for preparing TC4 titanium alloy seamless tube according to claim 1, characterized in that, The hot rolling parameters of S105 include: hot rolling temperature of 900-950℃, deformation per pass of 30-50%, final rolling temperature of ≥800℃, feed rate of 3-5mm / pass, and rolling speed of 80-100 passes / minute.

10. The method for preparing TC4 titanium alloy seamless tube according to claim 1, characterized in that, The cold rolling parameters of S106 include: the deformation amount per cold rolling pass is controlled at 20-30%, the rolling speed is 40-60 times / minute, the intermediate annealing temperature is 800-850℃, and the annealing time is 1.5-2.5h.

Citation Information

Patent Citations

  • Preparation method of near-alpha titanium alloy seamless tube

    CN117086125A

  • High-strength TA18 seamless titanium alloy and production method of large-diameter thin tube of high-strength TA18 seamless titanium alloy

    CN117867308A