Asphalt biomass-based hard carbon composite material as well as preparation method and application thereof

By doping biomass-based hard carbon and pitch-based hard carbon with aluminum phosphate alcohol and performing a cross-linking reaction, an efficient sodium-ion battery anode material is formed, which solves the problems of energy density and cost of existing materials and achieves specific capacity and the first Improvement of efficiency.

CN118851147APending Publication Date: 2024-10-29JIANG SU NA BO & XIN CAI LIAO YOU XIAN GONG SI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410862833.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-09-28
Filing Date
2024-06-28
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

The energy density and cost of existing sodium-ion battery anode materials are difficult to meet market demand, and the first-time efficiency and specific capacity of the materials are low.

Method used

Biomass-based hard carbon and pitch-based hard carbon are doped with aluminum phosphate alcohol, and the specific capacity and first efficiency of the material are improved through cross-linking reactions and carbonization processes. The outer shell is coated with amorphous carbon to improve the sodium ion conduction rate and cycle performance.

Benefits of technology

A hard carbon composite material with high specific capacity, high first-time efficiency and low cost has been achieved, which has improved the energy density and kinetic performance of sodium-ion batteries and improved high-temperature storage and cycle performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004919433420000061
    Figure BDA0004919433420000061
  • Figure BDA0004919433420000071
    Figure BDA0004919433420000071
  • Figure BDA0004919433420000072
    Figure BDA0004919433420000072
Patent Text Reader

Abstract

The asphalt biomass-based hard carbon composite material is obtained by mixing and ball-milling asphalt, biomass and aluminum phosphate alcohol, then adding a cross-linking agent and an organic sodium salt for cross-linking reaction, carbonizing and then depositing a carbon source, thereby obtaining the amorphous carbon-coated asphalt biomass-based hard carbon composite material. According to the hard carbon composite material, biomass asphalt serves as a base body, biomass serves as hard carbon and has the characteristics of being high in specific capacity and compaction density, the asphalt material is high in compaction density and good in isotropy, and the energy density and the dynamic performance of the hard carbon composite material are improved through the synergistic effect of biomass and the asphalt material; aluminum phosphate alcohol is added, has good fluidity, promotes cross-linking of aluminum phosphate alcohol and aluminum phosphate alcohol, facilitates cross-linking pore-forming and improves the specific capacity; organic sodium salt is doped, so that the irreversible capacity is reduced, and the first efficiency is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of energy storage materials and relates to a battery negative electrode material, in particular to a hard carbon composite material for a sodium ion battery. Background Art

[0002] As a kind of amorphous carbon that is difficult to graphitize, hard carbon has many internal pores, disordered layer structure, and good material isotropy. However, due to the large specific surface area and many pores, the first efficiency of the material is low and the compaction density is low. When used in full batteries, the energy density of the battery is low. The factors that affect the compaction density and first efficiency of hard carbon materials are mainly the type of raw materials, the coating materials and doping on the surface of the materials, and the type of raw materials has the greatest impact. At present, the raw materials of commercial hard carbon mainly include resin materials, asphalt-based materials, coal-based raw materials, biomass materials, etc. Resin materials have the characteristics of high specific capacity, poor kinetics, high cost, and high consistency, which are suitable for high energy density sodium ion batteries. Asphalt-based materials have the characteristics of long-range order and short-range disorder, which makes the specific capacity of the material low and the first efficiency high. However, the material is widely available and low in cost, which is suitable for low energy density sodium ion batteries. As the market's requirements for the energy density of negative electrode materials used in sodium-ion batteries increase and their costs are extremely low, there is a need to develop hard carbon composite materials with high specific capacity, high initial efficiency and low cost. Summary of the invention

[0003] In view of the shortcomings of the prior art, in order to improve the specific capacity and initial efficiency of the existing sodium ion battery negative electrode materials while taking into account the cost of the materials, the present invention dopes biomass-based hard carbon and asphalt-based hard carbon with aluminum phosphate alcohol, utilizes the cross-linking effect of aluminum phosphate alcohol and its fluidity to improve the specific capacity of the material, and coats amorphous carbon in the outer shell to improve the initial efficiency of the material.

[0004] The technical purpose of the present invention is achieved through the following technical solutions:

[0005] The technical purpose of the first aspect of the present invention is to provide a method for preparing an asphalt biomass-based hard carbon composite material, comprising:

[0006] The asphalt, biomass and aluminum phosphate alcohol are mixed and ball-milled to obtain a hard carbon precursor material;

[0007] The hard carbon precursor material, the crosslinking agent and the organic sodium salt are mixed, crosslinked and carbonized at a temperature of 200-400° C. to obtain a hard carbon intermediate product;

[0008] A carbon source gas is introduced into the hard carbon intermediate product to deposit and carbonize it, thereby obtaining an amorphous carbon-coated asphalt biomass-based hard carbon composite material.

[0009] Furthermore, the weight ratio of the asphalt, biomass and aluminum phosphate alcohol is 10-50:100:1-5; the asphalt is selected from at least one of petroleum asphalt, coal asphalt and mesophase asphalt; the biomass includes straw, trees, agricultural product processing waste, agricultural and forestry waste and other materials in the agricultural and forestry production process, including but not limited to coconut shells, apricot shells, lignin, walnut shells and cotton stalks. The asphalt and biomass are crushed before use, preferably to a size of less than 100 μm.

[0010] Furthermore, the hard carbon precursor material, the crosslinking agent and the organic sodium salt are mixed in a weight ratio of 100:10-30:1-5. The organic sodium salt is selected from one of sodium 4,4'-biphenyl disulfonate, sodium anthraquinone-2-sulfonate and hydrated sodium 2-dibenzofuran sulfonate. The crosslinking agent is an alkylated urea-formaldehyde resin, specifically, at least one selected from ethylated urea-formaldehyde resin and butylated urea-formaldehyde resin.

[0011] Furthermore, the cross-linking reaction time is 1-6 hours.

[0012] Furthermore, the carbonization temperature after the cross-linking reaction is 1200-1500° C. and the time is 1-6 hours.

[0013] Furthermore, the carbon source gas is selected from at least one of methane, acetylene and ethylene.

[0014] Furthermore, the deposition carbonization is carried out in a tubular furnace at a temperature of 700-1000° C. for a time of 1-6 hours.

[0015] The technical purpose of the second aspect of the present invention is to provide an asphalt biomass-based hard carbon composite material prepared by the above method.

[0016] The technical purpose of the third aspect of the present invention is to provide the application of the above-mentioned asphalt biomass-based hard carbon composite material as a negative electrode material for sodium ion batteries.

[0017] Implementing the technical solution of the present invention has the following beneficial effects:

[0018] (1) The hard carbon composite material of the present invention is based on biomass asphalt. Biomass as hard carbon has the characteristics of high specific capacity and high compaction density. Asphalt material has high compaction density and good isotropy. The two work synergistically to improve the energy density and dynamic performance of the hard carbon composite material. Furthermore, by selecting the mixing ratio of the two, their respective advantages can be better brought into play.

[0019] (2) The present invention selects aluminum phosphate alcohol as a wetting agent for mixing and cross-linking biomass and asphalt. Aluminum phosphate alcohol has good fluidity and can make biomass and asphalt react under the action of the cross-linking agent, which is beneficial to cross-linking pore formation and improves the specific capacity of the material.

[0020] (3) The present invention dopes a specific organic sodium salt during the cross-linking process, and obtains sodium-doped porous amorphous carbon after carbonization, which can improve the sodium ion conduction rate during the charge and discharge process and improve the rate performance. The obtained material is applied to sodium ion batteries, which have the characteristics of high specific capacity, low compaction density, high initial efficiency, good rate, etc., and improve the high temperature storage and cycle performance of the sodium ion battery.

[0021] (4) The material of the present invention is coated with amorphous carbon in the outer shell to prevent the inner core sodium salt and its porous carbon structure from directly contacting the electrolyte, thereby reducing its side reactions and reducing the irreversible capacity during the charge and discharge process, thereby improving the initial efficiency. DETAILED DESCRIPTION

[0022] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0023] Example 1

[0024] Step S1: 30 g of petroleum asphalt, 100 g of coconut shell and 3 g of aluminum phosphate alcohol were mixed evenly and added to a ball mill, and ball milled at a ball milling speed of 300 rpm for 6 h to obtain a hard carbon precursor material;

[0025] Step S2: 100 g of hard carbon precursor material, 20 g of ethylated urea-formaldehyde resin and 3 g of sodium 4,4'-biphenyl disulfonate were mixed, cross-linked and cured at 300° C. for 3 h, and then heated to 1300° C. for carbonization for 3 h to obtain a hard carbon intermediate product;

[0026] Step S3: The hard carbon intermediate product is transferred to a tubular furnace, and methane gas is introduced, and the product is deposited and carbonized at a temperature of 900° C. for 3 h to obtain an amorphous carbon-coated hard carbon composite material.

[0027] Example 2

[0028] Step S1: 10 g of coal tar, 100 g of apricot shell and 1 g of aluminum phosphate alcohol were mixed evenly and added to a ball mill for milling at a ball milling speed of 300 rpm for 6 h to obtain a hard carbon precursor material;

[0029] Step S2: 100 g of hard carbon precursor material, 10 g of butylated urea-formaldehyde resin and 1 g of sodium anthraquinone-2-sulfonate were mixed, cross-linked and cured at 200° C. for 6 h, and then heated to 1200° C. for carbonization for 6 h to obtain an intermediate product;

[0030] Step S3: The intermediate product is transferred to a tubular furnace, and acetylene gas is introduced, and carbonized at a temperature of 700° C. for 6 hours to obtain a hard carbon composite material of amorphous carbon.

[0031] Example 3

[0032] Step S1: 50 g of mesophase pitch, 100 g of lignin and 5 g of aluminum phosphate alcohol were mixed evenly and added to a ball mill for ball milling at a ball milling speed of 300 rpm for 6 h to obtain a hard carbon precursor material;

[0033] Step S2: 100 g of hard carbon precursor material, 30 g of butylated urea-formaldehyde resin and 5 g of hydrated sodium 2-dibenzofuran sulfonate were mixed, cross-linked and cured at 400° C. for 1 h, and then heated to 1500° C. for carbonization for 1 h to obtain an intermediate product;

[0034] S3: The intermediate product is transferred to a tubular furnace, and ethylene gas is introduced, and carbonized at a temperature of 1000° C. for 1 hour to obtain an amorphous carbon-coated hard carbon composite material.

[0035] Comparative Example 1

[0036] The difference from Example 1 is that no aluminum phosphate alcohol is added, specifically:

[0037] Step S1: 30 g of petroleum asphalt and 100 g of coconut shell were mixed evenly and added into a ball mill, and ball milled at a ball milling speed of 300 rpm for 6 h to obtain a hard carbon precursor material;

[0038] Step S2: 100 g of hard carbon precursor material, 20 g of ethylated urea-formaldehyde resin and 3 g of sodium 4,4'-biphenyl disulfonate were mixed, cross-linked and cured at 300° C. for 3 h, and then heated to 1300° C. for carbonization for 3 h to obtain a hard carbon intermediate product;

[0039] Step S3: The hard carbon intermediate product is transferred to a tubular furnace, and methane gas is introduced, and the product is deposited and carbonized at a temperature of 900° C. for 3 h to obtain an amorphous carbon-coated hard carbon composite material.

[0040] Comparative Example 2:

[0041] The difference from Example 1 is that sodium 4,4'-biphenyl disulfonate is not added, specifically:

[0042] Step S1: 30 g of petroleum asphalt, 100 g of coconut shell and 3 g of aluminum phosphate alcohol were mixed evenly and added to a ball mill, and ball milled at a ball milling speed of 300 rpm for 6 h to obtain a hard carbon precursor material;

[0043] Step S2: 100 g of hard carbon precursor material and 20 g of ethylated urea-formaldehyde resin are cross-linked and cured at 300° C. for 3 h, and then heated to 1300° C. for carbonization for 3 h to obtain a hard carbon intermediate product;

[0044] Step S3: The hard carbon intermediate product is transferred to a tubular furnace, and methane gas is introduced, and the product is deposited and carbonized at a temperature of 900° C. for 3 h to obtain an amorphous carbon-coated hard carbon composite material.

[0045] Comparative Example 3:

[0046] The difference from Example 1 is that no vapor deposition is performed, that is, the hard carbon intermediate is used as the product, specifically:

[0047] Step S1: 30 g of petroleum asphalt, 100 g of coconut shell and 3 g of aluminum phosphate alcohol were mixed evenly and added to a ball mill, and ball milled at a ball milling speed of 300 rpm for 6 h to obtain a hard carbon precursor material;

[0048] Step S2: 100 g of hard carbon precursor material, 20 g of ethylated urea-formaldehyde resin and 3 g of sodium 4,4'-biphenyl disulfonate were mixed, cross-linked and cured at 300° C. for 3 h, and then heated to 1300° C. and carbonized for 3 h to obtain a hard carbon composite material.

[0049] Comparative Example 4

[0050] The difference from Example 1 is that aluminum phosphate alcohol is added in an amount exceeding the scope of the present invention, specifically:

[0051] Step S1: 30 g of petroleum asphalt, 100 g of coconut shell and 10 g of aluminum phosphate alcohol were mixed evenly and added to a ball mill, and ball milled at a ball milling speed of 300 rpm for 6 h to obtain a hard carbon precursor material;

[0052] Step S2: 100 g of hard carbon precursor material, 20 g of ethylated urea-formaldehyde resin and 3 g of sodium 4,4'-biphenyl disulfonate were mixed, cross-linked and cured at 300° C. for 3 h, and then heated to 1300° C. for carbonization for 3 h to obtain a hard carbon intermediate product;

[0053] Step S3: The hard carbon intermediate product is transferred to a tubular furnace, and methane gas is introduced, and the product is deposited and carbonized at a temperature of 900° C. for 3 h to obtain an amorphous carbon-coated hard carbon composite material.

[0054] Comparative Example 5

[0055] Sodium carbonate is used to replace the organic sodium salt of the present invention, which illustrates the importance of selecting the type of organic sodium salt in the present invention:

[0056] Step S1: 30 g of petroleum asphalt, 100 g of coconut shell and 1 g of aluminum alcohol were mixed evenly and added to a ball mill, and ball milled at a ball milling speed of 300 rpm for 6 h to obtain a hard carbon precursor material;

[0057] Step S2: 100 g of hard carbon precursor material, 20 g of ethylated urea-formaldehyde resin and 3 g of sodium carbonate were mixed, cross-linked and cured at 300° C. for 3 h, and then heated to 1300° C. for carbonization for 3 h to obtain a hard carbon intermediate product;

[0058] Step S3: The hard carbon intermediate product is transferred to a tubular furnace, and methane gas is introduced, and the product is deposited and carbonized at a temperature of 900° C. for 3 h to obtain an amorphous carbon-coated hard carbon composite material.

[0059] Performance tests of the materials prepared in the above examples and comparative examples:

[0060] (1) Physical and chemical properties

[0061] The specific surface area, tap density, and powder conductivity of the amorphous carbon-coated hard carbon composite materials prepared in Examples 1-3 and Comparative Examples 1-5 were measured. The test method was tested according to the national standard GBT-24533-2019 "Graphite Negative Electrode Materials for Lithium Ion Batteries". The test results are shown in Table 1.

[0062] Table 1.

[0063]

[0064]

[0065] (2) Button battery test

[0066] The amorphous carbon-coated hard carbon composite material in the embodiment and the comparative example is used as the negative electrode material of the sodium ion battery to assemble into a button cell. The specific preparation method of the negative electrode material is as follows: the hard carbon composite material: CMC: SBR: SP: H2O mass ratio is 94:2.5:1.5:2:150 to prepare a negative electrode sheet; the sodium sheet is used as the counter electrode; the electrolyte is NaPF6 (the solvent is EC:DEC:PC:propylene glycol polyoxypropylene ether=1:2:1:0.05, the concentration is 1.3 mol / L); the diaphragm is a composite film of polyethylene PE, polypropylene PP and polyethylene propylene PEP. The button cell is assembled in an argon-filled glove box. The electrochemical performance was tested on a Wuhan Blue Electric CT2001A battery tester, with a charge and discharge voltage range of 0.00V to 2.0V and a charge and discharge rate of 0.1C. The first discharge capacity and first efficiency of the button cell were tested, and its rate performance (2C / 0.1C) was tested at the same time. The test method was determined according to the GBT-24533-2019 "Graphite Anode Materials for Lithium-ion Batteries" standard. The test results are shown in Table 2.

[0067] Table 2.

[0068]

[0069] It can be seen from Table 1 and Table 2 that the amorphous carbon-coated hard carbon composite material of the embodiment of the present invention is better than the comparative example in terms of the initial efficiency and its discharge specific capacity. The reason is that the deposition of amorphous carbon on the outer layer and the doping of organic sodium salt reduce the irreversible capacity of the material and improve the initial efficiency. At the same time, the sodium storage properties of the material are improved by pore formation through the cross-linking agent, thereby improving the specific capacity.

[0070] (3) Soft pack battery test:

[0071] The amorphous carbon-coated hard carbon composite materials in the examples and comparative examples were slurried and coated to prepare negative electrode sheets, and the layered oxide (NaFe 1 / 3 Mn 1 / 3 Ni 1 / 3 A 5Ah soft-pack battery was prepared using NaPF6 (the solvent was EC:DEC:PC:propylene glycol polyoxypropylene ether = 1:2:1:0.05, concentration 1.3 mol / L) as the positive electrode.

[0072] Test cycle performance: charge and discharge current 1.0C / 1.0C, voltage range 1-4.0V, cycle number 500 times.

[0073] Test rate performance: Test the initial cycle DCR of the soft-pack battery and the constant current ratio under 2C charging conditions.

[0074] The test results are shown in Table 3.

[0075] Table 3.

[0076] project Cycle retention rate (%) 2C constant current ratio (%) Example 1 95.1 94.6 Example 2 94.2 94.1 Example 3 95.5 95.7 Comparative Example 1 92.4 86.5 Comparative Example 2 91.1 88.4 Comparative Example 3 91.9 87.6 Comparative Example 4 93.6 93.1 Comparative Example 5 90.6 86.5

[0077] It can be seen from Table 3 that compared with the comparative example, the cycle performance in Examples 1-3 is significantly better than that in the comparative example. The reason for this is that the material in the example has a high specific surface area, which improves the liquid retention performance of the material. At the same time, the material is doped with sodium salt to improve the conduction rate of sodium ions in the material and improve the rate performance.

[0078] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing an asphalt biomass-based hard carbon composite material, comprising: The asphalt, biomass and aluminum phosphate alcohol are mixed and ball-milled to obtain a hard carbon precursor material; The hard carbon precursor material, the crosslinking agent and the organic sodium salt are mixed, crosslinked and carbonized at a temperature of 200-400° C. to obtain a hard carbon intermediate product; A carbon source gas is introduced into the hard carbon intermediate product to deposit and carbonize it, thereby obtaining an amorphous carbon-coated asphalt biomass-based hard carbon composite material.

2. The preparation method according to claim 1, characterized in that: The weight ratio of the asphalt, biomass and aluminum phosphate alcohol is 10-50:100:1-5.

3. The preparation method according to claim 1, characterized in that: The asphalt is selected from at least one of petroleum asphalt, coal asphalt and mesophase asphalt, and the biomass is selected from at least one of coconut shell, apricot shell, lignin, walnut shell and cotton stalk.

4. The preparation method according to claim 1, characterized in that: The hard carbon precursor material, the cross-linking agent and the organic sodium salt are mixed in a weight ratio of 100:10-30:1-5.

5. The preparation method according to claim 1, characterized in that: The organic sodium salt is selected from one of sodium 4,4'-biphenyl disulfonate, sodium anthraquinone-2-sulfonate and hydrated sodium 2-dibenzofuran sulfonate.

6. The preparation method according to claim 1, characterized in that: The cross-linking agent is an alkylated urea-formaldehyde resin, and the cross-linking reaction time is 1-6 hours.

7. The preparation method according to claim 1, characterized in that: The carbonization temperature after the cross-linking reaction is 1200-1500° C. and the time is 1-6 hours.

8. The preparation method according to claim 1, characterized in that: The carbon source gas is selected from at least one of methane, acetylene and ethylene, and the temperature of the deposition carbonization is 700-1000° C. and the time is 1-6 hours.

9. The asphalt biomass-based hard carbon composite material prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the asphalt biomass-based hard carbon composite material according to claim 9 as a negative electrode material for sodium ion batteries.