Preparation method of high-strength ultrafine-particle-size diamond grinding head

Through the use of low-temperature sintering and special combination materials, the problem of graphitization of ceramic diamond grinding heads at high sintering temperatures is solved, the strength and sharpness of the grinding head are improved, and it is suitable for ultra-precision machining.

CN118848835APending Publication Date: 2024-10-29JIANGSU UPUNA TECH CO LTD +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411255868.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Ceramic diamond grinding heads are prone to graphitization at high sintering temperatures, resulting in a decrease in sharpness. Lowering the sintering temperature will damage the strength and hardness of the grinding head, limiting its application in ultra-precision machining.

Method used

Using the low-temperature sintering method of ceramic binder, by mixing diamond micropowder, nano-alumina, polymethyl methacrylate microspheres, yellow dextrin, polyethylene glycol and ammonium bicarbonate, cold pressing molding and sintering are combined with epoxy resin The glue solidifies to form a high-strength ultra-fine particle size diamond grinding head.

Benefits of technology

While lowering the sintering temperature, the strength, hardness and sharpness of the grinding head are increased, the service life is extended, and the wear resistance and polishing performance of the grinding head are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118848835A_ABST
    Figure CN118848835A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a high-strength ultrafine-particle-size diamond grinding head, which comprises the following steps: proportionally obtaining components of the diamond grinding head, mixing the components of the diamond grinding head, and carrying out first ball milling to obtain a grinding head forming material; the diamond grinding head at least comprises the following components: a ceramic bond, diamond micro powder, nano aluminum oxide, polymethyl methacrylate microspheres, yellow dextrin, polyethylene glycol and ammonium bicarbonate, wherein the ceramic bond comprises the following components: lithium oxide, boric oxide, silicon oxide, aluminum oxide, cobalt oxide, zinc oxide and calcium fluoride; carrying out cold press molding on the formed material to obtain a grinding head blank; sintering the grinding head blank to obtain a grinding head mature blank; and the grinding head matured blank and the grinding head base body are bonded and cured, and the diamond grinding head is obtained. The ceramic binding agent adopted by the method has the characteristic of high connection strength, the sintering temperature of the binding agent is reduced by adding lithium oxide and boron oxide, and the hardness and strength of the binding agent are ensured by adding silicon oxide and aluminum oxide.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of precision machining, and in particular to a method for preparing a high-strength ultra-fine-grained diamond grinding head. Background Art

[0002] Diamond grinding heads are a general term for small-shank diamond-like abrasive tools, which are widely used in the grinding of hard and brittle materials such as sapphire, glass, silicon carbide, and cemented carbide. Diamond grinding heads are mainly divided into metal bond diamond grinding heads, resin bond diamond grinding heads, and ceramic bond diamond grinding heads according to the type of binder. The advantages of metal diamond grinding tools are high strength and good wear resistance, which are suitable for rough machining. Resin diamond grinding tools have high elasticity and good self-sharpening properties, and are suitable for fine machining and super-fine machining. However, the particle size of the resin binder limits the use of ultra-fine abrasive particles in resin grinding tools, resulting in less application in the field of ultra-precision machining. Ceramic diamond grinding tools have the advantages of high strength and high sharpness, and have many applications in the field of ultra-precision machining of hard and brittle materials such as tungsten steel, sapphire, and silicon carbide.

[0003] At present, although ceramic diamond grinding heads have the advantages of high hardness and good self-sharpening, diamonds are prone to graphitization when the sintering temperature of the ceramic binder is high, which leads to a significant decrease in the sharpness of the grinding head. In the field of ultra-precision machining, the diamond particle size of ceramic diamond grinding heads is usually finer than 7μm, which leads to a decrease in the graphitization temperature of diamond. In order to ensure the sharpness and strength of fine-grained grinding heads, the ceramic binder is required to have a lower sintering temperature and higher strength. However, the reduction in the sintering temperature of the binder will lead to a decrease in the strength and hardness of the grinding head, which will in turn shorten the service life of the grinding head.

[0004] How to reduce the sintering temperature of the ceramic binder and prevent the diamond in the grinding head from graphitizing without reducing the strength and hardness of the grinding head and improving the sharpness and wear resistance of the grinding head is an urgent problem to be solved. Summary of the invention

[0005] In view of the above problems, the present invention is proposed to provide a method for preparing a high-strength ultra-fine-grained diamond grinding head that overcomes the above problems or at least partially solves the above problems.

[0006] According to one aspect of the present invention, a method for preparing a high-strength ultrafine-grained diamond grinding head is provided, the method comprising: obtaining components of the diamond grinding head in proportion, mixing the components of the diamond grinding head and then performing a first ball milling to obtain a grinding head forming material, wherein the components of the diamond grinding head at least include a ceramic binder, diamond micropowder, nano-alumina, polymethyl methacrylate microspheres, yellow dextrin, polyethylene glycol and ammonium bicarbonate, and the components of the ceramic binder include lithium oxide, boron oxide, silicon oxide, aluminum oxide, cobalt oxide, zinc oxide and calcium fluoride; cold-pressing the forming material to obtain a grinding head green embryo; sintering the grinding head green embryo to obtain a grinding head cooked embryo; bonding the cooked grinding head embryo to a grinding head substrate, and curing to obtain a diamond grinding head.

[0007] Optionally, in the preparation method of a high-strength ultrafine-grained diamond grinding head according to the present invention, the mass fractions of the various components included in the diamond grinding head are: ceramic binder: 10 to 40 parts, diamond micropowder: 40 to 60 parts, nano-alumina: 10 to 20 parts, polymethyl methacrylate microspheres: 1 to 10 parts, yellow dextrin: 1 to 5 parts, polyethylene glycol: 5 to 10 parts, and ammonium bicarbonate: 1 to 3 parts.

[0008] Optionally, in the preparation method of a high-strength ultrafine-grained diamond grinding head according to the present invention, the molar ratio of the components included in the ceramic binder is: 5% to 25% mol of lithium oxide, 20 to 30% mol of boron oxide, 10 to 20% mol of silicon oxide, 1 to 10% mol of aluminum oxide, 1 to 5 mol% of cobalt oxide, 1 mol% to 5 mol% of zinc oxide, and 1 mol% to 5 mol% of calcium fluoride.

[0009] Optionally, the method for preparing a high-strength ultrafine-grained diamond grinding head according to the present invention also includes the step of preparing a ceramic binder: subjecting the components of the ceramic binder to a second ball milling in proportion to obtain a powdered binder material; melting the powdered binder material, and then quenching it with water to obtain glass material; subjecting the glass material and water of equal mass to a second ball milling, and drying them based on the first drying temperature to obtain a ceramic binder.

[0010] Optionally, in the preparation method of a high-strength ultrafine-grained diamond grinding head according to the present invention, each component of the diamond grinding head is obtained in proportion, and the components of the diamond grinding head are mixed and then subjected to a first ball milling to obtain a grinding head forming material, including: obtaining each component in a preset proportion; mixing the diamond micropowder, ceramic binder, and nano-alumina in each component to obtain a first mixture; subjecting the first mixture to a first ball milling with a certain proportion of deionized water, and drying and sieving at a second drying temperature after the first ball milling to obtain a second mixture; adding polymethyl methacrylate microspheres, yellow dextrin, and polyethylene glycol to the second mixture to obtain a grinding head forming material.

[0011] Optionally, in the preparation method of the high-strength ultrafine-grained diamond grinding head according to the present invention, the forming material is cold-pressed to obtain a grinding head green body, including: cold-pressing the forming material through a mold, demolding and drying to obtain a grinding head green body.

[0012] Optionally, in the preparation method of a high-strength ultrafine-grained diamond grinding head according to the present invention, the molding material is cold-pressed by a mold, including: placing a gasket in the mold and performing a first pressurization treatment, the thickness of the gasket is 1 mm, the pressure of the first pressurization treatment is 10 to 15 MPa, and the holding time is 10 to 20 s; removing the gasket and performing a second pressurization treatment, the pressure of the second pressurization treatment is 20 to 30 MPa, and the holding time is 30 to 50 s.

[0013] Optionally, in the preparation method of a high-strength ultrafine-grained diamond grinding head according to the present invention, the grinding head green embryo is sintered to obtain a cooked grinding head embryo, including: placing the grinding head green embryo in a sintering furnace for sintering, and during the sintering process, heating it to a sintering temperature based on a predetermined heating rate, and keeping it warm for a predetermined time to obtain a cooked grinding head embryo.

[0014] Optionally, in the method for preparing a high-strength ultrafine-grained diamond grinding head according to the present invention, bonding the grinding head embryo to the grinding head base and curing the bonding comprises: bonding the grinding head embryo to the grinding head base using epoxy resin glue.

[0015] Optionally, the method for preparing a high-strength ultrafine-grained diamond grinding head according to the present invention further includes: dressing the diamond grinding head using an internal and external cylindrical grinder through a dressing tool, wherein the axial runout and radial runout of the dressed diamond grinding head are in the range of 0 to 20 μm.

[0016] Optionally, in the preparation method of a high-strength ultrafine-grained diamond grinding head according to the present invention, the particle size of the ceramic binder is 0.6μm-1.2μm, the particle size of the diamond micropowder is 10000-20000 mesh, the particle size of nano-alumina is 100-300nm, the particle size of yellow dextrin is 50-100μm, the particle size of polymethyl methacrylate microspheres is 3-10μm, and the molecular weight of polyethylene glycol is 600g / mol.

[0017] Optionally, in the preparation method of a high-strength ultrafine-grained diamond grinding head according to the present invention, the first mixture is subjected to a first ball milling with a certain proportion of deionized water, including: obtaining grinding balls of the same mass as the mixture formed by the first mixture and deionized water; adding the grinding balls and the mixture into a ball mill for the first ball milling.

[0018] Optionally, in the method for preparing a high-strength ultrafine-grained diamond grinding head according to the present invention, the mass of deionized water is 30% of the first mixture.

[0019] Optionally, in the method for preparing a high-strength ultrafine-grained diamond grinding head according to the present invention, the first ball milling time is 20 to 30 minutes, and the rotation speed is 500 to 800 r / min.

[0020] Optionally, in the method for preparing a high-strength ultrafine-grained diamond grinding head according to the present invention, the second drying temperature is 150-200°C.

[0021] Optionally, in the method for preparing a high-strength ultrafine-grained diamond grinding head according to the present invention, the second ball milling time is 10 to 12 hours, and the rotation speed is 500 to 800 r / min.

[0022] Optionally, in the method for preparing a high-strength ultrafine-grained diamond grinding head according to the present invention, the first drying temperature is 100-120°C.

[0023] Optionally, in the method for preparing a high-strength ultrafine-grained diamond grinding head according to the present invention, the predetermined heating rate is 3-5° C. / min, the sintering temperature is 620-700° C., and the predetermined time is 1-2 h.

[0024] Optionally, in the method for preparing a high-strength ultrafine-grained diamond grinding head according to the present invention, the dressing tool is a metal sintered diamond grinding wheel with a mesh size of 800 to 1000.

[0025] According to the solution of the present invention, a method for preparing a high-strength ultra-fine-grained diamond grinding head is provided, wherein the components of the diamond grinding head at least include a ceramic binder, diamond micropowder, nano-alumina, polymethyl methacrylate microspheres, yellow dextrin, polyethylene glycol and ammonium bicarbonate, wherein the components of the ceramic binder include lithium oxide, boron oxide, silicon oxide, aluminum oxide, cobalt oxide, zinc oxide and calcium fluoride. The ceramic binder has the characteristics of high connection strength, the addition of lithium oxide and boron oxide reduces the sintering temperature of the binder, and the addition of silicon oxide and aluminum oxide ensures the hardness and strength of the binder. At the same time, the addition of calcium fluoride, cobalt oxide and zinc oxide improves the fluidity of the binder and improves the wettability of the binder to diamond.

[0026] The present invention uses polymethyl methacrylate microspheres with good spherical shape as the pore-forming agent of the diamond grinding head. When the polymethyl methacrylate microspheres are sintered at high temperature, they will evaporate quickly and will not chemically react with the ceramic binder and diamond, thus leaving a regular hole structure.

[0027] In order to make the organizational structure of the diamond grinding head more uniform and dense, the present invention uses a wet mixing process, and uses volatile ammonium bicarbonate as a dispersant, which can effectively prevent the agglomeration of the binder in water. The ceramic binder and diamond can be effectively and evenly dispersed after ball milling. Using nano alumina powder as a filler can effectively improve the hardness and strength of the grinding head, increase the polishing performance of the grinding head, and reduce the naturally stacked pores formed by the grinding head due to cold pressing.

[0028] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention, it can be implemented according to the contents of the specification. In order to make the above and other purposes, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are listed below. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Various other advantages and benefits will become apparent to those of ordinary skill in the art by reading the detailed description of the preferred embodiments below. The accompanying drawings are only for the purpose of illustrating the preferred embodiments and are not to be considered as limiting the present invention. Moreover, the same reference symbols are used throughout the accompanying drawings to represent the same components. In the accompanying drawings:

[0030] Figure 1 A flow chart of a method 100 for preparing a high-strength ultra-fine-grain diamond grinding head according to an embodiment of the present invention is shown;

[0031] Figure 2 A flow chart of preparing a grinding head forming material according to an embodiment of the present invention is shown;

[0032] Figure 3 A flow chart of a method for preparing a ceramic binder according to an embodiment of the present invention is shown;

[0033] Figure 4 A physical diagram of a diamond grinding head according to an embodiment of the present invention is shown. DETAILED DESCRIPTION

[0034] The exemplary embodiments of the present disclosure will be described in more detail below with reference to the accompanying drawings. Although the exemplary embodiments of the present disclosure are shown in the accompanying drawings, it should be understood that the present disclosure can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided to enable a more thorough understanding of the present disclosure and to fully convey the scope of the present disclosure to those skilled in the art.

[0035] For ceramic bond diamond grinding heads, in order to prepare high-strength and high-wear-resistant grinding heads while reducing the sintering temperature of the ceramic bond, the present invention proposes a method 100 for preparing high-strength ultra-fine-grained diamond grinding heads.

[0036] Figure 1 A flow chart of a method 100 for preparing a high-strength ultra-fine-grained diamond grinding head according to an embodiment of the present invention is shown. It should be noted that according to the method 100 for preparing a diamond grinding head of the present invention, by preparing a low-temperature ceramic binder, a diamond grinding head is prepared based on the low-temperature ceramic binder, and the sintering temperature of the ceramic binder is reduced, so that the final prepared diamond grinding head has high strength and hardness, high sharpness and wear resistance.

[0037] The method 100 starts at step 102. In step 102, components of a diamond grinding head are obtained in proportion, mixed, and subjected to a first ball milling to obtain a grinding head forming material. The components of the diamond grinding head at least include a ceramic binder, diamond micropowder, nano-alumina, polymethyl methacrylate (PMMA) microspheres, yellow dextrin, polyethylene glycol (PEG), and ammonium bicarbonate. The components of the ceramic binder include lithium oxide, boron oxide, silicon oxide, aluminum oxide, cobalt oxide, zinc oxide, and calcium fluoride.

[0038] Specifically, Figure 2 As shown, step 102 includes the following sub-steps:

[0039] Step 112, obtaining each component according to a preset ratio.

[0040] In some embodiments, the mass fractions of each component included in the diamond grinding head are: ceramic binder: 10-40 parts, diamond micropowder: 40-60 parts, nano-alumina: 10-20 parts, polymethyl methacrylate microspheres: 1-10 parts, yellow dextrin: 1-5 parts, polyethylene glycol: 5-10 parts, and ammonium bicarbonate: 1-3 parts. The particle size of the ceramic binder is 0.6μm-1.2μm, the particle size of the diamond micropowder is 10000-20000 mesh, the particle size of the nano-alumina is 100-300nm, the particle size of the yellow dextrin is 50-100μm, the particle size of the polymethyl methacrylate microspheres is 3-10μm, and the molecular weight of the polyethylene glycol is 600g / mol. The present invention uses polymethyl methacrylate microspheres with better spherical shape as pore-forming agents for diamond grinding heads. When polymethyl methacrylate microspheres are sintered at high temperatures, they evaporate quickly and do not chemically react with ceramic binders and diamonds, leaving behind a regular pore structure.

[0041] In some embodiments, Figure 3 As shown, the method 100 also includes a method for preparing a ceramic binder, and the specific process is as follows:

[0042] Step 302, the components of the vitrified binder are subjected to a second ball milling in proportion to obtain a powdered binder material. Preferably, the components of the vitrified binder and grinding balls are added to a ball mill for ball milling, wherein the mass ratio of the components of the vitrified binder to the grinding balls is 1:1.

[0043] In some embodiments, the molar ratio of each component included in the ceramic binder is: 5% to 25% mol of lithium oxide, 20 to 30% mol of boron oxide, 10 to 20% mol of silicon oxide, 1 to 10% mol of aluminum oxide, 1 to 5 mol% of cobalt oxide, 1 mol% to 5 mol% of zinc oxide, and 1 mol% to 5 mol% of calcium fluoride. The ceramic binder has the characteristics of high connection strength. The addition of lithium oxide and boron oxide reduces the sintering temperature of the binder, and the addition of silicon oxide and aluminum oxide ensures the hardness and strength of the binder. At the same time, the addition of calcium fluoride, cobalt oxide, and zinc oxide improves the fluidity of the binder and improves the wettability of the binder to diamond.

[0044] Step 304, the powdered binder material is melted and then quenched to obtain glass material. Preferably, a box-type resistance furnace can be used to melt the powdered binder material.

[0045] Step 306, the glass material and water of the same mass are subjected to a second ball milling, and dried at the first drying temperature to obtain a ceramic binder. In this embodiment, the second ball milling time is 10 to 12 hours, the rotation speed is 500 to 800 r / min, and the first drying temperature is 100 to 120°C.

[0046] After obtaining the components of the diamond grinding head, the process proceeds to step 122 to mix the diamond powder, ceramic binder, and nano-alumina in the components to obtain a first mixture. Diamond powder, ceramic binder, and nano-alumina are mixed in proportion and stirred evenly to obtain a first mixture.

[0047] In step 132, the first mixture is subjected to a first ball milling with a certain proportion of deionized water, and after the first ball milling, the mixture is dried at a second drying temperature and sieved to obtain a second mixture. Preferably, the mass of the deionized water may be 30% of the mass of the first mixture.

[0048] In some embodiments, the first ball milling specifically includes: (1) obtaining grinding balls of the same mass as the mixture formed by the first mixture and deionized water. That is, the mass ratio of the grinding balls to the mixture formed by the first mixture and deionized water is 1:1. (2) adding the grinding balls and the mixture into a ball milling jar for the first ball milling. The first ball milling time is 20 to 30 minutes, and the rotation speed is 500 to 800 r / min.

[0049] In this embodiment, the second drying temperature may be 150-200°C.

[0050] Finally, in step 142, polymethyl methacrylate microspheres, yellow dextrin and polyethylene glycol are added to the second mixture to obtain a grinding head forming material.

[0051] The step 102 of this embodiment can realize the mixing process of the ultra-fine particle size powder.

[0052] In the subsequent step 104, the forming material is subjected to cold pressing to obtain a grinding head green body. Specifically, the forming material can be subjected to cold pressing through a mold, and then demoulding and drying are performed to obtain a grinding head green body.

[0053] In some embodiments, the process of cold pressing the molding material through the mold is as follows:

[0054] A gasket may be placed in the mold first, and a first pressurization treatment may be performed. The thickness of the gasket is 1 mm, the pressure of the first pressurization treatment is 10-15 MPa, and the holding time is 10-20 seconds.

[0055] Then the gasket is removed and a second pressurization treatment is performed. The pressure of the second pressurization treatment is 20 to 30 MPa and the pressure holding time is 30 to 50 seconds.

[0056] The purpose of step 104 is to press and dry the mixed material in step 102 above.

[0057] In the subsequent step 106, the grinding head green embryo is sintered to obtain a grinding head cooked embryo. Specifically, the grinding head green embryo is placed in a sintering furnace for sintering. During the sintering process, the temperature is increased to the sintering temperature based on a predetermined heating rate, and the temperature is kept for a predetermined time to obtain a grinding head cooked embryo. In this embodiment, the predetermined heating rate can be 3 to 5°C / min, the sintering temperature can be 620 to 700°C, and the predetermined time can be 1 to 2 hours.

[0058] Finally, in step 108, the grinding head blank is bonded to the grinding head base and cured to obtain a diamond grinding head. In this embodiment, epoxy resin glue can be used to bond the grinding head blank to the grinding head base.

[0059] In some embodiments, step 100 further comprises: dressing the diamond grinding head by using an internal and external cylindrical grinder through a dressing tool, wherein the axial runout and radial runout of the diamond grinding head after the dressing are in the range of 0 to 20 μm. The dressing tool is a metal sintered diamond grinding wheel with a mesh size of 800 to 1000.

[0060] The preparation method 100 of the high-strength ultra-fine-grained diamond grinding head provided in this embodiment, the components of the diamond grinding head at least include a ceramic binder, diamond micropowder, nano-alumina, polymethyl methacrylate microspheres, yellow dextrin, polyethylene glycol and ammonium bicarbonate, wherein the components of the ceramic binder include lithium oxide, boron oxide, silicon oxide, aluminum oxide, cobalt oxide, zinc oxide and calcium fluoride. The ceramic binder has the characteristics of high connection strength, the addition of lithium oxide and boron oxide reduces the sintering temperature of the binder, and the addition of silicon oxide and aluminum oxide ensures the hardness and strength of the binder. At the same time, the addition of calcium fluoride, cobalt oxide and zinc oxide improves the fluidity of the binder and improves the wettability of the binder to diamond.

[0061] The present invention uses polymethyl methacrylate microspheres with good spherical shape as the pore-forming agent of the diamond grinding head. When the polymethyl methacrylate microspheres are sintered at high temperature, they will evaporate quickly and will not chemically react with the ceramic binder and diamond, thus leaving a regular hole structure.

[0062] In order to make the organizational structure of the diamond grinding head more uniform and dense, the present invention uses a wet mixing process, and uses volatile ammonium bicarbonate as a dispersant, which can effectively prevent the agglomeration of the binder in water. The ceramic binder and diamond can be effectively and evenly dispersed after ball milling. Using nano alumina powder as a filler can effectively improve the hardness and strength of the grinding head, increase the polishing performance of the grinding head, and reduce the naturally stacked pores formed by the grinding head due to cold pressing.

[0063] The following is a method for preparing a high-strength ultra-fine-grained diamond grinding head of the present invention described by way of specific examples. This description is only intended to enable those skilled in the art to better understand the present invention, but does not limit the present invention in any way.

[0064] Example 1

[0065] The raw materials of the diamond grinding head include: ceramic bond, diamond powder, yellow dextrin, PEG, PMMA microspheres. The total amount of raw materials of the grinding head is 100 parts, including 30 parts of ceramic bond, 44 parts of diamond powder, 10 parts of nano alumina, 5 parts of yellow dextrin, 4 parts of PMMA microspheres, 6 parts of PEG solution, and 1 part of NH4HCO3.

[0066] The ceramic binder is smelted from 50 μm or finer lithium oxide, boron oxide, silicon oxide, aluminum oxide, zinc oxide, cobalt oxide and calcium fluoride, and the molar ratio of each component is 25 mol%, 25 mol%, 30 mol%, 5 mol%, 7 mol%, 5 mol% and 3 mol% respectively.

[0067] The diamond micropowder is 18000 mesh (#) diamond micropowder, the particle size of yellow dextrin is 150 μm, the particle size of PMMA microspheres is 5 μm, and the molecular weight of PEG is 600 g / mol.

[0068] The preparation of the ceramic bond diamond grinding head using the above components specifically includes the following steps.

[0069] (1) Lithium oxide, boron oxide, silicon oxide, aluminum oxide, zinc oxide, cobalt oxide, and calcium fluoride are placed in a ball mill (grinding ball diameter is 5 mm, ball-to-material ratio is 1:1) and mixed thoroughly for 1 h at a speed of 400 r / min.

[0070] (2) The raw material powders mixed uniformly in step 1 are placed in a corundum crucible and smelted in a box-type resistance furnace at a smelting temperature of 1200° C., a heating rate of 1° C. / min, and a holding time of 1.5 h. After the holding is completed, the liquid in the crucible is rapidly quenched to obtain glass material.

[0071] Glass materials and deionized water of equal mass are placed in a ball mill for ball milling. The ball milling is carried out three times at a speed of 800r / min and a single ball milling time of 600min. For the first ball milling, the diameter of the mortar ball is a mixed ball of 15mm and 10mm, of which 15mm:10mm is 1:1 (ball-to-material ratio 3:1). After the first ball milling is completed, the mixed ball is taken out and 10mm, 8mm, and 5mm mixed balls are added (mixing ratio is 1:1, ball-to-material ratio 3:1). After the second ball milling is completed, the mixed ball is taken out and replaced with a 5mm ball (ball-to-material ratio is 2:1) for the third ball milling. After the three ball millings are completed, the upper clear liquid is poured out and placed in a blast drying oven at 120℃ for drying. After drying, the required low-temperature ceramic binder can be obtained by passing through a 325# sieve.

[0072] (3) The ceramic binder prepared in step (2) and diamond, PMMA, nano-alumina, ammonium bicarbonate, deionized water and 3 mm grinding balls are placed in a ball mill and mixed, with a ball-to-material ratio of 1:1, a material-to-water ratio of 1:1, a ball milling time of 30 min and a rotation speed of 800 r / min.

[0073] (4) The wet material obtained by wet mixing in step (3) is placed in an oven and dried at 180° C. for 2 hours. After drying, yellow dextrin is added and dry mixed for 10 minutes at a speed of 800 r / min.

[0074] (5) The powder in step (4) is passed through an 80-mesh sieve and placed in a ceramic mortar. PEG is added and ground and mixed for 10 min. After mixing, the powder is passed through an 80-mesh sieve again to obtain a molding material.

[0075] (6) The molding material of step (5) is placed in a mold for cold pressing, with a feed density of 2.2 g / cm3, a first molding pressure of 15 MPa, a holding time of 15 s, a second molding pressure of 25 MPa, and a holding time of 30 s. After demolding, the grinding head embryo is placed in a drying oven for drying at a temperature of 50°C and a drying time of 2 h. After the embryo is dried, it is placed in a sintering furnace for sintering at a temperature of 650°C, a heating rate of 3°C / min, and a holding time of 2 h. After the cooling is completed, a cooked embryo of the grinding head is obtained.

[0076] (7) The grinding head blank obtained in step (6) is cleaned, bonded to a tungsten steel substrate using epoxy resin, and cured and trimmed to obtain a ceramic diamond grinding head. The dressing tool is trimmed using a 1200-mesh metal-bonded diamond grinding wheel, and the trimming requires that the axial and radial runout of the grinding head be within 20 μm.

[0077] Example 2

[0078] The raw materials of the ceramic bond diamond grinding head include: ceramic bond, diamond powder, yellow dextrin, PEG solution, PMMA and ammonium bicarbonate. The total amount of raw materials of the grinding head is 100 parts, including 25 parts of ceramic bond, 47 parts of diamond powder, 10 parts of nano alumina, 5 parts of yellow dextrin, 7 parts of PMMA microspheres, 6 parts of PVA solution and 1 part of NH4HCO3.

[0079] The ceramic binder is smelted from 50 μm fine lithium oxide, boron oxide, silicon oxide, aluminum oxide, zinc oxide, cobalt oxide, and calcium fluoride, and the molar ratio of each component is 25 mol%, 25 mol%, 30 mol%, 3 mol%, 2 mol%, 10 mol% and 5 mol%. The diamond micropowder is 20000# diamond micropowder, the nano alumina is 300 nm, the yellow dextrin particle size is 200#, the PMMA particle size is 3 μm, and the molecular weight of PEG is 600 g / mol.

[0080] The preparation of the ceramic bond diamond grinding head using the above components specifically includes the following steps.

[0081] (1) Lithium oxide, boron oxide, silicon oxide, aluminum oxide, zinc oxide, cobalt oxide, and calcium fluoride are placed in a ball mill (grinding balls are 5 mm, ball-to-material ratio is 1:1) and mixed thoroughly for 1 h at a speed of 400 r / min.

[0082] (2) The raw material powders uniformly mixed in step (1) are placed in a corundum crucible and smelted in a box-type resistance furnace at a smelting temperature of 1000°C, a heating rate of 3°C / min, and a holding time of 1 hour. After the holding is completed, the liquid in the crucible is quenched to obtain glass material. Glass material and deionized water of equal mass are placed in a ball mill for ball milling. The ball milling and drying process parameters are the same as those in Example 1 above.

[0083] (3) Same as step (3) in Example 1.

[0084] (4) Same as step (4) in Example 1.

[0085] (5) Same as step (5) in Example 1.

[0086] (6) The molding material of step (5) is placed in a mold for cold pressing, with a feed density of 2.1 g / cm3, a first molding pressure of 15 MPa, a holding time of 15 s, a second molding pressure of 25 MPa, and a holding time of 30 s. After demolding, the grinding head embryo is placed in a drying oven for drying at a temperature of 50°C and a drying time of 2 h. After the embryo is dried, it is placed in a sintering furnace for sintering at a temperature of 600°C, a heating rate of 3°C / min, and a holding time of 2 h. After the cooling is completed, a cooked embryo of the grinding head is obtained.

[0087] (7) Same as step (6) in Example 1.

[0088] Mechanical properties testing of vitrified bond diamond grinding heads.

[0089] (1) The ceramic diamond grinding head molding material in Example 1-2 was prepared into a grinding wheel specimen of 50*6*6 mm, and the bending strength of the grinding wheel was tested by a three-point bending method, and the hardness of the grinding wheel was tested by a Rockwell hardness tester.

[0090] (2) The actual grinding head prepared in Example 1-2 is as follows Figure 4 As shown, the overall height of the grinding head is 40 mm ± 0.5 mm, the height of the grinding wheel layer is 6.5 mm ± 0.02 mm, and the diameter is 8.5 mm ± 0.02 mm.

[0091] The following shows the polishing process of two aspherical workpieces, silicon carbide and tungsten steel, performed for 24 hours using the grinding heads prepared in Examples 1-2.

[0092] When machining silicon carbide workpieces, the grinding wheel spindle speed is 47000r / min, the spindle speed is 200r / min, and the feed rate is 1μm / s. When machining tungsten steel workpieces, the grinding wheel spindle speed is 42000r / min, the spindle speed is 200r / min, and the feed rate is 0.5μm / s. The size of the workpiece and the grinding head is measured by a micrometer. The ratio of the size consumed by the grinding head to the workpiece is used as the wear ratio of the grinding head to infer the durability of the grinding head. The UA3P three-dimensional stereoscopic profile measuring instrument is used to detect the surface quality of the workpiece after machining. The specific data are shown in Tables 1 and 2.

[0093] Table 1 Specific parameters of grinding head for processing silicon carbide

[0094] Serial number Strength (MPa) Hardness(HRB) Silicon carbide (Ra) Silicon Carbide (PV) Wear ratio Example 1 92.75 75.4 6.4nm 0.10μmm 100% Example 2 72.86 62.1 3.2nm 0.11μm 120%

[0095] Table 2 Specific parameters of grinding head for machining tungsten steel

[0096] Serial number Strength (MPa) Hardness(HRB) Tungsten steel (Ra) Tungsten Carbide(PV) Wear ratio Example 1 92.75 75.4 5.2nm 0.11μmm 130% Example 2 72.86 62.1 2.9nm 0.09μm 150%

[0097] It can be seen from the above examples 1 and 2 that the diamond grinding head prepared by the method for preparing a high-strength ultra-fine-grained diamond grinding head provided by the present application has the characteristics of high connection strength using a ceramic binder, the addition of lithium oxide and boron oxide reduces the sintering temperature of the binder, and the addition of silicon oxide and aluminum oxide ensures the hardness and strength of the binder. At the same time, the addition of calcium fluoride, cobalt oxide, and zinc oxide improves the fluidity of the binder and improves the wettability of the binder to diamond.

[0098] The present invention uses polymethyl methacrylate microspheres with good spherical shape as the pore-forming agent of the diamond grinding head. When the polymethyl methacrylate microspheres are sintered at high temperature, they will evaporate quickly and will not chemically react with the ceramic binder and diamond, thus leaving a regular hole structure.

[0099] In order to make the organizational structure of the diamond grinding head more uniform and dense, the present invention uses a wet mixing process, and uses volatile ammonium bicarbonate as a dispersant, which can effectively prevent the agglomeration of the binder in water. The ceramic binder and diamond can be effectively and evenly dispersed after ball milling. Using nano alumina powder as a filler can effectively improve the hardness and strength of the grinding head, increase the polishing performance of the grinding head, and reduce the naturally stacked pores formed by the grinding head due to cold pressing.

[0100] In the description of this specification, unless otherwise clearly specified and limited, the terms "connected", "fixed", etc. should be understood in a broad sense. In addition, the directions or positional relationships indicated by the terms "upper", "lower", "inner", "outer", "top", "bottom", etc. are based on the directions or positional relationships shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the equipment or unit referred to must have a specific direction, be constructed and operated in a specific orientation, and therefore, cannot be understood as limiting the present invention.

[0101] A11. The method as described in A2, wherein the particle size of the ceramic binder is 0.6μm-1.2μm, the particle size of the diamond powder is 10000-20000 mesh, the particle size of the nano-alumina is 100-300nm, the particle size of the yellow dextrin is 50-100μm, the particle size of the polymethyl methacrylate microsphere is 3-10μm, and the molecular weight of the polyethylene glycol is 600g / mol. A12. The method as described in A5, wherein the first mixture is subjected to a first ball milling with a certain proportion of deionized water, comprising: obtaining grinding balls of the same mass as the mixture formed by the first mixture and deionized water; adding the grinding balls and the mixture into a ball milling jar for the first ball milling. A13. The method as described in A12, wherein the mass of the deionized water is 30% of the first mixture. A14. The method as described in A1 or A5, wherein the time of the first ball milling is 20-30min, and the rotation speed is 500-800r / min. A15. The method as described in A5, wherein the second drying temperature is 150-200°C. A16. The method as described in A4, wherein the second ball milling time is 10-12h and the rotation speed is 500-800r / min. A17. The method as described in A4, wherein the first drying temperature is 100-120°C. A18. The method as described in A8, wherein the predetermined heating rate is 3-5°C / min, the sintering temperature is 620-700°C, and the predetermined time is 1-2h. A19. The method as described in A10, wherein the dressing tool is a metal sintered diamond grinding wheel with a mesh size of 800-1000.

[0102] In the description of this specification, the description of the terms "one embodiment", "some embodiments", "specific embodiments", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0103] In the description provided herein, a large number of specific details are described. However, it is understood that embodiments of the present invention can be practiced without these specific details. In some instances, well-known methods, structures and techniques are not shown in detail so as not to obscure the understanding of this description.

[0104] Similarly, it should be understood that in order to streamline the disclosure and aid in understanding one or more of the various inventive aspects, in the above description of exemplary embodiments of the invention, various features of the invention are sometimes grouped together into a single embodiment, figure, or description thereof. However, this disclosed method should not be interpreted as reflecting the intention that the claimed invention requires more features than those explicitly recited in each claim. Therefore, the claims that follow the detailed description are hereby expressly incorporated into the detailed description, with each claim itself serving as a separate embodiment of the invention.

[0105] Furthermore, those skilled in the art will appreciate that although some embodiments described herein include certain features included in other embodiments but not other features, the combination of features from different embodiments is meant to be within the scope of the present invention and to form different embodiments.

[0106] Although the present invention has been described as a limited number of embodiments, it will be apparent to those skilled in the art, with the benefit of the above description, that other embodiments may be envisioned within the scope of the invention thus described. In addition, it should be noted that the language used in this specification is selected primarily for readability and didactic purposes, rather than for explaining or defining the subject matter of the present invention. Therefore, many modifications and variations will be apparent to those skilled in the art without departing from the scope and spirit of the appended claims. The disclosure of the present invention is illustrative and not restrictive with respect to the scope of the present invention, and the scope of the present invention is defined by the appended claims.

Claims

1. A method for preparing a high-strength ultra-fine-grain diamond grinding head, include: The components of the diamond grinding head are obtained in proportion, and the components of the diamond grinding head are mixed and then subjected to a first ball milling to obtain a grinding head forming material, wherein the components of the diamond grinding head at least include a ceramic binder, diamond micropowder, nano-alumina, polymethyl methacrylate microspheres, yellow dextrin, polyethylene glycol and ammonium bicarbonate, and the components of the ceramic binder include lithium oxide, boron oxide, silicon oxide, aluminum oxide, cobalt oxide, zinc oxide and calcium fluoride; After the forming material is subjected to cold pressing, a grinding head green embryo is obtained; Sintering the grinding head green embryo to obtain a grinding head cooked embryo; The grinding head embryo is bonded to the grinding head base, and then cured to obtain the diamond grinding head.

2. The method according to claim 1, in, The mass fractions of the various components included in the diamond grinding head are: Ceramic binder: 10-40 parts, diamond powder: 40-60 parts, nano-alumina: 10-20 parts, polymethyl methacrylate microspheres: 1-10 parts, yellow dextrin: 1-5 parts, polyethylene glycol: 5-10 parts, ammonium bicarbonate: 1-3 parts.

3. The method according to claim 1 or 2, in, The molar ratio of each component included in the ceramic binder is: Lithium oxide 5% to 25% mol, boron oxide 20 to 30% mol, silicon oxide 10 to 20% mol, aluminum oxide 1 to 10% mol, cobalt oxide 1 to 5 mol%, zinc oxide 1 to 5 mol%, calcium fluoride 1 to 5 mol%.

4. The method according to claim 3, in, The step of preparing the ceramic binder is also included: The components of the vitrified binder are subjected to a second ball milling according to a certain proportion to obtain a powdered binder material; The powdered binder material is melted and then quenched to obtain glass material; The glass material and water of the same mass are subjected to a second ball milling, and are dried based on the first drying temperature to obtain the ceramic binder.

5. The method according to claim 2, in, The steps of obtaining the components of the diamond grinding head in proportion, mixing the components of the diamond grinding head and then performing a first ball milling to obtain a grinding head forming material include: Obtain each component according to a preset ratio; Mixing the diamond micropowder, the ceramic binder and the nano-alumina in each component to obtain a first mixture; The first mixture is subjected to a first ball milling with a certain proportion of deionized water, and after the first ball milling, the mixture is dried at a second drying temperature and sieved to obtain a second mixture; The polymethyl methacrylate microspheres, yellow dextrin and polyethylene glycol are added to the second mixture to obtain the grinding head forming material.

6. The method according to claim 1, in, After the forming material is subjected to cold pressing, a grinding head green embryo is obtained, which comprises: The molding material is cold pressed into shape by a mold, and then demoulded and dried to obtain a grinding head green body.

7. The method according to claim 6, in, The molding material is cold pressed by a mold, comprising: Placing a gasket in the mold and performing a first pressurization treatment, wherein the thickness of the gasket is 1 mm, the pressure of the first pressurization treatment is 10 to 15 MPa, and the holding time is 10 to 20 seconds; The gasket is removed and a second pressurization treatment is performed, wherein the pressure of the second pressurization treatment is 20 to 30 MPa and the pressure holding time is 30 to 50 seconds.

8. The method according to claim 1, in, Sintering the grinding head green embryo to obtain a grinding head cooked embryo comprises: The grinding head green embryo is placed in a sintering furnace for sintering. During the sintering process, the temperature is increased to a sintering temperature based on a predetermined heating rate and maintained at a predetermined time to obtain a grinding head cooked embryo.

9. The method according to claim 1, in, The grinding head blank is bonded to the grinding head base body and then cured, including: The grinding head blank and the grinding head base are bonded by using epoxy resin glue.

10. The method according to claim 1, in, Also includes: The diamond grinding head is dressed by using a dressing tool and an internal and external cylindrical grinder, wherein the axial runout and radial runout of the diamond grinding head after the dressing are in the range of 0 to 20 μm.

Citation Information

Patent Citations

  • Cerium oxide based composite polishing powder and its preparation method

    CN103382369A

  • Hollow stacking abrasive particle, preparation method thereof, and superhard abrasive tool

    CN109202750A

  • Self-sharpening superhard material grinding wheel and preparation method thereof

    CN112659003A

  • Ceramic-based diamond grinding wheel for wafer thinning as well as preparation method and application of ceramic-based diamond grinding wheel

    CN116460756A

  • Diamond grinding head preparation method

    CN117484410A